A method for preparing and applying a composite carbon source for electronic panel wastewater

The composite carbon source, through multi-component spatial confinement design and dual cross-linked network regulation, solves the problems of low carbon source utilization and inhibited denitrifying bacteria activity in electronic panel wastewater, achieving efficient denitrification and nitrogen removal and enhancing the system's shock resistance.

CN123105850APending Publication Date: 2026-11-17广州科城水投技术服务有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611393212.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The problems in electronic panel wastewater include low carbon source utilization, inhibition of denitrifying bacteria activity by high salt, complexed heavy metals and alcohol-ketone solvents, carbon-nitrogen ratio imbalance and mismatch of carbon release rate.

Method used

A composite carbon source was prepared by employing a multi-component spatial confinement design and dual cross-linking network regulation, including a fast-acting carbon core, a slow-release framework, a detoxifying and inhibitory agent, and a cross-linking micronutrient. Polydopamine generated by the self-polymerization of dopamine hydrochloride and phytic acid-grafted sodium lignin sulfonate form stable composite microcapsules. Combined with supercritical CO2 foaming and pore-forming, a carbon source supply with rapid release in the early stage and slow release in the later stage was achieved.

Benefits of technology

It improves denitrification efficiency, enhances the system's shock resistance, increases carbon source utilization and denitrification rate, achieves highly efficient denitrification nitrogen removal, and maintains the activity of denitrifying bacteria under near-neutral pH conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105850A_ABST
    Figure CN123105850A_ABST
Patent Text Reader

Abstract

This invention discloses a composite carbon source for electronic panel wastewater, its preparation method, and its application. The composite carbon source particles contain sodium acetate trihydrate and D-glucose fast-acting carbon cores, sodium carboxymethyl cellulose / polyvinyl alcohol slow-release framework, phytic acid-grafted sodium lignin sulfonate and polydopamine-coated walnut shell biochar detoxifying and inhibitory agents, a citric acid / polyglycerol glycidyl ether double crosslinking system, and Fe-Mn-Mo-Se composite trace elements. The pH of the water film on the particle surface is maintained at 6.5–7.5, achieving a gradual and synergistic decomposition of EDTA-complexed heavy metals; the porous structure control enables rapid release in the first 7 days and slow release in the following 20 days. In electronic panel wastewater with COD / TN = 1.5–3.5, containing complexed heavy metals and alcohol / ketone solvents, the TN removal rate reaches 90.8%–92.4%, the carbon source utilization rate reaches 86.8%–89.6%, the shock recovery time is less than 11 hours, and the particle retention rate after 30 days is not less than 94.8%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wastewater treatment and denitrification technology, specifically to a composite carbon source designed for electronic panel wastewater with low biodegradability, high toxicity of complexed heavy metals, and complex stress characteristics, as well as its preparation method and application. Background Technology

[0002] The production processes of the electronic panel industry (PCB circuit boards, LCD / OLED display panels) cover etching, electroplating, developing, cleaning, photolithography, chemical polishing, and other steps. The combined wastewater has very unique characteristics, with the following features: Extremely low carbon-to-nitrogen ratio and severe deficiency of endogenous carbon: The wastewater is mainly composed of ammonia nitrogen and nitrate nitrogen, with very little organic biodegradable carbon. The B / C ratio is only 0.10 to 0.25, and the COD / TN ratio is 1.5 to 3.5. Natural carbon sources are almost unable to support denitrification. It has complex toxicity and extremely strong microbial inhibition: it contains developer, photoresist, alcohol and ketone organic solvents, and surfactants, which inhibit the activity of denitrifying bacteria over a long period of time. The combined stress of high salt, fluoride ions, and complexed heavy metals: The wastewater has high salt content, fluoride ion content of 50-300 mg / L, and a large amount of copper and nickel in EDTA complex form, which creates a combined stress on conventional microorganisms and makes them very easy to inactivate. The water quality and quantity fluctuate drastically, and the pH range is large. The pretreated effluent impacts the biological system, and traditional carbon sources have extremely poor adaptability.

[0003] When this type of wastewater undergoes direct biological denitrification, traditional carbon sources face three major shortcomings: 1. Functional segmentation, such as the composite carbon source for wastewater treatment disclosed in CN113264588B, whose composition and mass fraction are: 0%~5% methanol, 0%~5% ethanol, 5%~30% sodium acetate, 0%~5% glucose, 0.1%~2% molasses, 1%~5% humic acid fermentation broth, and the remainder being water; wherein, the COD of the humic acid fermentation broth is 1~80,000 mg / L. This composite carbon source achieves resource utilization, and the dosage can be as low as 0.4~0.8 times that of traditional carbon sources, while enriching a large number of denitrifying bacteria, significantly improving the nitrogen removal effect by 1.5~2.5 times. However, the physical compounding of methanol / sodium acetate / humic acid fermentation broth in this technical solution only focuses on "carbon supply" and there is no chemical bond between the components. When applied to the treatment of electronic panel wastewater, it releases more than 80% of COD within 0 to 2 hours after addition, which cannot match the growth kinetics of denitrifying bacteria. Moreover, the necessary complex-breaking agents (such as strong acid adjustment or calcination of calcite) are disconnected from the carbon source system, and strong acid conditions (pH 1 to 3) will directly inhibit or even inactivate the denitrifying functional bacteria.

[0004] 2. Carbon Release Kinetic Mismatch: For example, CN110255712B discloses a method for preparing a denitrifying carbon source, comprising the following steps: 1) introducing straw pyrolysis residue into an electrodialysis treatment system to obtain electrodialysis concentrate and electrodialysis desalination water; 2) introducing the electrodialysis desalination water into an ultrafiltration membrane separation unit for pretreatment, and then introducing the permeate from the ultrafiltration membrane separation unit into a nanofiltration membrane separation unit for treatment to obtain nanofiltration membrane concentrate and nanofiltration desalination water; 3) introducing the nanofiltration desalination water into a reverse osmosis membrane separation unit to obtain reverse osmosis membrane concentrate; 4) mixing the electrodialysis concentrate, nanofiltration membrane concentrate, and reverse osmosis concentrate to prepare a carbon source. The electrodialysis + membrane separation system effectively recovers and utilizes low-molecular-weight organic components in the pyrolysis residue of crop straw, which are easily utilized by denitrifying bacteria. Through compounding, a composite carbon source with a B / C ratio > 0.8 can be prepared, which has significant economic value in the field of nitrogen removal. CN116216931A discloses a method for preparing a denitrification solid slow-release carbon source and its application. The biomimetic structure improves the appearance, increasing the surface area and facilitating water flow. Attapulgite is modified to load iron ions, enhancing its adsorption and control of phosphorus in water. A caprolactone coating layer is prepared on its surface, enhancing its compatibility with polycaprolactone, and the long-chain structure strengthens the cross-linking strength with polycaprolactone. Based on this, a biomimetic denitrification unit using the denitrification solid slow-release carbon source is designed, with a defined structure for easy deployment and simple operation and management. This allows for widespread application, avoiding the use of large equipment and the separate construction of denitrification units, saving on treatment site and operation and management costs. However, the carbon release curve of this method, which enriches small molecule organic matter through membrane separation or single polymer slow-release particles, often exhibits a single exponential decay or delayed start-up (start-up period > 15 days), failing to cope with the instantaneous impact of electronic panel wastewater quality.

[0005] 3. Insufficient anti-toxicity design: Existing traditional carbon sources lack microscopic protective mechanisms against the combined stresses of high salt, fluorine, organic solvents, and complexed heavy metals. Alcohol and ketone solvents easily damage cell membranes, and complexed heavy metals continuously compete for electrons in the electron transport chain, leading to a significant decrease in specific denitrification rates. Specifically, EDTA has a significant impact on Cu... 2+The absolute stability constant of EDTA is as high as 18.80, but its conditional stability constant varies significantly under different pH conditions: it is 18.35 at pH 10, decreases to 15.48 at pH 7, and further decreases to about 14.81 at pH 6.5. While existing strong acid complex-breaking methods (pH 1–3) can effectively reduce the conditional stability constant of EDTA, extremely acidic environments can directly inhibit or even inactivate denitrifying bacteria (the suitable pH window for denitrifying bacteria is 6.5–8.5). How to achieve the mild decomposition of EDTA-complexed heavy metals within the near-neutral pH range (6.5–7.5) tolerable by the biochemical system, without affecting the activity of denitrifying bacteria, is a pressing technical challenge in this field. Furthermore, existing phytic acid-lignin grafting technology uses a direct esterification method, which is prone to hydrolysis and breakage of ester bonds in alkaline wastewater environments, leading to the loss of detoxification functional components. Therefore, there is an urgent need to develop more stable covalent bonding methods.

[0006] Therefore, those skilled in the art have been dedicated to finding a more comprehensive technical solution to address the problems of extremely low carbon source utilization due to the low biodegradability of electronic panel wastewater, the problem of high toxicity (complexed heavy metals, alcohol and ketone solvents and high salt) inhibiting the activity of denitrifying bacteria, and the problem of carbon-nitrogen ratio imbalance and mismatch between carbon release rate. Summary of the Invention

[0007] This invention aims to overcome any of the deficiencies in the prior art and provide a composite carbon source for denitrification of electronic panel wastewater, its preparation method, and its application. Through multi-component spatial confinement design and dual-crosslinking network regulation, in-situ directional competitive complex breaking is achieved, resulting in a good match between rapid release in the first 7 days and slow-release steady state in the following 20 days, thereby improving denitrification efficiency and systemic shock resistance under high toxicity stress.

[0008] To achieve the above objectives, the present invention provides a composite carbon source for electronic panel wastewater. The composite carbon source is characterized by being granular and comprising, by dry basis mass percentage: a fast-acting carbon core (sodium acetate trihydrate 26%–31%, D-glucose 11%–15%), a slow-release framework (sodium carboxymethyl cellulose (CMC-Na) 21%–25%, polyvinyl alcohol (PVA) 12%–15%), a detoxifying and inhibitory agent (phytic acid-grafted lignin sulfonate sodium (PA-LS) 8%–12%, polydopamine-coated walnut shell biochar (PDA@WBC) 3%–7%), and a cross-linking and micronutrient agent (citric acid and polyglycerol glycidyl ether (PGPE) double cross-linking system 3%–5%, Fe-Mn-Mo-Se composite trace elements 0.5%–1.5% (based on the total mass of Fe+Mn+Mo+Se elements)).

[0009] In this invention, the polyvinyl alcohol is preferably PVA-1799 (polyvinyl alcohol with a degree of polymerization of about 1700 and a degree of alcoholysis of 98% to 99%); the Fe-Mn-Mo-Se composite trace elements are provided in the form of ferrous sulfate, manganese sulfate, sodium molybdate and sodium selenite, and the mass ratio of Fe, Mn, Mo and Se is calculated based on each element; the grafting degree refers to the number of millimoles of phosphate groups contained in each gram of phytic acid-grafted sodium lignin sulfonate (calculated by total phosphorus determined by ICP-OES).

[0010] Preferably, the particles have porous channels inside, and the overall particle size is 1.5 to 2.5 mm.

[0011] Preferably, the phosphate grafting degree of the phytic acid-grafted sodium lignin sulfonate is 0.4 to 0.6 mmol / g.

[0012] Preferably, the degree of substitution (DS) of the sodium carboxymethyl cellulose is 0.8 to 1.0; the polyvinyl alcohol is PVA-1799; and the mass ratio of Fe, Mn, Mo, and Se in the Fe-Mn-Mo-Se composite trace element is (8 to 12):(4 to 6):(0.8 to 1.2):(0.08 to 0.12).

[0013] Further, the polydopamine-coated walnut shell biochar is prepared by the following method: walnut shells (from the Juglandaceae family) are washed, dried, crushed, and passed through a 40-60 mesh sieve, and carbonized at 650-750℃ for 2-4 h under a nitrogen atmosphere to obtain walnut shell biochar; the walnut shell biochar is dispersed in dopamine hydrochloride Tris-HCl buffer (dopamine hydrochloride 0.005-0.02 mol / L, Tris-HCl 0.05-0.1 mol / L, pH 8.5), and self-polymerized at 25-35℃ in the dark for 18-24 h, followed by washing and drying to obtain polydopamine-coated walnut shell biochar.

[0014] Another object of the present invention is to provide a method for preparing any of the above-mentioned composite carbon sources, comprising the following steps: Step 1, In-situ self-assembly of functional agents: Sodium phytic acid grafted lignin sulfonate and polydopamine-coated walnut shell biochar were dispersed in Tris buffer solution at pH 8.0-9.0 and sonicated for 10-20 min; dopamine hydrochloride was added, and the mixture was self-polymerized at 25-35℃ in the dark for 1.5-2.5 h, and the composite microcapsules were collected by centrifugation. Step 2, Precursor preparation: Dissolve the fast-acting carbon core component, sodium carboxymethyl cellulose, and polyvinyl alcohol in deionized water at 75-85℃, and stir to gelatinize for 0.5-1.5h; cool to 40-50℃, add the composite microcapsules obtained in Step 1 and the Fe-Mn-Mo-Se composite trace elements, and homogenize at 8000-12000rpm for 2-5min to form a homogeneous sol; Step 3, Emulsion confined space curing: The homogeneous sol is dropped into liquid paraffin containing Span-80 emulsifier, and high-speed shearing is performed at 10000-15000 rpm for 3-8 min to form a W / O emulsion; the double crosslinking system is slowly added, with the mass ratio of citric acid to polyglycerol glycidyl ether being (2.5-3.5):1, and crosslinking is performed at a constant temperature of 55-65℃ for 3-5 h to form crosslinked microspheres; Step 4, Supercritical CO2 foaming and pore formation: The cross-linked microspheres are washed alternately with ethanol and water, pre-dried at 55-65℃ to a moisture content of 10%-20%; placed in a supercritical CO2 device and saturated at 12-18MPa / 35-45℃ for 1.5-2.5h, followed by rapid depressurization at a rate of 1.5-2.5MPa / min; Step 5, Post-treatment and activation: Vacuum drying, sieving to obtain 1.5-2.5 mm particles; place in simulated wastewater containing denitrifying bacteria, stand at 28-32℃ for 20-28 h for activation, and obtain the composite carbon source.

[0015] Preferably, the preparation process of the phytic acid-grafted sodium lignin sulfonate in step 1 is as follows: dispersing sodium lignin sulfonate in pH In an alkaline aqueous solution of 9.0–10.0 g, epichlorohydrin (EPI) is slowly added dropwise at 50–60 °C for the first stage of pre-activation. The mass ratio of epichlorohydrin to sodium lignosulfonate is (0.3–0.5):1, and the dropping rate does not exceed 0.5 mL / min. The reaction is maintained at this temperature for 1–2 h, allowing the epoxy group of epichlorohydrin to selectively open onto the phenolic hydroxyl group of sodium lignosulfonate to form an ether bond intermediate. Phytic acid is then added, with a mass ratio of phytic acid to sodium lignosulfonate of (0.4–0.6):1. The temperature is raised to 55–65 °C and the reaction is carried out for 3–5 h. The phosphate group of phytic acid acts on the chloromethyl group of the ether bond intermediate through an SN2 substitution reaction, forming a phytic acid-sodium lignosulfonate graft product double-bridged by aryl ether bonds (Ar-OC) and alkyl phosphate bonds (COP). The grafting degree is controlled at 0.4–0.6 mmol / g.

[0016] Furthermore, in the first stage of pre-activation, epichlorohydrin is introduced by slow dropwise addition at a rate not exceeding 0.5 mL / min, and the concentration of NaOH aqueous solution does not exceed 0.5 mol / L, in order to control the self-polymerization side reaction of epichlorohydrin and the ring-closing side reaction of chlorohydrin ether; the mass ratio of epichlorohydrin to sodium lignosulfonate is controlled at (0.3-0.5):1, which is lower than the intermolecular crosslinking threshold of lignin, in order to prevent lignin self-crosslinking.

[0017] Preferably, in step 3, the amount of sorbitan oleate (Span-80) added to the liquid paraffin is 1.5% to 2.5% of the mass of the liquid paraffin; and in step 4, the depressurization rate of the supercritical CO2 is 2.0 ± 0.1 MPa / min.

[0018] Preferably, in step 5, the simulated wastewater containing denitrifying bacteria has a COD of 300–400 mg / L, a TN of 150–200 mg / L, and a pH of 6.8–7.2.

[0019] The present invention also provides an application of the above-mentioned composite carbon source in the denitrification treatment of comprehensive wastewater from electronic panels. The water quality characteristics of the comprehensive wastewater from electronic panels are as follows: COD / TN mass ratio of 1.5 to 3.5, EDTA complexed heavy metals content of 50 to 300 mg / L, fluoride ion concentration of less than 300 mg / L, and alcohol and ketone solvent concentration of less than 100 mg / L. The composite carbon source is added to the biochemical reactor in one go at a dosage that makes the COD / TN ratio in the reactor reach 6.0 to 7.0.

[0020] Preferably, the biochemical reactor is a moving bed biofilm reactor (MBBR) or a fluidized bed reactor, with dissolved oxygen less than 0.5 mg / L and operating temperature of 28–32 °C. After the composite carbon source is added, it operates by rapidly releasing carbon for the first 7 days and then slowly releasing it to a steady state for the next 20 days, maintaining the pH of the microenvironment at the particle-water interface at 6.5–7.5. The phosphate groups of the phytic acid-grafted sodium lignosulfonate form high-density chelating sites at the particle-water interface, which, combined with the catechol groups of the polydopamine-coated walnut shell biochar, rapidly capture free heavy metals, achieving a gradual and synergistic decomposition of EDTA-complexed heavy metals under near-neutral pH conditions.

[0021] Furthermore, the progressive synergistic decomposition includes three synergistic factors: (i) interfacial pH weakening factor: within the particle-water interface pH range of 6.5–7.5, EDTA weakens Cu 2+ The conditional stability constant decreased from an absolute value of 18.80 to 14.8–16.0; (ii) high-density phosphate group mass effect factor: the phosphate groups of the phytic acid-grafted lignin sulfonate sodium are enriched at the particle-water interface, forming a local phosphate site density much higher than that of liquid-phase EDTA; (iii) catechol kinetic capture factor: the catechol groups of the polydopamine-coated walnut shell biochar have an effect on free Cu 2+ It possesses rapid kinetic capture capability, thus improving its capture efficiency. The three factors constitute a positive feedback synergistic cycle. Comparative experiment 3 shows that when the cross-linked slow-release framework and interfacial chelation / capture function are lacking, the total removal rate of Cu / Ni decreases from 78.3% to 41.2%.

[0022] Preferably, the local pH of the biofilm layer on the particle surface is 6.0 to 6.5 as monitored in situ by microelectrodes. At this pH, the conditional stability constant of EDTA for Cu²⁺ is about 14.2, which continuously opens the competitive dissociation window.

[0023] The beneficial effects of this invention are: Compared with the prior art, the present invention has the following outstanding substantive features and significant progress: This invention utilizes the catechol / amino groups of polydopamine (PDA) generated by the self-polymerization of dopamine hydrochloride to form a coordination and hydrogen bond network with the phosphate groups of phytic acid-grafted sodium lignosulfonate (PA-LS), enabling the pre-assembly of detoxification functional components (PA-LS and PDA@WBC) into stable composite microcapsules. When the pH value of the microenvironment at the particle-water interface is stable at 6.5–7.5, EDTA has a significant effect on Cu 2+ The conditional stability constant decreased from an absolute value of 18.80 to 14.8–16.0 (a decrease of 2.8–4.0 log units), opening a thermodynamic window for competitive decomposition. The phosphate groups immobilized by PA-LS form high-density chelate sites at the particle-water interface, driving Cu through mass action effects. 2+ Gradual transfer from EDTA to the interfacial phosphate sites. Free Cu from the transient dissociation of EDTA. 2+ The catechol groups of PDA@WBC rapidly capture and immobilize the Cu, preventing Cu from being trapped and immobilized. 2+ The Cu / Ni is rechelated by EDTA, forming a positive feedback synergistic cycle mechanism of three factors, which increases the total removal rate of Cu / Ni to about 78.3%.

[0024] This invention constructs porous channels by controlling the supercritical CO2 depressurization rate to 2.0 ± 0.1 MPa / min and combining the flexibility and rigidity of a double crosslinking structure with citric acid:PGPE = 3:1. The carbon release curve exhibits a two-stage characteristic of rapid release in the early stage and slow release in the later stage, with a carbon source utilization rate of approximately 89.6%, a TN removal rate of 92.4%, and a specific denitrification rate (SDNR) of approximately 0.54 gN / (gVSS·d).

[0025] This invention utilizes epichlorohydrin-mediated selective two-stage activated etherification grafting to stably anchor phytic acid onto the sodium lignin sulfonate framework. The first stage leverages the strong nucleophilicity of phenolic hydroxyl groups under alkaline conditions to selectively open the EPI epoxy group onto the lignin phenolic hydroxyl group. The second stage couples the phytic acid phosphate group to the chloromethyl group via an SN2 substitution reaction. The resulting aryl ether bond (Ar-OC) and alkyl phosphate bond (COP) exhibit higher hydrolytic stability in alkaline wastewater environments than the phenolic ester bond formed by direct esterification, avoiding the hydrolytic breakage problem of ester bonds under alkaline conditions. The process design of slowly adding EPI and stepwise adding phytic acid effectively suppresses side reactions such as EPI self-polymerization, lignin self-crosslinking, and chlorohydrin ether ring closure, ensuring a stable grafting degree of 0.4–0.6 mmol / g.

[0026] The technical solution of this invention has strong resistance to combined stress and engineering adaptability: PDA@WBC effectively adsorbs and blocks alcohol and ketone solvents, while Fe-Mn-Mo-Se provides metal cofactors and micronutrient support for denitrifying bacteria. The CMC-Na / PVA dual network endows the particles with good mechanical strength, achieving a 96.5% retention rate after 30 days of hydraulic flushing; the system recovers to 90% TN removal rate in less than 8 hours after a pH shock from 5.0 to 9.5. The particle size of 1.5–2.5 mm is directly compatible with mainstream moving bed biofilm reactors (MBBR) / fluidized bed reactors, without requiring modification of existing biological treatment tanks. Attached Figure Description

[0027] Figure 1 This is a comparison chart of the COD carbon release kinetic curves of Example 1 and Comparative Examples 1-4 of the present invention; Figure 2 EDTA-Cu in Example 1 2+ The curve showing the change of Cu morphology distribution over time during the gradual unwinding process. Detailed Implementation

[0028] The embodiments described below are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the technical concepts and practical guidance described in the embodiments of the present invention without inventive effort are within the scope of protection of the present invention. Example 1

[0029] A composite carbon source for electronic panel wastewater, comprising, by dry basis mass percentage: 30% sodium acetate trihydrate, 13% D-glucose, 23% CMC-Na (DS=0.9), 14% PVA-1799, 10% PA-LS, 5% PDA@WBC, 3% citric acid, 1% polyglycerol glycidyl ether, and 1% Fe-Mn-Mo-Se composite trace elements, totaling 100% of all components.

[0030] Preparation method: (1) PA-LS preparation: 10g of sodium lignosulfonate was dispersed in 100mL of deionized water, and the pH was adjusted to 9.5 with 0.3mol / L NaOH aqueous solution. The mixture was heated to 55℃. Under mechanical stirring (300rpm), 3.5g of epichlorohydrin was slowly added dropwise at a rate of 0.4mL / min. After the addition was completed, the mixture was kept at this temperature for 1.5h to complete the first stage of pre-activation, which allowed the EPI epoxy group to selectively open onto the lignin phenolic hydroxyl group, forming the Lignin-O-CH2-CH(OH)-CH2-Cl ether bond intermediate. Subsequently, 5g of phytic acid was added, and the mixture was heated to 60℃ for 4h to carry out the second stage of coupling. The phytic acid phosphate group acted on the chloromethyl group through an SN2 substitution reaction to form a graft product double-bridged by aryl ether bond (Ar-OC) and alkyl phosphate bond (COP).

[0031] The grafted product was insoluble in hot water at 80°C, and phosphorus was not detected in the ethanol washing solution (molybdenum blue colorimetric method), indicating that the phosphate group had been covalently grafted onto the sodium lignosulfonate skeleton; the total phosphorus content of the product was determined by ICP-OES, and the grafting degree was calculated to be 0.48 mmol / g.

[0032] (2) Preparation of PDA@WBC: Walnut shells were washed with deionized water, dried at 105℃, crushed and passed through a 50-mesh sieve, and placed in a nitrogen-protected tube furnace (N2 flow rate 150 mL / min). The temperature was increased to 700℃ at 5℃ / min and held for 3 hours. After natural cooling, walnut shell biochar (WBC) was obtained. 10 g of WBC was dispersed in 1000 mL of dopamine hydrochloride Tris-HCl buffer (dopamine hydrochloride 0.01 mol / L, Tris-HCl 0.05 mol / L, pH 8.5) and self-polymerized at 30℃ in the dark for 24 hours. The product was washed with ethanol and deionized water until no dopamine residue was found. It was then vacuum dried at 60℃ for 12 hours to obtain polydopamine-coated walnut shell biochar (PDA@WBC).

[0033] After the polymerization reaction is completed, the color of the material gradually changes from light brown to dark brown, and its water solubility is significantly lower than that of WBC. After washing with deionized water until the washing liquid no longer stains, it indicates that polydopamine has been coated on the surface of walnut shell biochar.

[0034] (3) Preparation of composite carbon source: Step 1: In-situ self-assembly of functional agents: The prescribed amount of phytic acid-grafted lignin sulfonate sodium and polydopamine-coated walnut shell biochar were dispersed in 0.05 mol / L Tris buffer at pH 8.5 and sonicated for 15 min; dopamine hydrochloride was added (the amount was 2% of the total mass of phytic acid-grafted lignin sulfonate sodium and polydopamine-coated walnut shell biochar, and the polydopamine generated by the self-polymerization of dopamine hydrochloride was included in the PDA@WBC component), and the microcapsules were collected by centrifugation after self-polymerization at 30℃ in the dark for 2 h; Step 2, Precursor preparation: Dissolve the fast-acting carbon core component, sodium carboxymethyl cellulose, and polyvinyl alcohol in deionized water at 80°C and stir to gelatinize for 1 hour; cool to 45°C, add the composite microcapsules obtained in Step 1 and the Fe-Mn-Mo-Se composite trace elements, and homogenize at 10,000 rpm for 3 minutes to form a homogeneous sol. Step 3, Emulsion confined space curing: The homogeneous sol is dropped into liquid paraffin containing 2 wt% Span-80 emulsifier, and high-speed shearing is performed at 12000 rpm for 5 min to form a W / O emulsion; the double crosslinking system is slowly added, with the mass ratio of citric acid to polyglycerol glycidyl ether being 3:1, and crosslinking is performed at 60℃ for 4 h to form crosslinked microspheres; Step 4, Supercritical CO2 foaming and pore formation: The cross-linked microspheres are washed with alternating ethanol / water and pre-dried at 60℃ to a moisture content of 15%; they are placed in a supercritical CO2 device and saturated at 15MPa / 40℃ for 2 hours, and then rapidly depressurized at a rate of 2.0MPa / min. Step 5, Post-treatment and activation: During the washing and pre-drying process of cross-linked microspheres with ethanol / water, they aggregate into millimeter-sized polymers, which are then vacuum dried and sieved to obtain 1.5-2.5 mm particles. The particles are then placed in simulated wastewater containing denitrifying bacteria acclimation solution and activated at 30°C for 24 h to obtain the composite carbon source.

[0035] The resulting particles are brownish-brown spherical with abundant porous channels inside, and the proportion of particles with a diameter of 1.5–2.5 mm is >92%. Example 2

[0036] The method is basically the same as in Example 1, except that: the fast-acting carbon core is adjusted to 27% sodium acetate trihydrate and 15% D-glucose; 24% CMC-Na (DS=0.9); 8% PA-LS and 7% PDA@WBC; the crosslinking system is 2.5% citric acid and 1.0% polyglycerol glycidyl ether (mass ratio 2.5:1); 1.5% Fe-Mn-Mo-Se composite trace elements; the pressure relief rate is 1.8 MPa / min; the remaining components are the same as in Example 1, and the total of all components is 100%. Example 3

[0037] The method is basically the same as in Example 1, except that: the fast-acting carbon core is adjusted to 31% sodium acetate trihydrate and 11% D-glucose; PA-LS 12% and PDA@WBC 3%; the crosslinking system is 3.5% citric acid and 1.0% polyglycerol glycidyl ether (mass ratio 3.5:1); Fe-Mn-Mo-Se composite trace elements 1.5%; the pressure relief rate is 2.2 MPa / min; the remaining components are the same as in Example 1, and the total of all components is 100%.

[0038] Comparative Example 1 (Physical Compound) By weight, 28 parts of sodium acetate trihydrate, 12 parts of D-glucose, 10 parts of humic acid fermentation broth dry powder, 5 parts of attapulgite clay, and 45 parts of deionized water were mechanically mixed and slurried, spray-granulated, and dried with hot air at 80℃ to obtain granules.

[0039] Comparative Example 2 (Single Polymer Sustained-Release Type) Polycaprolactone (PCL) 70%, modified attapulgite (loaded Fe³⁺) 20%, caprolactone coating layer 10%, twin-screw extrusion granulation.

[0040] Comparative Example 3 (simple combination of strong acid complex cleavage and carbon source) Carbon source particles were obtained by physically mixing 28 parts of sodium acetate trihydrate, 12 parts of D-glucose, 10 parts of calcium phytate, and 20 parts of CMC-Na by weight. During addition, the pH of the influent was adjusted to 3.0 with sulfuric acid to break down the complex.

[0041] Comparative Example 4 (Conventional Hole Formation Process) The preparation process is the same as in Example 1, except that the depressurization rate in step 4 is changed to 0.8 MPa / min (conventional slow-release depressurization), and the other conditions remain unchanged.

[0042] Effect verification experiment 1. Experimental system: Pilot-scale SBR-MBBR coupled reactor (50L, MLSS=4500±200mg / L, HRT=12h, DO<0.5mg / L, 30±1℃).

[0043] 2. Simulated wastewater: COD=350±30mg / L, TN=180±15mg / L, Cu-EDTA=80±10mg / L, Ni-EDTA=45±5mg / L, F - =120±15mg / L, isopropanol + acetone =60±8mg / L, pH fluctuation 5.0~9.5.

[0044] 3. Dosing strategy: Based on COD / TN=6.5, add 1.5-2.5mm particles at a time, and take the average value after a 30-day stabilization period (n=3).

[0045] Table 1: Performance Comparison Data of Examples and Comparative Examples

[0046] The experimental results above show that in Example 1, with a depressurization rate of 2.0 MPa / min, the rapid release phase for the first 7 days matched the carbon demand during the denitrifying bacteria's growth period; the slow release phase for the following 20 days maintained a stable COD / TN ratio. In Comparative Example 4, due to excessively slow depressurization (0.8 MPa / min), carbon release degenerated into a single exponential decay, and the carbon source utilization rate plummeted to 72.3%, indicating that a specific depressurization rate and the synergistic effect of the double cross-linked network are key conditions for generating the expected carbon release kinetics. A comparison of the COD carbon release kinetic curves of the present invention and the comparative examples is shown in the figure below. Figure 1 As shown.

[0047] In-situ monitoring using microelectrodes showed that when the pH of the simulated wastewater fluctuated between 5.0 and 9.5, the pH of the water film on the particle surface in Example 1 remained between 6.5 and 7.5, indicating that the CMC-Na / PVA interfacial polymer film provides isolation against external pH fluctuations. Within this pH range, EDTA has a positive effect on Cu... 2+ The conditional stability constant decreased from 18.8 (absolute value) to 14.8–16 (a decrease of 2.8–4 log units), weakening the stability of the EDTA-Cu complex. Simultaneously, the local pH of the biofilm layer on the particle surface was 6.0–6.5, under which the EDTA stability constant was approximately 14.2, continuously opening the competitive decomposition window. The phosphate groups immobilized by PA-LS formed high-density chelation sites at the particle-water interface, driving Cu through mass action. 2+ Gradual transfer from EDTA to the interfacial phosphate sites. Free Cu from the transient dissociation of EDTA. 2+ The catechol groups of PDA@WBC are rapidly captured and immobilized in the porous structure, and the residual free Cu in the liquid phase is determined by ICP-OES. 2+ The calculated capture efficiency is higher than that of Comparative Example 3, effectively preventing Cu 2+ It is rechelated by EDTA. This forms a three-factor positive feedback synergistic cycle system, namely, kinetic capture and removal of free Cu. 2+ This process involves several key aspects: driving a positive shift in the equilibrium of mass action, fully utilizing the pH attenuation window, protecting microbial activity at near-neutral pH, and maintaining the interfacial chemical microenvironment, thereby achieving sustained effectiveness in kinetic capture. For example... Figure 2 As shown, this synergistic mechanism resulted in a total Cu / Ni removal rate of 78.3%, significantly higher than the 41.2% of Comparative Example 3. Comparative Example 3 did not form a cross-linked slow-release framework, and the local pH dropped to the acidic range after addition. Although the EDTA complex was destroyed under acidic conditions, the activity of denitrifying enzyme (NarGHI) was significantly inhibited, and there was no PA-LS interface phosphate site or PDA@WBC kinetic capture, resulting in a total Cu removal rate of only 41.2%.

[0048] Gas chromatography-mass spectrometry (GC-MS) analysis showed that PDA@WBC adsorbed 1.8 mg / g of isopropanol / acetone, reducing the solvent exposure concentration in the biofilm microenvironment. Inductively coupled plasma optical emission spectrometry (ICP-OES) analysis revealed that Fe / Mn / Mo / Se within the particles of Example 1 was slowly released into the liquid phase over 20 days (maintained at the μg / L level), providing metal cofactors for nitrate reductase (Nar) and nitrite reductase (Nir). Under the synergistic effect of the dual cross-linked network, the specific denitrification rate increased to 0.54 gN / (gVSS·d), a 200% increase compared to Comparative Example 1. Although Comparative Example 2 exhibited slow-release properties, the hydrophobic surface of PCL was unfavorable for microbial attachment, resulting in a longer initiation period and weaker shock resistance.

[0049] The present invention has been described in detail above with reference to the embodiments. It should also be noted that the specific technical features described in the above embodiments can be combined and modified in any suitable manner without contradiction. The present invention will not further describe the various possible combinations. Furthermore, other variations and combinations based on the various technical features of the present invention should also be considered as part of the content disclosed in this invention and fall within the protection scope of this invention.

Claims

1. A composite carbon source for electronic panel wastewater, used for denitrification treatment of wastewater, characterized in that, The composite carbon source is in particulate form and comprises the following components by dry weight percentage: (a) Fast-acting carbon nuclei: sodium acetate trihydrate 26%–31%, D-glucose 11%–15%; (b) Sustained-release matrix: sodium carboxymethyl cellulose 21%–25%, polyvinyl alcohol 12%–15%; (c) Detoxifying and depressant agents: 8%–12% phytic acid-grafted sodium lignosulfonate, 3%–7% polydopamine-coated walnut shell biochar; (d) Cross-linking and micronutrients: 3% to 5% of a double cross-linking system composed of citric acid and polyglycerol glycidyl ether, and 0.5% to 1.5% of Fe-Mn-Mo-Se composite trace elements.

2. The composite carbon source as described in claim 1, characterized in that, The composite carbon source particles have porous channels inside, and the overall particle size is 1.5 to 2.5 mm.

3. The composite carbon source as described in claim 1, characterized in that, The phosphate grafting degree of the phytic acid-grafted sodium lignin sulfonate is 0.4–0.6 mmol / g.

4. The composite carbon source as described in claim 1, characterized in that, The degree of substitution (DS) of the sodium carboxymethyl cellulose is 0.8–1.0; the polyvinyl alcohol is PVA-1799; and the mass ratio of Fe, Mn, Mo, and Se in the Fe-Mn-Mo-Se composite trace element is (8–12):(4–6):(0.8–1.2):(0.08–0.12).

5. A method for preparing a composite carbon source as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Step 1, In-situ self-assembly of functional agents: Sodium phytic acid grafted lignin sulfonate and polydopamine-coated walnut shell biochar were dispersed in Tris buffer solution at pH 8.0-9.0 and sonicated for 10-20 min; dopamine hydrochloride was added, and the mixture was self-polymerized at 25-35℃ in the dark for 1.5-2.5 h, and the composite microcapsules were collected by centrifugation. Step 2, Precursor preparation: Dissolve the fast-acting carbon core component, sodium carboxymethyl cellulose, and polyvinyl alcohol in deionized water at 75-85℃, and stir to gelatinize for 0.5-1.5h; cool to 40-50℃, add the composite microcapsules obtained in Step 1 and the Fe-Mn-Mo-Se composite trace elements, and homogenize at 8000-12000rpm for 2-5min to form a homogeneous sol; Step 3, Emulsion confined space curing: The homogeneous sol is dropped into liquid paraffin containing sorbitan oleate Span-80 emulsifier, and high-speed shearing is performed at 10000-15000 rpm for 3-8 min to form a W / O emulsion; the double crosslinking system is slowly added, with the mass ratio of citric acid to polyglycerol glycidyl ether being (2.5-3.5):1, and crosslinking is performed at a constant temperature of 55-65℃ for 3-5 h to form crosslinked microspheres; Step 4, Supercritical CO2 foaming and pore formation: The cross-linked microspheres are washed alternately with ethanol and water, pre-dried at 55-65℃ to a moisture content of 10%-20%; placed in a supercritical CO2 device and saturated at 12-18MPa / 35-45℃ for 1.5-2.5h, followed by rapid depressurization at a rate of 1.5-2.5MPa / min; Step 5, Post-treatment and activation: Vacuum drying, sieving to obtain 1.5-2.5 mm particles; place in simulated wastewater containing denitrifying bacteria, stand at 28-32℃ for 20-28 h for activation, and obtain the composite carbon source.

6. The preparation method according to claim 5, characterized in that, The preparation process of phytic acid-grafted sodium lignosulfonate in step 1 is as follows: sodium lignosulfonate is dispersed in an alkaline aqueous solution with pH 9.0-10.0, and epichlorohydrin is slowly added dropwise at 50-60°C for the first stage of pre-activation, so that the epoxy group of epichlorohydrin selectively ring-opens onto the phenolic hydroxyl group of sodium lignosulfonate to form an ether bond intermediate; then phytic acid is added, and the mass ratio of phytic acid to sodium lignosulfonate is (0.4-0.6):1, and the temperature is raised to 55-65°C for 3-5 hours to form a phytic acid-sodium lignosulfonate graft product double-bridged by aryl ether bonds and alkyl phosphate bonds, with the grafting degree controlled at 0.4-0.6 mmol / g.

7. The preparation method according to claim 5, characterized in that, The amount of sorbitan monooleate Span-80 added in step 3 is 1.5% to 2.5% of the mass of liquid paraffin; the depressurization rate of supercritical CO2 in step 4 is 2.0 ± 0.1 MPa / min.

8. The preparation method according to claim 5, characterized in that, The simulated wastewater containing denitrifying bacteria in step 5 has a COD of 300–400 mg / L, a TN of 150–200 mg / L, and a pH of 6.8–7.

2.

9. The application of a composite carbon source as described in any one of claims 1 to 4 in the denitrification and nitrogen removal treatment of integrated wastewater from electronic panels, characterized in that, The water quality characteristics of the comprehensive wastewater from electronic panels are as follows: COD / TN mass ratio is 1.5-3.5, containing 50-300 mg / L of EDTA-complexed heavy metals, fluoride ion concentration is less than 300 mg / L, and alcohol and ketone solvent concentration is less than 100 mg / L; the composite carbon source is added to the biochemical reactor in one go at a dosage that makes the COD / TN ratio in the reactor reach 6.0-7.

0.

10. The application as described in claim 9, characterized in that, The biochemical reactor is a moving bed biofilm reactor or a fluidized bed reactor, with dissolved oxygen less than 0.5 mg / L and operating temperature of 28–32 °C. After the composite carbon source is added, it is operated with rapid carbon supply for the first 7 days and slow release steady state for the next 20 days, and the pH of the particle-water interface microenvironment is maintained at 6.5–7.5.

Citation Information

Patent Citations

  • A method for preparing a denitrification carbon source

    CN110255712B

  • A composite carbon source for wastewater treatment

    CN113264588B

  • Preparation method and application of denitrification solid slow-release carbon source

    CN116216931A