A modified pyrrhotite autotrophic denitrification and dephosphorization packing and its preparation method
By surface sulfidation modification of pyrrhotite and its combination with biochar and foam/aerated concrete, a porous composite filler is formed, which solves the problems of low activity and poor stability of pyrrhotite filler and achieves efficient and low-cost denitrification and phosphorus removal.
Patent Information
- Application Number
- CN202511942432.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing pyrrhotite packing materials have low reactivity, are prone to passivation and deactivation, have poor physical stability, and rely on external carbon sources, resulting in high water treatment costs and unstable operation.
By surface-modifying pyrrhotite with sulfidation and combining it with biochar and foam/aerated concrete, a porous composite filler is formed, which provides electron transfer and microenvironment regulation, eliminating the need for external buffers.
It significantly improves reactivity and physical stability, reduces operating costs, achieves efficient and simultaneous nitrogen and phosphorus removal, and adapts to different water treatment conditions.
Smart Images

Figure CN123105849A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water treatment technology, specifically to a modified pyrrhotite autotrophic denitrification and dephosphorization packing material for advanced wastewater treatment and its preparation method. Background Technology
[0002] Eutrophication caused by excessive nitrogen and phosphorus in water bodies is a serious water environment problem. For urban sewage or certain industrial wastewater with a low carbon-to-nitrogen ratio (C / N), traditional heterotrophic denitrification processes require the addition of exogenous organic carbon (such as methanol and sodium acetate), resulting in high operating costs and the risk of secondary pollution. Sulfide-iron autotrophic denitrification technology uses sulfides and / or ferrous iron as electron donors and nitrates as electron acceptors, requiring no external organic carbon source. It offers advantages such as low cost and low sludge production, and has attracted considerable attention.
[0003] Pyrrhotite (Fe 1₋x S is a naturally occurring and abundant iron-sulfur mineral. Its crystal structure contains both Fe²⁺ and S²⁻, both of which can theoretically serve as electron donors for autotrophic denitrification. Furthermore, the oxidation product Fe³⁺ can form a precipitate with phosphate ions in water, thereby achieving simultaneous nitrogen and phosphorus removal. It is a highly promising water treatment material.
[0004] However, directly applying natural pyrrhotite to water treatment has significant drawbacks: 1) The mineral surface is chemically inert with a slow electron transfer rate, resulting in a long denitrification start-up cycle and low nitrogen removal load; 2) It is prone to surface passivation under the action of water and oxygen, forming a dense oxide layer (such as FeOOH), which hinders the further release of internal electron donors and causes rapid activity decay; 3) The sulfur oxidation process may produce a large amount of sulfate, leading to an increase in effluent salinity; 4) Simple mineral particles or packing materials formed by traditional binders (such as clay and organic polymers) are prone to problems such as particle pulverization, binder erosion, or structural collapse under long-term hydraulic scouring and microbial action, leading to packing bed compaction, blockage, and functional failure.
[0005] To address the aforementioned issues, existing technologies have attempted some improvements. For example, patent document [CN2014076323W] discloses a method for directly using pyrrhotite particles as denitrification filter media. While this technology utilizes the natural properties of pyrrhotite, it does not perform any activation or modification on the mineral, failing to solve the fundamental problems of low surface reactivity and slow start-up. Furthermore, the packing bed is prone to caking during long-term operation. Another patent document [CN117446968A] proposes using pyrrhotite in combination with biodegradable polymers (such as polylactic acid). Polylactic acid provides an organic carbon source during degradation, creating a local heterotrophic environment that promotes the denitrification rate to some extent. However, this method introduces an additional organic carbon source, increasing material costs, and the release rate of the carbon source is difficult to precisely match with the denitrification requirements, potentially leading to fluctuations in effluent COD and accelerating the biodegradation and destruction of the packing structure, affecting long-term operational stability.
[0006] In conclusion, developing an integrated sulfur-iron autotrophic denitrification packing material that combines high reactivity, excellent physical stability, no need for external carbon source, and long-term stable operation is of great significance for promoting the application of this technology in practical wastewater treatment projects. Summary of the Invention
[0007] The present invention aims to overcome the defects of existing technologies such as slow reaction kinetics, easy passivation and deactivation, poor physical stability, and dependence on external carbon sources or buffers of pyrrhotite fillers, and provides a novel composite filler and its preparation method by surface sulfidation modification, composite biochar and solidification with special inorganic materials.
[0008] To achieve the above objectives, the present invention adopts the following technical solution:
[0009] In a first aspect, this invention provides a modified pyrrhotite autotrophic denitrification and phosphorus removal packing material. This packing material is an irregular block or pre-formed regular morphology with a rich porous structure, made from the following raw materials in the indicated mass percentages: 40%–80% pyrrhotite sulfide, 15%–50% biochar, and 5%–25% solid shape retention agent; the sum of the mass percentages of all raw materials is 100%. The solid shape retention agent is foamed concrete or aerated concrete powder, preferably with a dry density of 300–800 kg / m³ and a particle size of 100–300 mesh. The pyrrhotite sulfide is a product of surface sulfidation modification with Na₂S solution. The biochar is a carbon material with certain alkaline functional groups and porous structure, which can serve as a microbial carrier, an electron mediator, and provide a certain pH buffering capacity, thus completely eliminating the need for traditional external buffers such as limestone in the formulation.
[0010] Secondly, the present invention provides a method for preparing the above-mentioned filler, comprising the following steps:
[0011] S1. Raw Material Preparation: Grind natural pyrrhotite to 80-200 mesh under an inert atmosphere (such as nitrogen) to prevent excessive oxidation. Prepare commercially available or conventionally produced biochar. Prepare foamed concrete or aerated concrete powder.
[0012] S2. Pyrrhotite sulfidation modification: The pyrrhotite powder obtained in step S1 is mixed with a Na2S solution with a concentration of 0.1–0.5 mol / L at a solid-liquid ratio of 1:(3–10). The pH is adjusted to 9–11 with NaOH solution, and the mixture is mechanically stirred at 20–30°C for 0.5–2 hours. The entire reaction is preferably carried out under an inert gas atmosphere. After the reaction is complete, the solid product is washed several times with deoxygenated deionized water under an inert gas atmosphere, and then dried at 50–80°C under an inert gas atmosphere for 6–24 hours to obtain pyrrhotite sulfide with a surface rich in active sulfur iron species.
[0013] S3. Mixing and Molding: Accurately weigh and mix the pyrrhotite sulfide, biochar, and foamed concrete (or aerated concrete) powder obtained in step S2 according to the designed mass percentage. Then, add 15% to 30% of the total mass of water to the dry mix and stir thoroughly to form a homogeneous slurry with a certain fluidity. Pour the slurry into a mold of the predetermined shape and gently vibrate to remove large air bubbles.
[0014] S4. Curing and Post-treatment: Transfer the poured mold to an environment with a temperature controlled at 20-40℃ and a relative humidity maintained above 90% for 3-7 days to allow the foamed concrete / aerated concrete to fully hydrate and form a solidified body. After demolding, dry the molded body at 40-60℃ to constant weight. Finally, according to actual application requirements, large molded bodies can be crushed and screened to obtain filler particles within a specific particle size range (e.g., 5-20mm).
[0015] Working principle and synergistic effect of the invention:
[0016] Activity enhancement mechanism: Na2S solution treatment situ generates a layer of nanoscale or amorphous FeS on the surface of pyrrhotite particles. x (e.g., FeS, FeS2) active layer. This layer has lower electrochemical impedance and higher catalytic activity, significantly improving the rate of autotrophic denitrification reaction.
[0017] Self-buffering and microenvironment regulation mechanisms: The biochar used typically contains a certain amount of alkaline ash (such as oxides or carbonates of potassium, calcium, and magnesium) and surface alkaline functional groups. This provides a partial inorganic carbon source for autotrophic denitrifying bacteria and effectively neutralizes the acids produced during the reaction.
[0018] Physical stability and biological habitat mechanism: During the hydration process, foamed concrete or aerated concrete forms a three-dimensional network rigid framework mainly composed of calcium silicate hydrate (CSH) gel. The micropores of the framework itself and the abundant pores of biochar together constitute a multi-level pore system, which optimizes mass transfer efficiency and provides an ideal place for microbial attachment and the formation of highly active biofilms.
[0019] Synergistic denitrification and phosphorus removal mechanism: pyrrhotite sulfide serves as the core electron donor and iron source, driving denitrification and generating Fe³⁺ for chemical phosphorus removal; biochar serves as a multifunctional auxiliary medium, providing additional electron transport pathways, microbial habitats, and microenvironment regulation capabilities.
[0020] Beneficial effects
[0021] Compared with the prior art, the present invention has the following significant advantages:
[0022] 1. High activity and fast start-up: Surface sulfidation modification fundamentally improves the reactivity of pyrrhotite, shortening the denitrification start-up time of the packing by more than 50% compared with the unmodified packing, and significantly improving the denitrification rate.
[0023] 2. Simplified formulation and integrated functions: By utilizing the inherent properties of biochar, the dual functions of microbial carrier and microenvironment regulation are achieved, successfully eliminating the need for the limestone component that must be added in traditional formulations, thus simplifying the types of raw materials.
[0024] 3. Excellent physicochemical stability: Using foamed concrete / aerated concrete as the shaping matrix, the filler can maintain its complete shape and pore structure even under long-term underwater immersion and continuous water flow, without the risk of softening or disintegration, thus solving the core problem of poor durability of traditional organic or clay binder fillers.
[0025] 4. Low operating cost and environmentally friendly: The entire process does not require the addition of organic carbon sources, relies on endogenous inorganic electron donors, and has low operating costs; the sludge yield is significantly lower than that of heterotrophic processes.
[0026] 5. Flexible application and strong versatility: The packing material has high strength and can be flexibly prepared into different shapes and particle sizes according to the requirements of different reactors (such as aerated biological filters, denitrification deep bed filters, and constructed wetlands), which is convenient for engineering promotion. Attached Figure Description
[0027] Figure 1 This invention provides a process for preparing the modified pyrrhotite autotrophic denitrification and dephosphorization packing material.
[0028] Figure 2 This is a comparison chart showing the removal effect of the packing material on total nitrogen (TN) in Examples 1, 2, and 3.
[0029] Figure 3This is a comparison chart showing the removal effect of the packing material on total phosphorus (TP) in Examples 1, 2, and 3. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the embodiments described herein are for illustrative purposes only and are not intended to limit the scope of protection of this invention.
[0031] Example 1
[0032] This embodiment prepares a filler with foamed concrete as the shape retention agent and a moderate proportion of pyrrhotite sulfide.
[0033] Raw material preparation: Natural pyrrhotite (Fe≈58%, S≈36%), crushed and ball-milled in a nitrogen atmosphere, then passed through a 150-mesh standard sieve. Commercially available bamboo biochar (passed through a 200-mesh sieve, specific surface area ≈350 m² / g). Solid shape retention agent: Commercially available foamed concrete blocks (dry density 400 kg / m³), mechanically crushed and ball-milled, then passed through a 200-mesh sieve.
[0034] Sulfide Modification: Weigh 200g of 150-mesh pyrrhotite powder and place it in a 2L three-necked flask. Continuously purge with high-purity nitrogen (0.5 L / min) for 15 minutes to remove oxygen. Under nitrogen protection, add 1.0L of 0.25 mol / L Na₂S·9H₂O solution (solid-liquid ratio 1:5) that has been deoxygenated by nitrogen. Stabilize the pH of the mixture to 10.2±0.2 by adding 1 mol / L NaOH solution dropwise. React at 25℃ and 250 rpm for 2 hours with mechanical stirring. After the reaction, under continuous nitrogen purging, wash the solid product five times with nitrogen-deoxygenated deionized water by centrifugation (6000 rpm, 5 min). Transfer the washed wet solid to a vacuum drying oven and dry at 60℃ under a nitrogen atmosphere for 24 hours to obtain black powdered pyrrhotite sulfide, which is then sealed and stored.
[0035] Mixing and Molding: Weigh the following by weight percentage: 60% pyrrhotite sulfide, 25% bamboo biochar, and 15% foamed concrete powder. Place the three dry powders in a mixer and mix for 30 minutes until the color is uniform. Add 20% (by weight) of purified water to the uniformly mixed dry powder and stir in a mixer for 15 minutes to form a viscous but flowable slurry. Pour the slurry into multiple cylindrical plastic molds (10mm in diameter and 10mm in height) with a release agent applied to the inner wall. Gently vibrate the molds to remove air bubbles and smooth the surface.
[0036] Curing and Post-treatment: After molding, the samples were placed in a constant temperature and humidity curing chamber and cured for 7 days at a temperature of 25±2℃ and a relative humidity of ≥95%. After demolding, the cylindrical packing blocks were placed in a 50℃ forced-air drying oven and dried to constant weight (approximately 48 hours). Some of the dried packing blocks were lightly crushed using a jaw crusher and sieved through a standard sieve to separate regular particles with a particle size of 8-12mm, which were then used as the final packing product.
[0037] Performance Testing. Test Apparatus: Three parallel acrylic columns (5cm inner diameter, 50cm height, designated as columns A, B, and C) were used as upflow biological filter columns. Each column was filled with 1.0L (approximately 650g) of the prepared packing material, to a filling height of approximately 35cm. Inoculation and Biofilm Formation: 2L of concentrated activated sludge solution containing denitrifying bacteria (MLSS≈15g / L) was injected into each column. After standing for 24 hours, a peristaltic pump was turned on to circulate simulated wastewater at a low flow rate (HRT=12h) for 7 consecutive days to allow biofilm formation. Simulated wastewater: Prepared with deionized water, its main components are: NaNO3 providing NO3⁻-N concentration of 20±1 mg / L, KH2PO4 providing PO4³⁻-P concentration of 2.0±0.2 mg / L, and NaHCO3 providing alkalinity (calculated as CaCO3) of 80 mg / L (simulating low-alkalinity influent), and also containing trace nutrients (MgSO4, CaCl2, trace element solution). The influent pH is adjusted to 7.0±0.2.
[0038] Operating conditions: During the formal experimental phase, the hydraulic retention time (HRT) was controlled at 2.0 hours, and the temperature was maintained at 22±1℃. Continuous water intake was used for operation.
[0039] Monitoring and Results: The system operated continuously for 30 days. Performance stabilized from day 15. Daily samples were taken from day 20 to 30 to measure the influent and effluent water quality. Results showed that the effluent TN concentration remained stable between 3.8 and 5.2 mg / L, with an average removal rate of 78.5%; the effluent TP concentration remained stable between 0.18 and 0.35 mg / L, with an average removal rate of 85.5%; and the system effluent pH value remained within the range of 6.9 to 7.6, demonstrating good self-buffering capacity. After operation, the packing material was removed for observation; the particles were intact, with no obvious wear or pulverization.
[0040] Example 2
[0041] This embodiment prepares a filler with a high proportion of biochar and aerosol concrete as the shape retention agent.
[0042] Raw material preparation: Pyrrhotite: Same as in Example 1, ground through a 150-mesh sieve. Biochar: Commercially available wood-based granular charcoal (passed through a 150-mesh sieve, specific surface area ≈ 280 m² / g). Solid shape retention agent: Commercially available aerated concrete panels (dry density 600 kg / m³), pulverized and ball-milled through a 150-mesh sieve.
[0043] Sulfurization modification: The process is the same as in Example 1, except the Na2S solution concentration is changed to 0.15 mol / L and the reaction time is 1.5 hours. Mixing and molding: Raw material ratio (mass percentage): 45% pyrrhotite sulfide, 45% wood-based biochar pellets, and 10% aerated concrete powder. The amount of water added is 18% of the total dry mass. The mixture is poured into a cubic silicone mold with a side length of 15 mm. Curing and post-treatment: Curing conditions: temperature 30℃, humidity >90%, time 5 days. After demolding and drying, the cubic filler is used directly without crushing, and the edges and corners are slightly naturally worn.
[0044] Performance testing: The testing equipment, inoculation, simulated wastewater (TN=20 mg / L, TP=2 mg / L) and operating conditions (HRT=2h, T=22℃) were the same as in Example 1.
[0045] Monitoring results: During the stable operation period (days 15-30), the average TN concentration in the effluent was 4.5 mg / L (average removal rate 77.5%), and the average TP concentration was 0.12 mg / L (average removal rate 94.0%). The effluent pH ranged from 7.1 to 7.8. The cubic shape of the packing material remained intact, and the biofilm coverage on the surface was uniform.
[0046] Example 3
[0047] This embodiment prepares a filler material that uses foamed concrete as a shape retention agent but has a very high proportion of pyrrhotite sulfide, for treating wastewater with high nitrogen load.
[0048] Raw material preparation: Pyrrhotite: ground through a 100-mesh sieve (particle size ≤150μm). Biochar: commercially available bamboo biochar as in Example 1. Solid shape retention agent: foamed concrete powder as in Example 1. Sulfide modification: process as in Example 1. Mixing and molding: Raw material ratio (mass percentage): 75% sulfide pyrrhotite, 15% bamboo biochar, 10% foamed concrete powder.
[0049] The amount of water added is 25% of the total dry material mass. Due to the high proportion of active powder, the slurry is slightly dry and requires vigorous stirring. The pouring process is the same as in Example 1. Curing and post-treatment: Curing conditions are the same as in Example 1. After demolding and drying, the slurry is crushed and sieved to remove irregular particles with a diameter of 10-15 mm.
[0050] Performance Testing: Simulated Wastewater Adjustment: The influent NO3⁻-N concentration was increased to 40±2 mg / L, the TP concentration remained at 2.0 mg / L, and the alkalinity was increased to 150 mg / L (calculated as CaCO3) to address the higher acid production potential. Other components remained the same. The HRT was adjusted to 3.0 hours to ensure sufficient reaction time. Other conditions were the same as in Example 1.
[0051] Monitoring results: The system reached stability after 20 days. During the stabilization period from day 25 to day 35, the average TN concentration in the effluent was 9.8 mg / L (corresponding to an average removal rate of 75.5%), indicating that it maintained a high nitrogen removal capacity even under high load; the average TP concentration in the effluent was 0.25 mg / L (average removal rate of 87.5%). The pH of the effluent remained stable between 6.8 and 7.5. The packing material had a robust granular structure and no emissions.
[0052] Example Analysis
[0053] The above three embodiments are all implemented within the scope of protection of the claims of this invention, fully demonstrating the feasibility, effectiveness, and flexibility of the technical solution:
[0054] Coverage of proportions: Examples 1 (60:25:15), 2 (45:45:10) and 3 (75:15:10) represent different typical formulations with a high proportion of pyrrhotite sulfide, a low to high proportion of biochar, and a basic amount of solid shape retention agent, which fully cover the range of proportions of the core raw materials described in claim 1.
[0055] Process Feasibility: All embodiments employed the core vulcanization modification process and foamed concrete / aerated concrete casting and curing process of this invention, verifying the operability and repeatability of the preparation method. Commercially available biochar was used directly, simplifying pretreatment.
[0056] Performance verification: When treating simulated wastewater with different nitrogen loads, the three packing materials with different ratios all showed efficient and stable simultaneous nitrogen and phosphorus removal performance (TN removal rate >75%, TP removal rate >85%), and demonstrated good pH self-stabilization ability of the system, which confirmed the buffer and carrier functions of biochar in the system.
[0057] In summary, the results of the embodiments show that the modified pyrrhotite autotrophic denitrification denitrification and phosphorus removal packing and its preparation method provided by the present invention successfully solve the key problems pointed out in the background art, such as low activity, need for external buffering agents, and poor physical stability, and have significant technological progress and broad prospects for promotion and application.
[0058] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A modified pyrrhotite autotrophic denitrification and dephosphorization packing material, characterized in that, It is made from the following raw materials by mass percentage: 40%–80% pyrrhotite sulfide, 15%–50% biochar, and 5%–25% solid shape retention agent; the sum of the mass percentages of each raw material is 100%; the solid shape retention agent is foamed concrete or aerated concrete.
2. The modified pyrrhotite autotrophic denitrification and dephosphorization packing material according to claim 1, characterized in that, The pyrrhotite sulfide has a particle size of 80–200 mesh; the foamed concrete or aerated concrete has a dry density of 300–800 kg / m³ and a particle size of 100–300 mesh.
3. The modified pyrrhotite autotrophic denitrification and dephosphorization packing material according to claim 1, characterized in that, The pyrrhotite sulfide is prepared by the following method: natural pyrrhotite is ground into powder and mixed with a Na2S solution with a concentration of 0.1-0.5 mol / L at a solid-liquid ratio of 1:(3-10). The mixture is stirred for 0.5-2 hours at a pH of 9-11 and a temperature of 20-30℃. Then, solid-liquid separation, washing, and drying of the solid are carried out under inert gas protection to obtain the pyrrhotite sulfide.
4. A method for preparing a modified pyrrhotite autotrophic denitrification and dephosphorization packing material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: S1. Raw material preparation: Grind natural pyrrhotite to 80-200 mesh; prepare biochar and foamed concrete or aerated concrete powder; S2. Pyrrhotite sulfidation modification: Mix the pyrrhotite powder obtained in step S1 with a concentration of 0.1-0.5... A mol / L Na2S solution is mixed at a solid-liquid ratio of 1:(3-10), the pH is adjusted to 9-11, and the mixture is stirred at 20-30℃ for 0.5-2 hours. After the reaction, the mixture is washed under inert gas protection and then dried at 50-80℃ under inert gas protection for 6-24 hours to obtain pyrrhotite sulfide. S3, Mixing and molding: The pyrrhotite sulfide, biochar, and foamed concrete or aerated concrete powder obtained in step S2 are mixed in the following mass percentages: pyrrhotite sulfide 40%-80%, biochar 15%-50%, foamed concrete or aerated concrete 5%-25%. After mixing evenly, 15%-30% of the total mass of the mixture is added to water and stirred to form a slurry, which is then poured into a mold. S4, Curing: The mold is cured at a temperature of 20-40℃ and a humidity of ≥90% for 3-7 days. After demolding, the modified pyrrhotite autotrophic denitrification denitrification and phosphorus removal filler is obtained.
5. The preparation method according to claim 4, characterized in that, The inert gas mentioned in step S2 is nitrogen or argon.
6. The preparation method according to claim 4, characterized in that, In step S4, the demolded filler is dried to constant weight at 40-60℃, and the resulting porous block is crushed and screened into particles of 5-20mm.
Citation Information
Patent Citations
Deep nitrogen and phosphorus removal method based on polylactic acid cooperated with pyrrhotite denitrification
CN117446968A