An electric melting furnace for manufacturing pharmaceutical glass

By introducing electrode protection and corrosion protection mechanisms into the electric melting furnace used in pharmaceutical glass manufacturing, and combining them with a global evaluation model, real-time monitoring and active cooling of the molybdenum electrode and the furnace wall were achieved, solving the problems of molybdenum electrode oxidation and glass melt contamination, and improving production efficiency and safety.

CN123105960APending Publication Date: 2026-11-17HONGGUANG MEDICINE PACKAGING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611610379.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing electric melting furnaces used for pharmaceutical glass manufacturing, the molybdenum electrodes are prone to oxidation during high-temperature and high-load production. Traditional cooling methods are inefficient and cannot effectively prevent the erosion of molten glass, leading to heavy metal spot contamination. Furthermore, the erosion monitoring is delayed, posing a risk of material leakage accidents.

Method used

The system employs an electrode protection mechanism and an erosion protection mechanism, combined with a multi-zone power adjustment module and a global evaluation model, to monitor the erosion status of the electrodes and pool walls in real time. Through medium cooling and power adjustment, it actively freezes the erosion path to prevent heavy metal contamination. Furthermore, it improves heat exchange efficiency through spiral cooling channels and targeted cooling channels, thereby achieving dynamic adaptive sealing.

Benefits of technology

It effectively prevents the oxidation of molybdenum electrodes and contamination of molten glass, improves melting efficiency, avoids heavy metal spots, and ensures the uniformity of molten glass and safe production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105960A_ABST
    Figure CN123105960A_ABST
Patent Text Reader

Abstract

This invention discloses an electric melting furnace for pharmaceutical glass manufacturing, relating to the field of electric melting furnace technology for glass manufacturing. It includes a furnace body, a control system mounted on the furnace body, and a multi-zone power adjustment module electrically connected to the control system. This invention uses a global evaluation model, with boundary erosion risk value as the core control variable, to achieve a fundamental shift from the traditional "single-point passive temperature control priority" to "full furnace boundary safety and thermal field coordination priority." When erosion exceeds the limit, the system actively drives targeted physical freezing in the localized area and forces an active transfer of the entire furnace thermal field load, ensuring that the electric melting furnace's operating state meets the requirements for leak prevention and contamination prevention. By establishing a three-dimensional mapping of the physical boundary at the control system level, process engineers can directly monitor the invisible erosion situation below the 1600℃ liquid surface online, thereby avoiding the risk of heavy metal contamination of the molten glass and maintaining the stable temperature field required for molten glass homogenization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electric melting furnace technology for glass manufacturing, and specifically to an electric melting furnace for manufacturing pharmaceutical glass. Background Technology

[0002] The safety of pharmaceutical packaging materials is directly related to the health and lives of the people. In recent years, with the upgrading of my country's pharmaceutical industry, the traditional high-energy-consuming industry is being transformed into the manufacturing of new special materials. The high-end pharmaceutical glass industry, represented by 5.0 neutral borosilicate glass, has ushered in rapid development. 5.0 neutral borosilicate glass has excellent chemical stability and thermal shock resistance, but its formula contains high levels of boron oxide and aluminum oxide, resulting in extremely high melting temperatures (usually between 1600℃ and 1650℃). Moreover, the glass melt has high viscosity and is extremely chemically corrosive to furnace materials. Currently, high-quality pharmaceutical glass is usually melted in a fully electric furnace with a "cold top". The fully electric furnace mainly relies on the direct Joule heating of molybdenum electrodes inserted into the glass melt.

[0003] However, in actual high-temperature and high-load production, existing technologies face the following insurmountable technical bottlenecks: molybdenum electrodes are highly susceptible to oxidation in oxygen-rich environments exceeding 400°C. At the glass melt interface at 1600°C, traditional electrode protection typically relies solely on externally installed circulating water jackets for crude cooling. This simple surface heat exchange is not only inefficient but also prone to localized boiling and scaling within the water jacket, failing to effectively prevent the highly active borosilicate glass melt from physically scouring and penetrating the electrode root. Once the molybdenum electrode suffers severe erosion and peeling, the resulting tiny molybdenum particles directly mix into the glass melt, causing heavy metal spots in pharmaceutical glass. This is an irreparable and fatal flaw for pharmaceutical packaging, which has extremely stringent standards. Furthermore, traditional electrode propulsion mechanisms are mostly rigid mechanical propulsion, lacking the ability to sensitively detect microscopic erosion displacement. Often, operators only notice the problem after the electrode has already suffered severe wear or even caused a leakage accident, resulting in significant lag and blindness. Summary of the Invention

[0004] The purpose of this invention is to provide an electric melting furnace for manufacturing pharmaceutical glass, so as to solve the problems in the background art mentioned above.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: An electric melting furnace for manufacturing pharmaceutical glass includes a furnace body, a control system mounted on the furnace body, and a multi-zone power adjustment module electrically connected to the control system; it also includes a top cover, rotatably connected to the top of the furnace body, for forming a closed melting chamber together with the furnace body. Electrode protection mechanism: Several electrode protection mechanisms are fixedly installed in a ring at equal intervals at the bottom of the furnace body, and one end of the electrode protection mechanism extends into the interior of the furnace body for electrically heating the material in the melting chamber. The electrode protection mechanism has an independent medium cooling channel. The corrosion protection mechanism is fixedly installed on the top of the furnace body and is set at the liquid level in the melting chamber. It is used to monitor the corrosion status of the furnace wall structure at the liquid level. The corrosion protection mechanism has a three-dimensional conductive wire matrix and a regional targeted cooling channel. The control system is equipped with a solid-state boundary cooperative protection unit, which is configured to perform the following steps: Acquire the electrode working electrical parameter signals fed back in real time by the electrode protection mechanism, as well as the pool wall circuit break signal output by the three-dimensional conductive wire matrix in the erosion protection mechanism; Based on the electrode working electrical parameter signal and the pool wall open circuit signal, the regional melting efficiency index, which characterizes the heat absorption and convection state of the glass melt in each region of the furnace, is calculated in real time, and the boundary erosion risk value, which characterizes the erosion depth of the electrode neck and the degree of spalling of the refractory material of the pool wall, is calculated simultaneously. The preset global evaluation model is invoked. The global evaluation model includes a positive weight term for the regional melting efficiency index and a negative penalty term for the boundary erosion risk value. When the boundary erosion risk value or the regional melting efficiency index deviates from the preset safety and process threshold, a global thermal field reconstruction instruction is generated based on the global evaluation model. The global thermal field reconstruction command drives the corresponding electrode protection mechanism and erosion protection mechanism to adjust the flow rate of the cooling medium inside them, so as to cut off the erosion path through physical freezing of the interface, thereby inhibiting the precipitation of heavy metals and refractory material impurities and contamination of the medical glass melt; at the same time, the multi-zone power adjustment module is synchronously driven to dynamically adjust the input power of the electrode protection mechanism in each zone and perform iterative optimization. Under the constraint of prioritizing the reduction of boundary erosion risk penalty, the stable temperature field required for glass homogenization and bubble removal is maintained by actively transferring the heat field load of the entire furnace, thereby maximizing the sum of the weighted terms of the regional melting efficiency index of the entire furnace.

[0006] A further improvement of the technical solution of the present invention is that: the regional melting efficiency index includes at least the actual input electrical power of the electrode protection mechanism in each region; the boundary erosion risk value includes at least the electrode end erosion depth calculated from the electrode working electrical parameter signal, and the pool wall spalling depth calculated from the three-dimensional conductive wire matrix open circuit signal. The construction logic of the global evaluation model is as follows: set a comprehensive threshold for safety and process; When both the electrode tip erosion depth and the pool wall spalling depth are less than the combined safety and process threshold, the penalty weight of the boundary erosion risk value approaches zero. The global thermal field reconstruction command aims to maximize the sum of the melting efficiency indicators of the entire furnace area, driving each electrode protection mechanism to operate close to the maximum value within its rated safe power range, so as to maintain efficient glass melt melting and homogenization. When the erosion depth at any electrode tip or the spalling depth of the pool wall exceeds the combined safety and process threshold, the penalty weight of the boundary erosion risk value increases rapidly and non-linearly, and the global thermal field reconstruction command is forced to prioritize curbing the erosion rate and preventing impurity precipitation. The control system forcibly drives the electrode protection mechanism or erosion protection mechanism corresponding to the damaged coordinate to increase the flow rate of the cooling medium in order to implement local phase change freezing at the interface; at the same time, it actively reduces the input power of the electrode protection mechanism in the damaged area and transfers the heat load to the other electrode protection mechanisms in a safe state, so as to ensure the processing uniformity of the pharmaceutical glass melt while compensating for the lack of local thermal field, until the increase in the erosion depth of the electrode tip and the peeling depth of the pool wall returns to the comprehensive threshold range of safety and process.

[0007] A further improvement of the technical solution of the present invention is that: the electrode protection mechanism includes an installation sleeve that is fixedly installed at equal intervals at the bottom of the furnace body. An inner cylinder is coaxially fixed inside the installation sleeve. An electrode body is inserted through the inner cylinder. The heating end of the electrode body extends into the melting chamber to perform Joule heating on the material. The wiring end of the electrode body extends to the outside of the furnace body and is electrically connected to the multi-zone power adjustment module. The inner cylinder has a spiral hole extending in a spiral shape. Two connecting pipes are symmetrically connected to one end of the inner cylinder located on the outer wall of the furnace body. The two connecting pipes are respectively connected to the medium inlet end and the medium outlet end of the spiral hole to form an independent medium cooling channel and be controlled by the global thermal field reconstruction command.

[0008] A further improvement of the technical solution of the present invention is that: the inner wall of the inner cylinder is provided with a plurality of permeation holes at equal intervals and through the central axis, and the inlet end of each permeation hole is connected to the interior of the spiral hole. The outlet end of the permeation hole is configured to direct the cooling medium flowing inside the spiral hole and spray it to the assembly gap between the inner cylinder and the electrode, so that the high-temperature glass liquid leaking outward along the assembly gap will undergo phase change and condense when it comes into contact with the cooling medium, thereby constructing a solid glass sealing barrier in situ within the assembly gap.

[0009] A further improvement of the technical solution of the present invention is that: the corrosion protection mechanism includes a mounting ring conformally embedded in the liquid level area of ​​the inner wall of the furnace body. The interior of the mounting ring has a number of alloy wires embedded in a spatial grid array to form a three-dimensional conductive wire matrix. Each alloy wire is electrically connected to the control system through an independent circuit. The outer wall cold side of the furnace body corresponding to the mounting ring has a number of mounting seats fixed in a ring array. The mounting seats have conduits for conveying cooling medium fixedly inserted inside. A number of nozzles are equidistantly arranged on the conduits facing the outer wall of the furnace body. The conduits and each nozzle are connected to each other and together form a regional targeted cooling channel.

[0010] A further improvement of the technical solution of the present invention is that the alloy wire is made of high-temperature resistant platinum-rhodium alloy material. When it comes into direct contact with the high-temperature glass melt along with the refractory material of the surrounding pool wall being eroded and peeled off, it undergoes irreversible melting, so as to accurately characterize the pool wall erosion boundary at the melting point and trigger the pool wall open circuit signal.

[0011] A further improvement of the technical solution of the present invention is that the base material of the mounting ring is the same as the refractory material of the inner wall of the furnace. When the mounting ring faces the thermodynamic erosion and chemical erosion of the high-temperature glass melt, its own physical erosion rate is synchronized with the erosion rate of the surrounding furnace wall, so as to ensure that the erosion boundary characterized by the melting of the alloy wire is equivalent.

[0012] A further improvement of the technical solution of the present invention is that: the spray axis of the nozzle is inclined at an upward angle of 30°, the bottom wall of the inner cavity of the mounting base is constructed with an inclined fluid guiding surface, the fluid guiding surface is configured to directionally collect and drain the cooling medium and condensate after phase change heat transfer, so as to prevent water accumulation inside the mounting base, and the top of the mounting base is hinged with an openable cover plate, which, when closed, together with the outer wall of the mounting base and the furnace body, forms a relatively sealed targeted cooling chamber.

[0013] Due to the adoption of the above technical solution, the technical progress achieved by this invention compared to the prior art is as follows: 1. This invention uses boundary erosion risk value as the core control variable and a global evaluation model to achieve a fundamental shift from the traditional "single-point passive temperature control priority" to "full furnace boundary safety and thermal field coordination priority". When erosion exceeds the limit, the system will actively drive local targeted physical freezing and force active transfer of the entire furnace thermal field load to ensure that the electric melting furnace operation meets the leakage prevention and pollution prevention limits. By establishing a three-dimensional mapping of the physical boundary at the control system end, process personnel can directly monitor the invisible erosion situation below the 1600℃ liquid surface online, thereby avoiding the risk of heavy metal contamination of the glass melt and maintaining the stable temperature field required for glass melt homogenization.

[0014] 2. This invention, by setting spiral holes extending in a spiral shape in the inner cylinder of the electrode protection mechanism, forces the cooling medium to undergo high-speed spiral centrifugal motion, which destroys the thermal boundary layer of the tube wall and greatly improves the turbulent heat transfer coefficient; by using centrifugal force to quickly peel off any tiny bubbles that may be generated from the tube wall, it fundamentally eliminates the scaling phenomenon caused by local nucleation boiling, ensuring the long-term unobstructed cooling channel, thereby providing a reliable hydrodynamic guarantee for the subsequent precise interface freezing at the electrode root.

[0015] 3. This invention uses permeation holes to directionally spray high-pressure cooling medium into the micro-assembly gap, forcing the outward leakage of high-temperature molten glass to undergo phase change and condense, thus constructing a high-viscosity solid glass sealing ring in situ within the gap. The process medium itself achieves dynamic adaptive sealing with "replenishment as it is damaged", cutting off the bidirectional path of external oxygen entering and liquid glass seeping out, thereby avoiding the oxidation and pulverization of the molybdenum electrode at high temperatures, and further preventing the highly corrosive molten glass from peeling and scouring the electrode root.

[0016] 4. This invention pre-embeds a three-dimensional grid-like arrangement of platinum-rhodium alloy wires inside the mounting ring, which is made of the same material as the furnace wall. By utilizing the sacrificial physical melting of the alloy wires when in contact with the high-temperature molten glass, the erosion state is transformed into an intuitive binary electrical signal on / off state. This eliminates the signal lag and measurement reference drift caused by thermal inertia, which not only gives the system positioning reliability, but also avoids the secondary disaster of glass discoloration caused by the melting of conventional sensors.

[0017] 5. This invention locks the latent heat of phase change of the cooling medium in the local hot spot area where erosion occurs by setting a nozzle with a 30° tilt angle on the outer wall of the furnace body and a closed targeted cooling chamber, thus implementing spatial point-to-point directional physical cooling; combined with the unidirectional drainage mechanism of the fluid guiding surface to prevent water accumulation, it not only successfully curbs the erosion rate of the pool wall, but also avoids the serious cold end effect caused by traditional large-area water spraying cooling of the entire furnace wall, thereby minimizing the interference with the overall temperature field and homogenization defoaming process inside the furnace. Attached Figure Description

[0018] The invention will now be further described with reference to the accompanying drawings.

[0019] Figure 1 This is a first-view structural diagram of the overall device of the present invention; Figure 2 This is a second-view structural diagram of the overall device of the present invention; Figure 3 This is a first-view structural schematic diagram of the electrode protection mechanism of the present invention; Figure 4 This is a schematic diagram of the electrode protection mechanism of the present invention from a second perspective. Figure 5This is a first-view structural diagram of the erosion protection mechanism of the present invention; Figure 6 This is a second-view structural schematic diagram of the erosion protection mechanism of the present invention.

[0020] In the diagram: 1. Furnace body; 2. Top cover; 3. Electrode protection mechanism; 4. Erosion protection mechanism; 5. Mounting sleeve; 6. Inner cylinder; 7. Electrode body; 8. Spiral hole; 9. Permeation hole; 10. Connecting pipe; 11. Mounting ring; 12. Alloy wire; 13. Mounting base; 14. Conduit; 15. Nozzle; 16. Guide surface; 17. Cover plate. Detailed Implementation

[0021] The present invention will be further described in detail below with reference to the embodiments.

[0022] Example 1 like Figures 1-6 As shown, the present invention provides an electric melting furnace for manufacturing pharmaceutical glass, including a furnace body 1, a control system disposed on the furnace body 1, and a multi-zone power adjustment module electrically connected to the control system; it also includes a top cover 2, which is rotatably connected to the top of the furnace body 1 and is used to form a closed melting chamber together with the furnace body 1. Electrode protection mechanism 3, several electrode protection mechanisms 3 are fixedly installed in a ring at equal intervals at the bottom end of the furnace body 1, and one end of the electrode protection mechanism 3 extends into the interior of the furnace body 1, for electrically heating the material in the melting chamber. The electrode protection mechanism 3 has an independent medium cooling channel. The erosion protection mechanism 4 is fixedly installed at the top of the furnace body 1 and is set at the liquid level in the melting chamber. It is used to monitor the erosion status of the furnace wall structure at the liquid level. The erosion protection mechanism 4 is pre-embedded with a three-dimensional conductive wire matrix and has a regional targeted cooling channel. The control system is equipped with a solid-state boundary cooperative protection unit, which is configured to perform the following steps: The electrode working electrical parameter signal fed back in real time by the electrode protection mechanism 3, and the pool wall circuit break signal output by the three-dimensional conductive wire matrix in the erosion protection mechanism 4 are obtained. Based on the electrode working electrical parameter signal and the pool wall open circuit signal, the regional melting efficiency index, which characterizes the heat absorption and convection state of the glass melt in each region of the furnace, is calculated in real time, and the boundary erosion risk value, which characterizes the erosion depth of the electrode neck and the degree of spalling of the refractory material of the pool wall, is calculated simultaneously. The preset global evaluation model is invoked. The global evaluation model includes a positive weight term for the regional melting efficiency index and a negative penalty term for the boundary erosion risk value. When the boundary erosion risk value or the regional melting efficiency index deviates from the preset safety and process threshold, a global thermal field reconstruction instruction is generated based on the global evaluation model. The global thermal field reconstruction command drives the corresponding electrode protection mechanism 3 and erosion protection mechanism 4 to adjust the flow rate of the cooling medium inside them, so as to cut off the erosion path through physical freezing of the interface, thereby inhibiting the precipitation of heavy metals and refractory material impurities and contamination of the medical glass melt; at the same time, the multi-zone power adjustment module is synchronously driven to dynamically adjust the input power of the electrode protection mechanism 3 in each zone and perform iterative optimization. Under the constraint of prioritizing the reduction of boundary erosion risk penalty, the stable temperature field required for glass homogenization and bubble removal is maintained by actively transferring the heat field load of the entire furnace, thereby maximizing the sum of the weighted terms of the regional melting efficiency index of the entire furnace.

[0023] In this embodiment, by using the boundary erosion risk value as the core control variable, a global evaluation model is used to achieve a fundamental shift from the traditional "single-point passive temperature control priority" to "full furnace boundary safety and thermal field coordination priority." Pharmaceutical glass (such as 5.0 neutral borosilicate glass) is extremely sensitive to impurities. When localized refractory material or molybdenum electrode erosion occurs, the system actively intervenes, forcibly reconstructing the global thermal field distribution and implementing targeted physical freezing to ensure that the electric melting furnace's operating status meets extremely stringent heavy metal contamination-free requirements. By simulating the physical wear mechanism of the furnace wall and electrodes at the equipment end, process engineers can directly monitor the invisible erosion below the 1600℃ liquid surface online, fundamentally eliminating the risk of furnace leakage or glass melt contamination.

[0024] Specifically, the solid-state boundary cooperative protection unit configured within the control system is a core algorithm module running in an industrial computer or PLC, and it is specifically configured to execute the following steps: Step S1: Obtaining the underlying physical state The control system collects the electrical parameter signals of the electrodes in the 3 circuits of each electrode protection mechanism in real time (including voltage, current and micro impedance variation values, the nonlinear drift of the electrical parameters accurately characterizes the end consumption state of the molybdenum electrode under the scouring of high temperature glass melt), and at the same time receives the pool wall open circuit signal output by the three-dimensional conductive wire matrix in the erosion protection mechanism 4 in real time (characterizing the physical spalling of refractory material under specific spatial coordinates).

[0025] Step S2: Calculation of Composite Core Indicators Based on the acquired underlying signals, the system calculates two sets of core indicators in real time: First, the regional melting efficiency index: based on the actual input power and temperature rise curve of the electrodes in each region, the efficiency value characterizing the heat absorption and convection activity of the glass melt in each region of the furnace is calculated. Second, boundary erosion risk value: Simultaneously calculate the quantitative risk value that characterizes the erosion depth of the electrode neck and the degree of spalling of the refractory material in the pool wall. This is the core bias factor that causes "stones" and "heavy metal spots" to form in medical glass.

[0026] Step S3: Construction of Global Evaluation Model The system calls a preset global evaluation model to construct a comprehensive scoring function with multiple objectives. This model sets the zone melting efficiency index as a positive gain weight term (encouraging the system to pursue higher glass melting speed) and sets the boundary erosion risk value as a negative penalty term (constraining the system to ensure the safety of the furnace hardware). The system defines control guidelines under different erosion levels through algorithms to ensure that there are clear judgment boundaries when the two processes conflict.

[0027] Step S4: Thermal Field Linkage Correction and Iterative Optimization When the boundary erosion risk value or the regional melting efficiency index deviates from the preset safety and process thresholds, the control system generates a global thermal field reconstruction command based on the above model and executes a hardware and software coordinated optimization operation: 1. Physical barrier (anti-pollution): Drive the electrode protection mechanism 3 and the corrosion protection mechanism 4 corresponding to the damaged coordinate to precisely adjust the flow rate of the cooling medium inside them. Utilize the latent heat of phase change to quickly build a solid glass stagnation layer (physical freezing) at the damaged corrosion interface, forcibly cutting off the further corrosion path of the glass melt, thereby completely inhibiting the precipitation of heavy metals (molybdenum) and refractory material impurities and preventing them from contaminating the medical glass melt.

[0028] 2. Heat transfer (homogenization): While implementing forced cooling in a localized area, the multi-zone power regulation module is driven simultaneously to dynamically reduce the electrode power in the damaged area and actively transfer the heat load to the remaining electrode protection mechanism 3, which is in a safe state.

[0029] Through the above closed-loop iterative optimization, under the mandatory constraint of prioritizing the reduction of the boundary erosion risk value penalty term, the system uses the active transfer of the entire furnace thermal field load to fill the local cold end effect, maintains the stable temperature field required for the homogenization and defoaming of pharmaceutical glass, and ultimately maximizes the sum of the weight terms of the regional melting efficiency index of the entire furnace.

[0030] like Figure 1 and Figure 2 As shown, preferably, the regional melting efficiency index includes at least the actual input electrical power of the electrode protection mechanism 3 in each region; the boundary erosion risk value includes at least the electrode end erosion depth calculated from the electrode working electrical parameter signal, and the pool wall spalling depth calculated from the three-dimensional conductive wire matrix open circuit signal. The construction logic of the global evaluation model is as follows: set a comprehensive threshold for safety and process; When both the electrode tip erosion depth and the pool wall spalling depth are less than the combined safety and process threshold, the penalty weight of the boundary erosion risk value approaches zero. The global thermal field reconstruction command aims to maximize the sum of the melting efficiency indicators of the entire furnace area, driving each electrode protection mechanism 3 to operate close to the maximum value within its rated safe power range, so as to maintain efficient glass melt melting and homogenization. When the erosion depth at any electrode tip or the spalling depth of the pool wall exceeds the combined safety and process threshold, the penalty weight of the boundary erosion risk value increases rapidly and non-linearly, and the global thermal field reconstruction command is forced to prioritize curbing the erosion rate and preventing impurity precipitation. The control system forcibly drives the electrode protection mechanism 3 or erosion protection mechanism 4 corresponding to the damaged coordinate to increase the flow rate of the cooling medium in order to implement local phase change freezing at the interface; at the same time, it actively reduces the input power of the electrode protection mechanism 3 in the damaged area and transfers the heat load to the other electrode protection mechanisms 3 in a safe state, so as to ensure the processing uniformity of the pharmaceutical glass melt while compensating for the lack of local thermal field, until the increase in the erosion depth of the electrode tip and the peeling depth of the pool wall returns to the comprehensive threshold range of safety and process.

[0031] In this embodiment, to implement the above-mentioned multi-objective optimization logic, the formula for constructing the global evaluation model is as follows:

[0032] in: This represents the overall operational score under the current hot and cool conditions. This represents the total number of heating zones. This represents the current regional melting efficiency index for region i. This is a preset process weighting constant; A dynamic penalty term function for the boundary erosion risk value; The system has a preset safety margin threshold. Based on the relationship between the real-time calculated boundary erosion risk value R and this threshold, the system executes a segmented control strategy: 1. Efficiency-first region (safe state): When R < (i.e., both electrode mechanical consumption and pool wall spalling are within safety tolerances), dynamic penalty term function The output value approaches zero. At this point, the global score... Mainly determined by the first part of the formula (efficiency term), the control system exhibits the characteristic of prioritizing melting efficiency. The global thermal field reconstruction command drives each molybdenum electrode to operate close to its maximum value within its rated safe power range. Even if this leads to a small, expected uniform loss in the refractory material, the system will tolerate it to ensure efficient defoaming and homogenization of 5.0 neutral borosilicate glass.

[0033] 2. Forced Correction Zone (High-Risk State): When R When the erosion of any electrode or pool wall exceeds the safety limit, the penalty term weight increases rapidly and non-linearly, and its functional relationship adopts an exponential growth model.

[0034] (In the formula, e is the natural constant, and k and m are preset penalty gain constants). Once the threshold is exceeded, the penalty value increases instantly, affecting the global score. The temperature drops precipitously. At this point, the evaluation model is absolutely dominated by the penalty term, and the optimization direction generated by the control system is forcibly reversed. A thermal field reconstruction command with the highest priority of reducing the boundary erosion rate is generated. The specific execution process of iterative optimization (forced correction mode) is as follows: In the forced correction zone, the control logic of the control system deviates from the conventional PID temperature control and directly executes physical isolation and load transfer: Targeted physical freezing: The control system forcibly drives the proportional servo valve of the spiral infiltration cooling unit or the targeted cooling grid at the damaged coordinate to fully open, using the latent heat of phase change of the cooling medium to forcibly generate and maintain a solid glass stagnant layer at the erosion interface. Full furnace load transfer: The input power of the molybdenum electrode in the damaged area is simultaneously and actively reduced (to reduce the local hot fluid convection scouring), and the missing heat load is transferred to the other healthy electrodes in the furnace in the "efficiency priority zone" according to the preset thermal field coupling matrix. The above forced correction process continues until the erosion rate fed back by the displacement loop signal or the conductive wire matrix at the bottom stops increasing, and the boundary erosion risk value R returns to the safety margin threshold. Within the specified range, the control system re-enters the monitoring of the regional melting efficiency index. Optimization calculation.

[0035] Example 2 like Figure 3 and Figure 4 As shown, based on Embodiment 1, the present invention provides a technical solution: Preferably, the electrode protection mechanism 3 includes an installation sleeve 5 fixedly installed at equal intervals at the bottom of the furnace body 1. An inner cylinder 6 is coaxially fixed inside the installation sleeve 5. An electrode body 7 is inserted through the inner cylinder 6. The heating end of the electrode body 7 extends into the melting chamber to perform Joule heating on the material. The wiring end of the electrode body 7 extends to the outside of the furnace body 1 and is electrically connected to the multi-zone power adjustment module. The inner cylinder 6 has a spiral hole 8 extending in a spiral shape. Two connecting pipes 10 are symmetrically connected to one end of the inner cylinder 6 located on the outer wall of the furnace body 1. The two connecting pipes 10 are respectively connected to the medium inlet end and the medium outlet end of the spiral hole 8 to jointly form an independent medium cooling channel and be controlled by the global thermal field reconstruction command.

[0036] In this embodiment, the mounting sleeve 5 serves as a pressure-bearing structural component, rigidly anchoring the entire assembly to the bottom wall of the furnace body 1. The inner cylinder 6 serves as a thermal insulation and heat exchange interface, coaxially sleeved outside the electrode body 7. The electrode body 7 is driven by an external power source (multi-zone power adjustment module), releasing a large current at the exposed end extending into the glass melt, utilizing the conductivity of the glass melt to generate Joule heat. When the control system issues a thermal field reconstruction command, the external cooling medium (soft water or heat transfer oil) is pumped into the inner cylinder 6 through one of the connecting pipes 10. The cooling medium is forced to flow in a high-speed spiral around the axis along the spiral holes 8 under the action of pump pressure, fully absorbing the high heat conducted at the root of the electrode body 7, and then discharged through the connecting pipe 10 at the other end, forming a closed-loop independent cooling channel. Traditional straight-tube water jackets, due to their large cross-section and low flow velocity, are prone to localized nucleation boiling (vaporization) at the end near 1600℃, leading to a surge in thermal resistance and severe scaling. This solution designs the flow channel as a spiral-shaped extension of spiral holes 8, which significantly increases the fluid flow and heat exchange area while forcing the fluid to undergo high-speed spiral centrifugal motion. This not only disrupts the thermal boundary layer of the pipe wall and greatly improves the turbulent heat transfer coefficient, but also uses centrifugal force to quickly peel off any tiny bubbles that may be generated from the pipe wall, fundamentally eliminating localized boiling and scaling, and ensuring long-term unobstructed cooling channels. This localized cooling causes the highly corrosive neutral borosilicate glass liquid to undergo a phase change and condense in situ when attempting to penetrate outwards through the gaps, transforming into a high-viscosity, high-hardness solid glass sealing ring. This solid ring not only forms an ultimate physical seal, completely blocking the continuous scouring and chemical erosion of the electrode body 7 by the liquid glass, but also prevents the peeling off of oxides from the source.

[0037] like Figure 3 and Figure 4 As shown, preferably, the inner wall of the inner cylinder 6 is provided with a plurality of permeation holes 9 equidistantly and through it around its central axis, and the inlet end of each permeation hole 9 is connected to the interior of the spiral hole 8; the outlet end of the permeation hole 9 is configured to direct the cooling medium flowing in the spiral hole 8 to the assembly gap between the inner cylinder 6 and the electrode body 7, so that the high-temperature glass liquid leaking outward along the assembly gap will undergo phase change and condense when it comes into contact with the cooling medium, thereby constructing a solid glass sealing barrier in situ within the assembly gap.

[0038] In this embodiment, during the mechanical assembly process, there is an unavoidable microscopic assembly gap (fitting tolerance) and a hot clearance caused by the difference in thermal expansion coefficients between the inner cylinder 6 and the electrode body 7. When a pressurized cooling medium is introduced into the spiral hole 8, the high-pressure fluid will generate a throttling effect through the equidistantly distributed permeation holes 9, forming several tiny jets that are directed into the microscopic assembly gap. Under the operation of the electric furnace, the liquid glass in the melting chamber, which reaches 1600°C, will attempt to leak outwards (cold end) along the assembly gap under the drive of the hydrostatic pressure in the furnace. At this time, the cooling medium sprayed out through the permeation holes 9 will directly meet the high-temperature glass liquid that is leaking outwards. The cooling medium will use its latent heat of vaporization or convective heat transfer to instantly remove the sensible heat of the glass liquid, forcing the temperature of the high-temperature glass liquid at the interface to drop sharply below its softening point (transition temperature), and the low-viscosity Newtonian fluid will instantly undergo a phase change and condense into a high-hardness amorphous solid, thereby completely physically blocking the assembly gap. Traditional packing seals or mechanical seals are prone to failure under extreme high-temperature thermal alternation. This solution utilizes the process medium (the molten glass itself) as the sealing material to construct a "dynamic self-healing" barrier. When the electrode body 7 undergoes mechanical displacement due to operation or deformation of the assembly gap caused by thermal expansion and contraction, the old solid glass ring may shatter. However, once the new molten glass seeps in, it will immediately undergo phase change and solidify again under the jet cooling of the permeation hole 9. This "repair as it is damaged" physical mechanism achieves a reliable flexible dynamic seal mechanically. The solid glass sealing barrier constructed by the permeation hole 9 has a bidirectional blocking effect. Inward, it completely cuts off the path for external air (oxygen) to enter the high-temperature zone through the assembly gap, preventing severe oxidation and pulverization of the molybdenum electrode body 7 above 400°C. Outward, it prevents the highly corrosive liquid medical glass from continuously scouring and peeling off the electrode root, ensuring that no heavy metal molybdenum particles are mixed into the molten glass.

[0039] Example 3 like Figure 5 and Figure 6 As shown, based on Embodiment 1, the present invention provides a technical solution: Preferably, the corrosion protection mechanism 4 includes a mounting ring 11 conformally embedded in the liquid level area of ​​the inner wall of the furnace body 1. The interior of the mounting ring 11 is pre-embedded with a number of alloy wires 12 in a spatial grid array to form a three-dimensional conductive wire matrix. Each alloy wire 12 is electrically connected to the control system through an independent circuit. A number of mounting seats 13 are fixed in a ring array on the cold side of the outer wall of the furnace body 1 corresponding to the mounting ring 11. A conduit 14 for conveying cooling medium is fixedly inserted inside the mounting seat 13. A number of nozzles 15 are equidistantly arranged on the conduit 14 facing the outer wall of the furnace body 1. The conduit 14 and each nozzle 15 are connected to each other and together form a regional targeted cooling channel.

[0040] In this embodiment, the liquid level surface of the pharmaceutical glass electric melting furnace is a solid-liquid-gas "three-phase interface", which is the area most severely affected by the scouring and chemical corrosion of the glass melt. The mounting ring (11) is set to coincide with the liquid level surface. The several alloy wires 12 embedded inside it form a three-dimensional rectangular or polar coordinate grid of X, Y, Z in space. When the inner wall of the mounting ring 11 facing the melting chamber is eroded and peeled off, causing the alloy wire 12 at a certain spatial depth to be directly exposed to the high temperature glass melt and melt, the control system instantly captures the circuit break signal, thereby accurately locating the three-dimensional coordinates and depth geometry of the erosion pit in physical space. The nozzle 15 array on the cold side outer wall of the furnace body 1 has a mapping relationship with the alloy wire 12 matrix on the inner wall in physical space. When the control system captures the erosion limit signal of the local coordinate through the above-mentioned three-dimensional conductive wire matrix, it immediately generates a region reconstruction command and opens the electromagnetic servo valve on the conduit 14 at the corresponding coordinate. The nozzle 15 at a specific location then sprays cooling micro-mist onto the outer wall of the furnace body 1 corresponding to the damaged coordinate, implementing spatial point-to-point directional physical cooling; Traditional furnace wall monitoring relies solely on thermocouples embedded within the refractory bricks, providing only single-dimensional temperature data with significant latency and failing to determine the actual thinning of the refractory bricks. This solution utilizes an array of three-dimensional conductive wires to physically fuse the erosion process, transforming the erosion state into a direct electrical signal on / off state. Within the control system, a true three-dimensional model of the erosion boundary is reverse-mapped and topologically constructed. This physical coordinate-level detection accuracy provides fundamental data support for subsequent thermal field reconstruction. If conventional methods of large-area water cooling across the entire furnace wall are used when erosion occurs, it will lead to... A sudden drop in edge temperature can cause severe glass melt congealing or crystallization defects (i.e., cold end effect), disrupting the homogenization process. This solution achieves thermodynamic micro-management through a "targeted cooling channel": external spraying is only applied to the coordinate area where erosion and spalling occur. The latent heat of phase change of the 15 micro-mist nozzle is used to rapidly remove the heat from the local erosion point and form a solid glass stagnant layer on the inner wall surface. Meanwhile, the undamaged healthy area remains insulated. This targeted external cooling mechanism successfully curbs pool wall erosion and prevents furnace leakage while minimizing interference with the overall temperature field and glass melting convection process inside the furnace.

[0041] like Figure 5 and Figure 6 As shown, preferably, the alloy wire 12 is made of high-temperature resistant platinum-rhodium alloy. When it comes into direct contact with the high-temperature molten glass along with the refractory material of the surrounding pool wall being eroded and peeled off, it undergoes irreversible melting, so as to accurately characterize the pool wall erosion boundary at the melting point and trigger the pool wall open circuit signal.

[0042] In this embodiment, the platinum-rhodium alloy has excellent initial high-temperature resistance characteristics and can be stably embedded in the refractory brick to withstand normal high-temperature heat conduction. However, when the furnace wall refractory material undergoes substantial chemical erosion and physical spalling due to long-term service, the embedded alloy wire 12 loses the protection of the refractory layer and is directly exposed and immersed in molten pharmaceutical glass at temperatures above 1600°C. The ultra-high temperature thermal shock and strong corrosive chemical field of the liquid glass will rapidly destroy the material strength and crystal structure of the alloy wire 12. The alloy wire 12 undergoes irreversible "melting" under the design threshold. The impedance of its electrical circuit changes from a stable low-resistance state to an infinite open circuit state. The control system continuously applies low-voltage detection signals to each independent circuit. When the alloy wire 12 melts, the electrical circuit at that specific grid coordinate is instantly cut off, and the feedback signal undergoes a step jump. This binary (0 / 1) hard-wired logic change from "conduction" to "discontinuation" is captured by the control system as the highest priority hardware interrupt signal, thereby directly anchoring the exact physical arrival point of the erosion interface in the three-dimensional space model. Traditional industrial electric melting furnaces often use pre-embedded thermocouples to monitor temperature gradients and indirectly estimate the amount of erosion in the furnace wall. However, the heat conduction inside the refractory material has a significant hysteresis effect and is easily affected by power fluctuations within the furnace, leading to the failure of the calculation model. This solution abandons the fuzzy temperature gradient derivation and directly uses the "sacrificial physical damage" of the material as the final judgment criterion. This mechanism only exists in physical on / off states, eliminating the signal lag caused by thermal inertia. It avoids the possibility of false alarms from both mechanical and physical underlying principles, giving the system positioning reliability. If conventional industrial sensors or base metals (such as copper, iron, nickel, etc.) are used as the detection medium, they will immediately cause a violent coloring reaction or catalytic stone formation after melting and mixing into the glass melt, resulting in the scrapping of the entire furnace of expensive medical glass. The platinum-rhodium alloy used in this solution is an extremely stable precious metal material. Even if trace elements dissolve into the glass melt after performing the sacrificial detection function, it will not produce colored heavy metal spots in the 5.0 neutral borosilicate glass, nor will it damage its chemical stability.

[0043] Example 4 like Figure 5 and Figure 6 As shown, based on Example 1, the present invention provides a technical solution: preferably, the base material of the mounting ring 11 is the same as the refractory material of the inner wall of the furnace body 1. When the mounting ring 11 faces the thermodynamic erosion and chemical erosion of the high-temperature glass melt, its own physical erosion rate is synchronized with the erosion rate of the surrounding furnace body 1 pool wall, so as to ensure that the erosion boundary characterized by the melting of the alloy wire 12 has equivalence.

[0044] In this embodiment, the furnace body 1, which is in contact with the molten glass, typically uses high-purity fused zirconia alumina (AZS) and other advanced refractory materials. This solution mandates that the substrate of the mounting ring 11 be manufactured using the same material formula and sintering process as the substrate of the substrate. This consistency constraint ensures that the mounting ring 11 is absolutely identical to the surrounding original substrate in terms of key thermodynamic indicators such as bulk density, apparent porosity, high-temperature compressive strength, and resistance to molten glass erosion. In the actual fluid dynamic environment of the electric furnace, the mounting ring 11 and the surrounding substrate are subjected to the convective scouring and strong alkaline chemical erosion of the molten glass at temperatures above 1600°C. Due to the identical substrate material, the "physical retreat rate (thinning rate)" of the mounting ring 11 facing the molten glass is forced to synchronize with the thinning rate of the surrounding substrate. Therefore, when the surface of the mounting ring 11 is eroded and peeled off, causing the alloy wire 12 at a specific depth inside to be exposed and melted, the spatial depth where the alloy wire 12 is located is geometrically and physically equivalent to the actual depth of the surrounding substrate being eroded. If the material of mounting ring 11 has a higher hardness or corrosion resistance than the surrounding pool wall, over time, mounting ring 11 will form a "protrusion" on the pool wall, thereby changing the local hydrodynamic boundary, causing eddy currents in the molten glass (exacerbating surrounding erosion) and resulting in a severe lag in the open circuit signal of alloy wire 12. Conversely, if the material is inferior to the surrounding pool wall, it will form a "pit," causing premature false alarms. This solution, through a "material homogeneity" design, eliminates the measurement reference drift caused by material differences, ensuring that the detection interface always maintains a smooth conformal streamline surface with the real pool wall, avoiding disordered disturbances in local thermal convection. In industrial control systems, the accuracy of any top-level algorithm depends on the authenticity of the underlying sensor data. This structure not only "places" the sensor into the furnace wall but also allows the sensor to "grow" in the furnace wall. This physicochemical synchronous yielding mechanism ensures the authenticity of the control system when reverse mapping the three-dimensional morphology of the pool wall, thus providing a solid data foundation for the subsequent execution of the "global thermal field reconstruction command."

[0045] like Figure 5 and Figure 6 As shown, preferably, the spray axis of the nozzle 15 is inclined at an upward angle of 30°. The bottom wall of the inner cavity of the mounting base 13 is constructed with an inclined fluid guiding surface 16. The fluid guiding surface 16 is configured to collect and drain the cooling medium and condensate after phase change heat transfer in a directional manner to prevent water accumulation inside the mounting base 13. The top of the mounting base 13 is hinged with an openable cover plate 17. When the cover plate 17 is closed, it together with the mounting base 13 and the outer wall of the furnace body 1 to form a relatively sealed targeted cooling chamber.

[0046] In this embodiment, the most severely corroded area inside the pharmaceutical glass electric melting furnace is located at the "three-phase interface" (i.e., the liquid level line) where the liquid glass, furnace atmosphere, and refractory material meet. Since the mounting base 13 is fixed to the outer wall of the furnace body 1, the spray axis of the nozzle 15 is rigidly constrained to an upward angle of 30°. When the high-pressure cooling medium (micro-mist) is sprayed out, its two-phase jet field overcomes gravity and sprays upward in a parabolic trajectory. The core impact area of ​​the jet is projected and covers the outer wall area of ​​the furnace body 1 directly corresponding to the three-phase interface, directly penetrating the thermal boundary layer there. When the system performs cooling intervention, the cover plate 17 hinged to the top of the mounting base 13 is in a closed and locked state. 17. The shell of the mounting base 13 and the outer wall of the furnace body 1 are physically combined to form a miniature "targeted cooling chamber". This chamber forcibly constrains the flow field of the micro-mist sprayed by the nozzle 15, so that it can only have high-intensity convective heat transfer and boiling heat exchange with the hot furnace wall in this limited three-dimensional space. After the sprayed micro-mist takes away the heat of the furnace wall and undergoes a vaporization phase change, some of the incompletely vaporized droplets and the water droplets that condense when they cool will drip down along the outer wall of the furnace body 1 or the inner wall of the cover plate 17 under the action of gravity. The fluid guiding surface 16 uses the preset slope difference to physically guide these low enthalpy waste liquids, quickly collect them to the drain port and discharge them to the outside of the mounting base 13. If an open spray system is used, the cooling mist can easily diffuse randomly into the workshop environment, leading not only to low heat exchange efficiency but also to unnecessary cooling of other healthy areas of the furnace body 1 due to the escaped cold airflow (causing a large-area cold end effect). This solution uses a chamber constructed by the cover plate 17 to lock the latent heat of phase change of the cooling medium in the local hot spot area where corrosion occurs, achieving absolute thermal isolation in space. This results in an order-of-magnitude leap in the cooling efficiency ratio (COP). In industrial cooling systems, if the coolant accumulates in a local structure for a long time, it will not only cause severe corrosion of the metal structural components, but the accumulated water will also cause uncontrollable local supercooling due to continuous adhesion to the cold surface of the furnace wall, thereby inducing destructive thermal stress cracking inside the refractory material. The one-way drainage mechanism of the fluid guiding surface 16 ensures that the targeted cooling chamber always maintains a state of "rapid gas-liquid replacement and no liquid accumulation", achieving dual protection in terms of mechanical life and thermodynamic safety.

[0047] The present invention has been described in detail above. However, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, any modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. An electric melting furnace for manufacturing pharmaceutical glass, comprising a furnace body (1), a control system disposed on the furnace body (1), and a multi-zone power adjustment module electrically connected to the control system; characterized in that, It also includes: a top cover (2), which is rotatably connected to the top of the furnace body (1) and is used to form a closed melting chamber together with the furnace body (1); Electrode protection mechanism (3), several of the electrode protection mechanisms (3) are fixedly installed in a ring at equal intervals at the bottom end of the furnace body (1), and one end of the electrode protection mechanism (3) extends into the interior of the furnace body (1) for electrically heating the material in the melting chamber. The electrode protection mechanism (3) has an independent medium cooling channel. The erosion protection mechanism (4) is fixedly installed at the top of the furnace body (1) and is set in relation to the liquid level in the melting chamber. It is used to monitor the erosion status of the furnace wall structure at the liquid level. The erosion protection mechanism (4) is pre-embedded with a three-dimensional conductive wire matrix and has a regional targeted cooling channel. The control system is equipped with a solid-state boundary cooperative protection unit, which is configured to perform the following steps: Obtain the electrode working electrical parameter signal fed back in real time by the electrode protection mechanism (3), and the pool wall circuit break signal output by the three-dimensional conductive wire matrix in the erosion protection mechanism (4); Based on the electrode working electrical parameter signal and the pool wall open circuit signal, the regional melting efficiency index, which characterizes the heat absorption and convection state of the glass melt in each region of the furnace, is calculated in real time, and the boundary erosion risk value, which characterizes the erosion depth of the electrode neck and the degree of spalling of the refractory material of the pool wall, is calculated simultaneously. A preset global evaluation model is invoked, which includes a positive weight term for the regional melting efficiency index and a negative penalty term for the boundary erosion risk value. When the boundary erosion risk value or the regional melting efficiency index deviates from the preset safety and process threshold, a global thermal field reconstruction instruction is generated based on the global evaluation model. The global thermal field reconstruction command drives the corresponding electrode protection mechanism (3) and the erosion protection mechanism (4) to adjust the flow rate of the cooling medium inside them, so as to cut off the erosion path through physical freezing of the interface, thereby inhibiting the precipitation of heavy metals and refractory material impurities and contamination of the medical glass melt; at the same time, the multi-zone power adjustment module is synchronously driven to dynamically adjust the input power of the electrode protection mechanism (3) in each zone and perform iterative optimization. Under the constraint of prioritizing the reduction of the boundary erosion risk value penalty term, the stable temperature field required for glass homogenization and bubble removal is maintained by actively transferring the heat field load of the entire furnace, thereby maximizing the sum of the weighted terms of the regional melting efficiency index of the entire furnace.

2. The electric melting furnace for manufacturing pharmaceutical glass according to claim 1, characterized in that: The regional melting efficiency index includes at least the actual input electrical power of the electrode protection mechanism (3) in each region; the boundary erosion risk value includes at least the electrode end erosion depth calculated from the electrode working electrical parameter signal and the pool wall spalling depth calculated from the three-dimensional conductive wire matrix open circuit signal. The construction logic of the global evaluation model is as follows: set a comprehensive threshold for safety and process; When the erosion depth at the electrode tip and the spalling depth of the pool wall are both less than the comprehensive safety and process threshold, the penalty weight of the boundary erosion risk value approaches zero. The global thermal field reconstruction command aims to maximize the sum of melting efficiency indicators of the entire furnace area and drives each electrode protection mechanism (3) to operate close to the maximum value within its rated safe power range in order to maintain efficient glass melt melting and homogenization. When the erosion depth at any electrode tip or the spalling depth of the pool wall exceeds the comprehensive safety and process threshold, the penalty weight of the boundary erosion risk value increases rapidly and non-linearly, and the global thermal field reconstruction command is forced to prioritize curbing the erosion rate and preventing impurity precipitation. The control system forcibly drives the electrode protection mechanism (3) or the erosion protection mechanism (4) corresponding to the damaged coordinate to increase the flow rate of the cooling medium in order to implement local phase change freezing at the interface; at the same time, it actively reduces the input power of the electrode protection mechanism (3) in the damaged area and transfers the heat load to the other electrode protection mechanisms (3) in a safe state, so as to ensure the processing uniformity of the pharmaceutical glass melt while compensating for the lack of local thermal field, until the increase in the erosion depth of the electrode end and the peeling depth of the pool wall returns to the comprehensive safety and process threshold range.

3. The electric melting furnace for manufacturing pharmaceutical glass according to claim 2, characterized in that: The electrode protection mechanism (3) includes an installation sleeve (5) fixedly installed at equal intervals at the bottom of the furnace body (1). An inner cylinder (6) is coaxially fixed inside the installation sleeve (5). An electrode body (7) is inserted through the inner cylinder (6). The heating end of the electrode body (7) extends into the melting chamber to perform Joule heating on the material. The wiring end of the electrode body (7) extends to the outside of the furnace body (1) and is electrically connected to the multi-zone power adjustment module. The inner cylinder (6) has a spiral hole (8) extending in a spiral shape inside. Two connecting pipes (10) are symmetrically connected at one end of the inner cylinder (6) located on the outer wall of the furnace body (1). The two connecting pipes (10) are respectively connected to the medium inlet end and the medium outlet end of the spiral hole (8) to form an independent medium cooling channel and be controlled by the global thermal field reconstruction command.

4. The electric melting furnace for manufacturing pharmaceutical glass according to claim 3, characterized in that: The inner wall of the inner cylinder (6) is provided with a plurality of permeation holes (9) equidistantly spaced around its central axis, and the inlet end of each permeation hole (9) is connected to the interior of the spiral hole (8). The outlet end of the permeation hole (9) is configured to direct the cooling medium flowing in the spiral hole (8) and spray it to the assembly gap between the inner cylinder (6) and the electrode body (7), so that the high-temperature glass liquid that leaks outward along the assembly gap will undergo phase change and condense when it comes into contact with the cooling medium, thereby constructing a solid glass sealing barrier in situ within the assembly gap.

5. The electric melting furnace for manufacturing pharmaceutical glass according to claim 4, characterized in that: The corrosion protection mechanism (4) includes a mounting ring (11) conformally embedded in the liquid level area of ​​the inner wall of the furnace body (1). The interior of the mounting ring (11) is pre-embedded with a number of alloy wires (12) in a spatial grid array to form the three-dimensional conductive wire matrix. Each alloy wire (12) is electrically connected to the control system through an independent circuit. The furnace body (1) is fixed with a number of mounting seats (13) in a ring array on the cold side of the outer wall corresponding to the mounting ring (11). The interior of the mounting seat (13) is fixedly provided with a conduit (14) for conveying cooling medium. A number of nozzles (15) are equidistantly arranged on the conduit (14) facing the outer wall of the furnace body (1). The conduit (14) is connected to each nozzle (15) and together they form the area targeted cooling channel.

6. The electric melting furnace for manufacturing pharmaceutical glass according to claim 5, characterized in that: The alloy wire (12) is made of high-temperature resistant platinum-rhodium alloy. When it comes into direct contact with the high-temperature glass melt along with the refractory material of the surrounding pool wall being eroded and peeled off, it undergoes irreversible melting to accurately characterize the pool wall erosion boundary at the melting point and trigger the pool wall open circuit signal.

7. The electric melting furnace for manufacturing pharmaceutical glass according to claim 6, characterized in that: The base material of the mounting ring (11) is the same as the refractory material of the inner wall of the furnace body (1). When the mounting ring (11) faces the thermodynamic erosion and chemical erosion of the high temperature glass melt, its own physical erosion rate is synchronized with the erosion rate of the surrounding furnace body (1) pool wall, so as to ensure that the erosion boundary characterized by the melting of the alloy wire (12) is equivalent.

8. The electric melting furnace for manufacturing pharmaceutical glass according to claim 7, characterized in that: The spray axis of the nozzle (15) is inclined at a 30° angle upward. The bottom wall of the inner cavity of the mounting base (13) is constructed with an inclined fluid guiding surface (16). The fluid guiding surface (16) is configured to collect and drain the cooling medium and condensate after phase change heat transfer in a directional manner to prevent water accumulation inside the mounting base (13). The top of the mounting base (13) is hinged with an openable cover plate (17). When the cover plate (17) is closed, it together with the outer wall of the mounting base (13) and the furnace body (1) to form a relatively sealed targeted cooling chamber.