Microcrystalline glass and its preparation method, electronic equipment

By introducing high-modulus and high-bond-energy atoms such as silicon, aluminum, and yttrium, as well as magnesium spinel crystals into glass-ceramics, and combining them with a chemical strengthening layer, the problem of lateral crack propagation in glass-ceramics when exposed to sharp objects or friction has been solved. This has resulted in improved hardness and scratch resistance, extending the service life of electronic devices.

CN123105995APending Publication Date: 2026-11-17HONOR DEVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510639892.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing microcrystalline glass is prone to cracking and lateral expansion when exposed to sharp objects or friction, resulting in increased scratch width and affecting the aesthetics and lifespan of cover plates and electronic devices.

Method used

Microcrystalline glass, which contains glass phases of silicon, aluminum, yttrium and magnesium spinel or zinc magnesium spinel crystals, enhances the resistance to lateral crack propagation by increasing modulus and bond energy density, and improves impact resistance by using a chemical strengthening layer.

Benefits of technology

It significantly improves the hardness and scratch resistance of microcrystalline glass, extending the service life of covers and electronic devices, while maintaining transparency and optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105995A_ABST
    Figure CN123105995A_ABST
Patent Text Reader

Abstract

This application provides a microcrystalline glass, its preparation method, and an electronic device, relating to the field of electronic device technology. The microcrystalline glass comprises a matrix microcrystalline glass, which includes a main crystalline phase and a glassy phase. The glassy phase coats the main crystalline phase. The main crystalline phase includes magnesium spinel crystals or zinc-magnesium spinel crystals. The glassy phase includes at least silicon atoms, aluminum atoms, and yttrium atoms, and has a three-dimensional random network structure. Therefore, the microcrystalline glass exhibits high strength and hardness, and demonstrates excellent resistance to lateral crack propagation in the face of sharp objects or friction / puncture scenarios, resulting in shallow cracks and good scratch resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electronic devices, and more particularly to a microcrystalline glass, a method for preparing the same, and electronic devices. Background Technology

[0002] Due to its transparency and high-temperature resistance, glass has been widely researched and applied in daily life, such as in protective devices. However, glass also has some shortcomings, such as poor scratch resistance and susceptibility to scratches or damage, which limits its application in some fields.

[0003] With the widespread use of electronic devices, the requirements for glass materials are becoming increasingly stringent. For example, the vast majority of screen protectors used in current mobile phones (e.g., as cover plates) are made of glass. Currently, the ordinary glass used in cover plates is mainly a lithium aluminum silicon system based on silicon dioxide. This ordinary glass has characteristics such as low hardness and fragility, making it prone to scratches or damage when exposed to sharp objects or friction.

[0004] Therefore, glass-ceramics have been increasingly researched and applied in the field of electronic devices. Currently, the glass-ceramics commonly used in cover plates are mainly silicate systems based on lithium disilicate crystals. Although this type of glass-ceramic offers a significant improvement in hardness, the low modulus and low bond energy of lithium disilicate crystals make it prone to lateral crack propagation when exposed to scratches and punctures. This increases the width of the scratches and affects the aesthetics and lifespan of the cover plate and electronic devices. Summary of the Invention

[0005] This application provides a microcrystalline glass, its preparation method, and its application. The microcrystalline glass has high strength and hardness, and has a good ability to resist the lateral propagation of cracks when facing sharp objects or friction and puncture scenarios, and keeps the cracks very shallow, thereby having good scratch resistance and improving the aesthetics and lifespan of cover plates and electronic devices.

[0006] To achieve the above objectives, this application adopts the following technical solution:

[0007] In a first aspect, a microcrystalline glass is provided, comprising: a matrix microcrystalline glass, the matrix microcrystalline glass comprising a main crystalline phase and a glass phase, the glass phase coating the main crystalline phase, the main crystalline phase comprising magnesium spinel crystals or zinc magnesium spinel crystals, the glass phase comprising at least silicon atoms, aluminum atoms and yttrium atoms, and the glass phase having a three-dimensional random network structure.

[0008] This application provides a microcrystalline glass. By containing atoms such as silicon, aluminum, and yttrium in the glass phase, the modulus and bond energy volume density of the matrix microcrystalline glass are improved, thereby significantly enhancing the intrinsic strength and hardness of the microcrystalline glass. At the same time, the microcrystalline glass has magnesium spinel crystals or zinc magnesium spinel crystals with higher elastic modulus and hardness as the main crystal phase. While ensuring transparency, it also improves the ability to resist the lateral propagation of cracks when facing sharp objects or friction puncture scenarios. In this way, when an external force first hits the glass phase of the microcrystalline glass and causes a crack, and the crack then propagates inward and contacts the internal spinel crystal, the microcrystalline glass can absorb the crack propagation according to its own crystal vibration, making the crack very shallow and not easily seen by the naked eye.

[0009] In one possible implementation of the first aspect, the microcrystalline glass comprises, by weight percentage, the following components: a silica-containing glass component, 40 wt%-50 wt%; an alumina-containing glass component, greater than or equal to 25 wt%; a spinel component, 1 wt%-12 wt%; a self-nucleating agent, 1 wt%-8 wt%; and a yttrium-containing modifier, greater than 0 wt% and less than or equal to 8 wt%.

[0010] In this implementation, on the one hand, by including atoms such as silicon, aluminum, and yttrium in the glass phase, the density and chemical bond energy of the three-dimensional random network structure of the matrix glass-ceramic are increased from the glass bulk composition, thereby improving the modulus and bond energy volume density of the matrix glass-ceramic, and thus significantly improving the intrinsic strength and hardness of the glass-ceramic. On the other hand, the matrix glass-ceramic has magnesium spinel crystals or zinc magnesium spinel crystals with higher elastic modulus and hardness as the main crystal phase, which not only ensures optical performance, but also improves the ability to resist the lateral propagation of cracks when facing sharp objects or friction puncture scenarios.

[0011] In one possible implementation of the first aspect, the microcrystalline glass comprises, by weight percentage, the following components: a silica-containing glass component, 40 wt%-50 wt%; an alumina-containing glass component, greater than or equal to 25 wt%; a spinel component, 1 wt%-12 wt%; a self-nucleating agent, 1 wt%-8 wt%; a yttrium-containing modifier, greater than 0 wt% and less than or equal to 8 wt%; and a flux, 1 wt%-5 wt%.

[0012] In this implementation, the flux can lower the melting point of the raw materials during the preparation of the matrix microcrystalline glass, so that the melting temperature is not too high and a good melting effect can be achieved. This is beneficial for industrial production and also saves energy and costs.

[0013] In one possible implementation of the first aspect, the microcrystalline glass comprises, by weight percentage, the following components: a silica-containing glass component, 40 wt%-50 wt%; an alumina-containing glass component, greater than or equal to 25 wt%; a spinel component, 1 wt%-12 wt%; a self-nucleating agent, 1 wt%-8 wt%; a yttrium-containing modifier, greater than 0 wt% and less than or equal to 8 wt%; and a clarifying agent, 0.05 wt%-0.7 wt%.

[0014] In this implementation, the clarifying agent can be used during the formation of the matrix glass, specifically to expel a large amount of gas generated during the melting process, thereby making the microcrystalline glass more uniform and clearer, thus meeting its requirements as a cover plate.

[0015] In one possible implementation of the first aspect, the silicon-containing glass component comprises silicon dioxide; the aluminum-containing glass component comprises aluminum oxide; the spinel component comprises TO, wherein T comprises any one of magnesium, magnesium and zinc; the self-nucleating agent comprises XO2, wherein X comprises at least one of titanium and zirconium; the yttrium-containing modifier comprises yttrium oxide; the flux comprises at least one of boron trioxide and phosphorus pentoxide; and the clarifying agent comprises antimony trioxide.

[0016] In this implementation method, the components are simple and easy to obtain, which is conducive to industrial production and application.

[0017] In one possible implementation of the first aspect, the glass-ceramic further includes a first chemical strengthening layer, which comprises a Na / Li exchange layer that coats the matrix glass-ceramic.

[0018] In this implementation, the first chemical strengthening layer can improve the impact resistance of the glass-ceramic, as well as its resistance to punctures from rough surfaces, and it also has high optical properties such as light transmittance.

[0019] In one possible implementation of the first aspect, the matrix microcrystalline glass comprises, by weight percentage, the following components: a silicon-containing glass component, 40 wt%-50 wt%; an aluminum-containing glass component, greater than or equal to 25 wt%; a spinel component, 1 wt%-12 wt%; a self-nucleating agent, 1 wt%-8 wt%; a yttrium-containing modifier, greater than 0 wt% and less than or equal to 8 wt%; and a first chemical strengthening component, 1 wt%-8 wt%; wherein the first chemical strengthening component comprises R₂O, wherein R comprises at least one of lithium and sodium.

[0020] In this implementation method, the components are simple and easy to obtain, which is conducive to industrial production and application.

[0021] In one possible implementation of the first aspect, the glass-ceramic further includes a second chemically strengthened layer, which comprises a K / Na exchange layer and covers a Na / Li exchange layer.

[0022] In this implementation, the second chemical strengthening layer not only further optimizes and improves the high impact resistance of the glass-ceramic, but also further improves its resistance to drops from rough surfaces.

[0023] In one possible implementation of the first aspect, the matrix glass-ceramic comprises, by weight percentage, the following components: a silicon-containing glass component, 40 wt%-50 wt%; an aluminum-containing glass component, greater than or equal to 25 wt%; a spinel component, 1 wt%-12 wt%; a self-nucleating agent, 1 wt%-8 wt%; a yttrium-containing modifier, greater than 0 wt% and less than or equal to 8 wt%; a first chemical strengthening component, 1 wt%-8 wt%; and a second chemical strengthening component, 1 wt%-8 wt%. The second chemical strengthening component includes E₂O, wherein E includes at least one of sodium and potassium.

[0024] In this implementation method, the components are simple and easy to obtain, which is conducive to industrial production and application.

[0025] In one possible implementation of the first aspect, the microcrystalline glass comprises, by mass percentage, the following components: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or (Mg,Zn)Al2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3 and / or P2O5, 1wt%-5wt%; and Sb2O3, 0.05wt%-0.7wt%.

[0026] In this implementation, on the one hand, the high silicon and aluminum content, along with the presence of yttrium in the glass phase, can improve the density and chemical bond energy of the three-dimensional random network structure of the glass phase. This means introducing more network-forming bodies and high-bond-energy components into the matrix glass-ceramic, thereby achieving high-modulus, high-density, and high-hardness glass-ceramics. On the other hand, the nucleating agent becomes the lowest energy point in the glass phase. Driven by the thermal force of the internal thermal field of the matrix glass-ceramic, other ions and / or atoms migrate and aggregate near the nucleating agent. Further temperature increases result in highly crystalline, small-sized spinel crystals, which are encapsulated by the glass phase. Thus, when a crack propagates and encounters a spinel crystal, the spinel crystal's intrinsic strength counteracts the crack propagation energy, making further propagation difficult. Furthermore, if the crack propagation potential exceeds the intrinsic strength of the spinel crystal, the crack will propagate along the low-bond-energy positions of the crystal lattice points rather than laterally, significantly enhancing the scratch resistance of the glass-ceramic.

[0027] In one possible implementation of the first aspect, the crystallinity of the main crystalline phase is greater than or equal to 45%.

[0028] In this implementation, the main crystalline phase forms a more complete and regular crystal structure, making the atomic arrangement inside the glass-ceramic more compact and orderly, thus increasing the hardness of the glass-ceramic and effectively resisting scratches and friction, reducing scratches or damage. At the same time, the main crystalline phase grows uniformly during the crystallization process, reducing defects and weak areas inside the glass-ceramic. This allows it to withstand external forces more evenly and is less prone to stress concentration in local areas, which can lead to scratches or damage. In addition, high crystallinity means that more atoms are in a stable chemical bond state. Therefore, when subjected to scratches and friction, more energy is required to break these chemical bonds, thus making the glass-ceramic exhibit better scratch resistance.

[0029] In one possible implementation of the first aspect, the shape of the main crystalline phase includes a spherical shape with a diameter of 10 nm to 20 nm.

[0030] In this implementation, the grain size of the microcrystalline glass is smaller, and the internal structure of the microcrystalline glass is more uniform and ordered, which can enhance the hardness of magnesium aluminum silicon spinel. At the same time, the small-particle-size main crystalline phase can make the internal stress distribution of the microcrystalline glass more uniform. This improves the ability of the microcrystalline glass to resist the lateral propagation of cracks when facing sharp objects or friction and puncture scenarios, so that the cracks are very shallow and difficult to propagate laterally. In addition, they are not easily seen by the naked eye, resulting in better performance of the microcrystalline glass.

[0031] In one possible implementation of the first aspect, the density of the glass-ceramic is greater than or equal to 2.8 g / cm³. 3 .

[0032] In this implementation, the high density of the microcrystalline glass increases its hardness and enhances its scratch resistance. At the same time, the dense structure has a stronger ability to absorb impact energy, which can reduce the risk of breakage when dropped. In addition, the dense structure can also reduce the penetration of corrosive substances and improve acid and alkali resistance.

[0033] In one possible implementation of the first aspect, the grayscale value of the microcrystalline glass under rubbing with 1500gf garnet sandpaper is less than or equal to 1.5.

[0034] In this implementation, under the same friction conditions, the color change of the microcrystalline glass surface is not obvious, its surface remains relatively intact, and there are no large number of scratches or damages caused by friction. In addition, the surface hardness of the microcrystalline glass is high, and the internal structure of the microcrystalline glass remains relatively stable and has good wear resistance. Thus, the microcrystalline glass has good scratch resistance.

[0035] In one possible implementation of the first aspect, the microcrystalline glass has a transmittance of greater than or equal to 88% at a wavelength of 550 nm when the thickness is 0.5 mm to 0.65 mm.

[0036] In this implementation, microcrystalline glass absorbs and scatters less light at a wavelength of 550nm, maintaining the intensity and direction of light propagation, thus providing a clear and transparent visual effect. Furthermore, after the microcrystalline glass is made into a cover plate, it can be directly placed on the display screen without affecting its normal display.

[0037] In one possible implementation of the first aspect, the microcrystalline glass, with a thickness of 0.5 mm to 0.65 mm, has a reflectivity of less than or equal to 10% at a wavelength of 550 nm.

[0038] In this implementation, the microcrystalline glass allows more light to pass through at a wavelength of 550nm, resulting in excellent optical performance. When this microcrystalline glass is applied to the cover glass, the display can be clearer and the colors more realistic. Simultaneously, in strong light environments, it can reduce ambient light interference and improve visual comfort.

[0039] In one possible implementation of the first aspect, the haze of the microcrystalline glass is less than or equal to 2.0% when the thickness is 0.5 mm to 0.65 mm.

[0040] In this implementation, the microcrystalline glass has a uniform internal crystal structure with few defects, and the light passing through it mainly travels in straight lines with minimal scattering. Therefore, when this microcrystalline glass is applied to a cover plate, it can make the edges of the displayed image sharp and the details clear. It can also improve the contrast of the display, reduce color distortion, decrease fingerprints and oil stains, and maintain long-term light transmittance.

[0041] In one possible implementation of the first aspect, the Young's modulus of the glass-ceramic is greater than or equal to 98 GPa.

[0042] In this implementation, the microcrystalline glass has high stiffness and resistance to deformation, enabling its surface to withstand greater external forces without easily undergoing plastic deformation. This increases surface hardness and makes it less susceptible to scratches or damage from sharp objects. Furthermore, when an object attempts to scratch the microcrystalline glass, its higher Young's modulus allows it to effectively distribute the external force over a larger area, preventing the force from concentrating at a localized point and causing scratches. Additionally, the higher Young's modulus allows the microcrystalline glass to resist wear caused by friction, reducing the likelihood of surface scratches and thus maintaining surface smoothness and integrity.

[0043] In one possible implementation of the first aspect, the Vickers hardness of the glass-ceramic is greater than or equal to 930 HV.

[0044] In this implementation, the surface of the microcrystalline glass can withstand greater pressure without producing obvious indentations or scratches. Thus, when a sharp object comes into contact with the surface of the microcrystalline glass, the high Vickers hardness enables the microcrystalline glass to effectively resist the object's penetration, thereby reducing the occurrence of scratches or damage. At the same time, the atoms on the surface of the microcrystalline glass are tightly bonded and have a stable structure. This tight structure gives it high surface strength, enabling it to withstand friction and collisions from external objects without easily being damaged. In addition, it can better maintain a smooth surface, reduce the degree of scratches caused by wear, extend its service life, and maintain good appearance and performance.

[0045] In a second aspect, an electronic device is provided, the electronic device including a glass component, such as the microcrystalline glass in the first aspect or any possible implementation of the first aspect.

[0046] This application provides an electronic device in which the aesthetics of the glass components are improved and the lifespan of the electronic device is also extended.

[0047] Thirdly, a method for preparing a microcrystalline glass is provided, the method comprising:

[0048] The silicon-containing glass component, aluminum-containing glass component, spinel component, self-nucleating agent and yttrium-containing regulator are mixed as raw materials. After the raw materials are melted at a certain temperature and held for a period of time, they are then subjected to cooling treatment and annealing treatment in sequence to obtain matrix glass bricks.

[0049] The matrix glass bricks are subjected to nucleation and crystallization treatments in sequence to obtain matrix microcrystalline glass. The matrix microcrystalline glass includes a main crystalline phase and a glass phase. The glass phase coats the main crystalline phase. The main crystalline phase includes magnesium spinel crystals or zinc magnesium spinel crystals. The glass phase includes at least silicon atoms, aluminum atoms and yttrium atoms. The glass phase has a three-dimensional random network structure.

[0050] This application provides a method for preparing glass-ceramics, which yields a glass phase with high silicon and aluminum content and containing yttrium. By introducing more network forgings and high bond energy components into the matrix glass-ceramic, a high-modulus, high-density, and high-hardness glass-ceramic is obtained. Furthermore, through nucleation and crystallization treatments, highly crystalline, small-sized spinel crystals are precipitated, with the spinel crystals encapsulated within the glass phase. Thus, when a crack propagates and encounters a spinel crystal, the spinel crystal's intrinsic strength counteracts the crack propagation energy, making further propagation difficult. Moreover, if the crack propagation potential exceeds the intrinsic strength of the spinel crystal, the crack will propagate along the low bond energy positions of the crystal lattice points rather than laterally, significantly enhancing the scratch resistance of the glass-ceramic. In addition, the nucleation and crystallization temperatures in this preparation method are not high, resulting in low energy consumption and low cost, which is beneficial for industrial production and application.

[0051] In one possible implementation of the third aspect, a silica-containing glass component, an aluminum-containing glass component, a spinel component, a self-nucleating agent, and a yttrium-containing modifier are mixed as raw materials. The raw materials are melted at a certain temperature and held for a period of time, followed by sequential cooling and annealing treatments to obtain a matrix glass brick comprising:

[0052] Based on mass percentage, 40wt%-50wt% of SiO2, ≥25wt% of Al2O3, 1wt%-12wt% of MgO or MgO and ZnO, 1wt%-8wt% of TiO2 and / or ZrO2, 1wt%-8wt% of Y2O3, 1wt%-5wt% of B2O3 and / or P2O5, and 0.05wt%-0.7wt% of Sb2O3 are selected as raw materials and mixed for a period of time. The raw materials are then melted at 1600℃-1700℃ for a period of time and then poured into a cooled mold to obtain matrix glass bricks.

[0053] The matrix glass bricks were subjected to nucleation and crystallization treatments in sequence to obtain matrix microcrystalline glass, including:

[0054] The matrix glass bricks are annealed at 500℃-600℃ for a period of time and then cooled to obtain matrix glass.

[0055] The matrix glass is nucleated at 600℃-690℃ for a period of time, and then crystallized at 700℃-850℃ for a period of time to obtain matrix microcrystalline glass.

[0056] In this implementation, on the one hand, from the perspective of preparing the glass phase, a glass phase with high silicon and aluminum content and containing yttrium is obtained, which can improve the density and chemical bond energy of the three-dimensional random network structure of the glass phase. That is, more network forgings and high bond energy components are introduced into the matrix glass-ceramic, thereby obtaining a glass-ceramic with high modulus, high density and high hardness. On the other hand, from the perspective of preparing the crystal, nucleation and crystallization treatments are performed sequentially. The nucleating agent becomes the lowest energy point in the glass phase. Driven by the thermal force energy of the internal thermal field of the matrix glass-ceramic, other ions and / or atoms migrate and gather near the nucleating agent. Further increasing the temperature can precipitate highly crystalline, small-sized spinel crystals, which are then encapsulated by the glass phase. When a crack propagates and encounters a spinel crystal, the spinel crystal's intrinsic strength counteracts the crack propagation energy, making further propagation difficult. Furthermore, if the crack propagation potential exceeds the intrinsic strength of the spinel crystal, the crack will propagate along the lower bond energy positions of the crystal lattice points rather than laterally, significantly enhancing the scratch resistance of the glass-ceramic. In addition, this preparation method uses relatively low nucleation and crystallization temperatures, resulting in low energy consumption and low cost, which is beneficial for industrial production and application.

[0057] In one possible implementation of the third aspect, by mass percentage, 40wt%-50wt% of SiO2, greater than or equal to 25wt% of Al2O3, 1wt%-12wt% of MgO or MgO and ZnO, 1wt%-8wt% of TiO2 and / or ZrO2, 1wt%-8wt% of Y2O3, 1wt%-5wt% of B2O3 and / or P2O5, and 0.05wt%-0.7wt% of Sb2O3 are selected as raw materials and mixed for a period of time. The raw materials are then melted at 1600℃-1700℃ for a period of time and then poured into a cooled mold to obtain a matrix glass brick comprising:

[0058] Based on mass percentage, 40wt%-50wt% of SiO2, greater than or equal to 25wt% of Al2O3, 1wt%-12wt% of MgO or MgO and ZnO, 1wt%-8wt% of TiO2 and / or ZrO2, 1wt%-8wt% of Y2O3, 1wt%-5wt% of B2O3 and / or P2O5, 0.05wt%-0.7wt% of Sb2O3, and 1wt%-8wt% of Li2O, Na2O and K2O are selected as raw materials and mixed for a period of time. The raw materials are then melted at 1600℃-1700℃ for a period of time and then poured into a cooled mold to obtain matrix glass bricks.

[0059] After nucleating the matrix glass at 600℃-690℃ for a period of time, and then crystallizing it at 700℃-850℃ for a period of time to obtain matrix microcrystalline glass, the preparation method also includes:

[0060] The matrix glass-ceramic is subjected to at least one surface treatment to obtain the initial glass-ceramic;

[0061] The initial glass-ceramic is subjected to at least one chemical strengthening treatment to obtain glass-ceramic.

[0062] In this implementation, atoms with larger atomic radii from the salt solution replace atoms with smaller atomic radii in the original glass-ceramic. For example, Na replaces Li, K replaces Li and / or Na. During this process, compressive stress adheres to the surface of the matrix glass-ceramic to form at least one compressive stress layer. The compressive stress layer can resist the impact force generated during impact, further improving the scratch resistance of the glass-ceramic.

[0063] This application provides a microcrystalline glass, its preparation method, and an electronic device. The microcrystalline glass incorporates atoms such as silicon, aluminum, and yttrium in its glass phase, increasing the modulus and bond energy volume density of the matrix microcrystalline glass, thereby significantly improving its intrinsic strength and hardness. Simultaneously, the microcrystalline glass uses magnesium spinel or zinc-magnesium spinel crystals, which have higher elastic modulus and hardness, as the main crystalline phase. This ensures transparency while also improving its resistance to lateral crack propagation when exposed to sharp objects or friction. When an external force first strikes the glass phase of the microcrystalline glass, causing a crack, and the crack then propagates inward to contact the internal spinel crystals, the microcrystalline glass can absorb the crack propagation through its own crystal vibrations, resulting in a shallow crack that is not easily visible to the naked eye. Therefore, applying microcrystalline glass to electronic devices improves the lifespan and other performance aspects of the devices, resulting in a better user experience. Attached Figure Description

[0064] Figure 1 This is a schematic diagram of the overall structure of an electronic device provided in an embodiment of this application;

[0065] Figure 2 for Figure 1 A schematic diagram of the disassembled structure of an electronic device;

[0066] Figure 3 A structural schematic diagram of a display screen and cover plate provided for related technologies;

[0067] Figure 4 A molecular dynamics simulation diagram illustrating crystal failure during crack propagation in a silicate microcrystalline glass primarily composed of lithium disilicate crystals, providing insights for related technologies.

[0068] Figure 5 This is a molecular dynamics simulation diagram of crystal failure during crack propagation in a microcrystalline glass provided in an embodiment of this application.

[0069] Figure 6 Stress-strain simulation curves of a pure magnesium spinel crystal and silicate microcrystalline glass mainly composed of lithium disilicate crystals provided in the embodiments of this application;

[0070] Figure 7 A process flow diagram for preparing a matrix microcrystalline glass provided in this application embodiment;

[0071] Figure 8 A process flow diagram for preparing another matrix microcrystalline glass provided in this application embodiment;

[0072] Figure 9 A process flow diagram for the preparation of a microcrystalline glass provided in this application embodiment;

[0073] Figure 10A flowchart illustrating the preparation process of another microcrystalline glass provided in this application embodiment;

[0074] Figure 11 A schematic diagram of grayscale value testing for a microcrystalline glass provided in an embodiment of this application;

[0075] Figure 12 A schematic diagram of the scratch microstructure of a microcrystalline glass provided in an embodiment of this application;

[0076] Figure 13 A schematic diagram of the scratch morphology of a common lithium aluminum silicon glass, mainly composed of silicon dioxide, is provided for related technologies.

[0077] Figure label:

[0078] 01-Mobile phone; 100-Display screen; 101-Mid-frame; 102-Back cover; 103-Circuit board assembly; 1031-Main circuit board; 1032-Electronic components; 104-Battery; 105-Cover plate; 02-Silica microcrystalline glass mainly composed of lithium disilicate crystals; 1-Microcrystalline glass; 11-Main crystalline phase; 12-Glassy phase; 21-Horizontal platform surface; 22-Garnet sandpaper; 23-Linear abrasion tester; 231-First rod of linear abrasion tester; 24-Weight load. Detailed Implementation

[0079] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0080] In the description of this application, it is important to understand that the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0081] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0082] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms "a" and "the" as used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0083] In the various embodiments of this application, the sequence number of each process does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0084] The weight of the relevant components mentioned in the embodiments of this application can refer not only to the specific content of each component, but also to the proportional relationship between the weights of each component. Therefore, as long as the content of the relevant components is scaled up or down proportionally according to the embodiments of this application, it is within the scope disclosed in the embodiments of this application.

[0085] The terms "first," "second," etc., are used for descriptive purposes only to distinguish objects, such as substances, from one another, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. For example, without departing from the scope of the embodiments of this application, "first XX" may also be referred to as "second XX," and similarly, "second XX" may also be referred to as "first XX." Thus, features defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature.

[0086] First, some terms used in the embodiments of this application will be explained to enable those skilled in the art to better understand them.

[0087] Chemically strengthened glass-ceramics: These are chemically tempered glass-ceramics that have undergone a high-temperature ion exchange process. In a high-temperature molten salt, large alkali metal ions replace small alkali metal ions in the glass, creating a volume difference in the exchanged ions. This generates compressive stress from high to low on the surface of the glass, hindering and delaying the propagation of microcracks, thereby improving the mechanical strength of the glass.

[0088] Sodium-lithium ion exchange: refers to the process in which sodium ions in a salt bath replace lithium ions in glass during chemical strengthening. Na / Li exchange layer: refers to a sodium-containing layer in chemically strengthened glass-ceramics where sodium ions partially replace lithium ions.

[0089] Potassium-sodium ion exchange: refers to the replacement of sodium ions in glass with potassium ions in a salt bath during chemical strengthening. K / Na exchange layer: refers to a potassium-containing layer in chemically strengthened glass-ceramics where potassium ions partially replace sodium ions.

[0090] Haze: A measure of the degree to which a material scatters light, defined as the percentage of scattered light flux transmitted through the material to the total transmitted light flux.

[0091] Mohs hardness: A standard for expressing the hardness of a material. It is determined by scratching the surface of the material with a pyramidal diamond needle using the scratch method, and measuring the depth of the scratch. The depth of the scratch is the Mohs hardness.

[0092] Vickers hardness: A standard for expressing the hardness of a material. It is determined by pressing a diamond pyramid indenter with an included angle of 136° between its opposite faces into the surface of the material under a specified load, holding it for a certain time, removing the load, measuring the diagonal length of the indentation, calculating the surface area of ​​the indentation, and finally determining the average pressure on the surface area of ​​the indentation as the Vickers hardness value of the material.

[0093] The above is a brief introduction to the terms used in the embodiments of this application, and will not be repeated below.

[0094] This application does not limit the specific type of electronic device. In some embodiments, the electronic device of this application may include mobile phones, wearable devices (e.g., smart bracelets, smartwatches, and headphones), tablets, laptops, handheld computers, notebooks, ultra-mobile personal computers (UMPCs), cellular phones, personal digital assistants (PDAs), augmented reality (AR) / virtual reality (VR) devices, and other Internet of Things (IoT) devices and in-vehicle electronic devices, as well as devices such as televisions, large screens, printers, and projectors.

[0095] This application does not limit the specific form of the electronic device. For ease of explanation, a mobile phone will be used as an example below.

[0096] Figure 1 This is a schematic diagram of the mobile phone 01 to which some embodiments of this application are applicable. Figure 2 for Figure 1 The diagram shows the disassembly of mobile phone 01. Among them, Figure 1 and Figure 2 The mobile phone 01 shown is an example of a phablet. In other embodiments, it can be other types of mobile phones, such as foldable phones.

[0097] exist Figure 1 and Figure 2 In the example, mobile phone 01 may include a display screen 100, a mid-frame 101, a back cover 102, a circuit board assembly 103, and a battery 104, etc. It is understood that... Figure 1 and Figure 2 The accompanying drawings below only schematically show some components of the mobile phone 01. The actual shape, size, position, and structure of these components are not subject to change. Figure 1 and Figure 2 And the limitations of the figures below.

[0098] like Figure 1 and Figure 2 As shown, the display screen 100 in mobile phone 01 is located on one side of the mid-frame 101. In applications, the display screen 100 can be used to display images and videos, etc. The display screen 100 can be any of the following: liquid crystal display (LCD), organic light emitting diode (OLED) display, mini light emitting diode (Mini LED) display, and micro light emitting diode (Micro LED) display.

[0099] In addition, the display screen 100 can be a foldable screen, depending on the actual application.

[0100] refer to Figure 2 As shown, the back cover 102 is located on the side of the mid-frame 101 away from the display screen 100, and the back cover 102 and the mid-frame 101 form an internal accommodating space for the mobile phone 01. This internal accommodating space is used to accommodate the circuit board assembly 103 and the battery 104, etc. The battery 104 is used to provide power to structures such as the display screen 100 and the circuit board assembly 103 inside the mobile phone 01.

[0101] like Figure 2 As shown, the circuit board assembly 103 includes a main circuit board 1031 and electronic components 1032, etc. The main circuit board 1031 is used to carry the electronic components 1032 and to complete signal interaction with the electronic components 1032. Figure 2The following explanation uses circuit board assembly 103, which includes two electronic components 1032, as an example. Of course, the number of electronic components 1032 is not limited to two; the specific number depends on the actual application. In applications, the main circuit board 1031 may include printed circuit boards (PCBs) and flexible printed circuit boards (FPCs). Electronic components 1032 may include, but are not limited to, chips, resistors, capacitors, inductors, potentiometers, electron tubes, heat sinks, electromechanical components, connectors, semiconductor discrete devices, sensors, power supplies, switches, micromotors, electronic transformers, relays, and subscriber identity modules (SIM cards).

[0102] Please refer to this again. Figure 2 The mobile phone 01 also includes a cover plate 105, which can be stacked with the display screen 100. Specifically, the cover plate 105 can be fixed to the frame of the mobile phone 01, mainly for protecting the display screen 100 and preventing dust.

[0103] Will Figure 2 The display screen 100 and the cover plate 105 are cut along F1F2 to obtain Figure 3 The cross-sectional view of the display screen 100 and the cover plate 105 shown.

[0104] In applications, the cover glass is typically made of glass, such as ordinary glass. Currently, the ordinary glass used in cover glass 105 is mainly a lithium aluminum silicon system material based on silicon dioxide. This is because the lithium aluminum silicon system material based on silicon dioxide has certain wear resistance, high transparency, and strong resistance to common chemicals. It also has a low coefficient of thermal expansion, resulting in minimal dimensional changes under different temperature environments. However, the lithium aluminum silicon system material based on silicon dioxide also has characteristics such as low hardness and brittleness, causing the cover glass 105 made from it to be prone to scratches or damage when exposed to sharp objects or friction. Moreover, as the phone 01 is used for a longer period of time, scratches or damage will increase, which will not only affect the appearance of the phone 01, but also disrupt the stress balance of the cover glass 105, leading to a decrease in the impact resistance of the cover glass 105, and thus affecting the performance of the phone 01.

[0105] Compared to traditional ordinary glass, microcrystalline glass, when made into cover glass 105, has the following advantages: First, it is less prone to cracking or breaking when subjected to external impact, effectively protecting the internal components of the phone 01 and reducing the risk of damage due to accidental drops or collisions; Second, it has high hardness and good wear resistance, resisting various scratches that may be encountered in daily use, making cover glass 105 less susceptible to scratches or damage, extending its lifespan, and maintaining the clarity and aesthetics of the display screen 100; Third, it has high transparency and low haze, providing excellent visual effects, making the display screen 100 clearer and more vibrant, with high color reproduction, and effectively reducing light reflection, allowing users to clearly see the display even in strong light environments. The content reduces eye fatigue; fourth, it has a low coefficient of thermal expansion, capable of withstanding large temperature changes without significant deformation or cracking. This means that even if some electronic components 1032 generate heat during prolonged use of the phone 01, the cover glass 105 can maintain stable performance, with minimal impact on the overall structure and performance of the phone 01 due to thermal expansion and contraction; fifth, it can be processed into thin sheets, enabling the phone 01 to be lightweight and thin while maintaining strength and performance, making it easy to carry and improving the user experience; sixth, it possesses good chemical stability and is not easily corroded by chemical substances, thus resisting corrosion from sweat and cosmetics during daily use, keeping the performance and appearance of the cover glass 105 as unaffected as possible. Therefore, microcrystalline glass, as the material for the cover glass 105, has received increasingly widespread research and application.

[0106] Currently, the most commonly used microcrystalline glass is a silicate system based on lithium disilicate crystals. Silicate microcrystalline glass based on lithium disilicate crystals has a significantly higher hardness than ordinary lithium aluminum silicon glass based on silicon dioxide. Figure 4 The diagram shows the crystal failure of silicate microcrystalline glass O2, which is mainly composed of lithium disilicate crystals, during crack propagation. Figure 4 As shown, due to the low modulus and low bond energy of lithium disilicate crystal-based silicate glass 02, the cover plate 105 made from it is prone to crack propagation along the crystal interface (lateral propagation) when subjected to scratches or punctures. This means that under the same scratch conditions, the scratches or damage caused by the lithium disilicate crystal-based silicate glass 02 appear wider macroscopically. Figure 4 The crack width w02 is larger and more obvious, affecting the aesthetics of the cover plate 105 and the lifespan of the mobile phone 01.

[0107] Therefore, how to minimize scratches or damage to microcrystalline glass and apply it to cover plates, thereby ensuring the aesthetic appearance and service life of the cover plates, is an urgent problem to be solved.

[0108] The above only introduces the content related to the inventive point. Other content can be obtained by referring to relevant technologies, and will not be explained in detail here.

[0109] This application provides a microcrystalline glass with high modulus and high hardness, which makes the cover plate 105 made of it less prone to lateral crack expansion when faced with scratches and punctures. The scratches are small and very faint to the naked eye, resulting in a longer service life for the cover plate 105. In addition, it also makes the mobile phone 01 more aesthetically pleasing and provides a better user experience.

[0110] Figure 5 A microcrystalline glass 1 according to an embodiment of this application is shown.

[0111] like Figure 5 As shown, the microcrystalline glass 1 provided in this application embodiment includes: a matrix microcrystalline glass, which includes a main crystalline phase 11 ( Figure 5 (Within the dashed line) and glass phase 12, which encapsulates the main crystalline phase 11. The main crystalline phase 11 includes magnesium spinel crystals or zinc magnesium spinel crystals, and the glass phase 12 includes at least silicon atoms, aluminum atoms and yttrium atoms. The glass phase 12 has a three-dimensional random network structure.

[0112] In applications, the main crystal phase 11 can be pure magnesium spinel crystal MgAl2O4, in which case the main crystal phase 11 contains magnesium (Mg), aluminum (Al), and oxygen (O); or, the main crystal phase 11 can be zinc magnesium spinel crystal (Mg,Zn)Al2O4, in which case the main crystal phase 11 contains Mg, Al, O, and zinc (Zn).

[0113] It should be noted that some impurity phases other than the main crystalline phase 11 are inevitably present in the matrix glass-ceramic, such as cordierite (Mg2Al4Si5O). 18 ), mullite (Al6Si2O) 13 One or more of the following, such as zirconium dioxide (ZrO2) and silicon dioxide (SiO2), are used. Since these crystals are impurity phases, their content should be as low as possible. The lower the content, the more and purer the main crystal phase 11.

[0114] It should be understood that glass phase 12 covering main crystalline phase 11 means that glass phase 12 covers the entire outer surface of main crystalline phase 11.

[0115] In applications, the matrix microcrystalline glass of this application embodiment may include the following components by weight percentage: silicon-containing glass component, 40wt%-50wt%; aluminum-containing glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; and yttrium-containing modifier, greater than 0wt% and less than or equal to 8wt%.

[0116] The aforementioned silicon-containing glass components may include SiO2, etc. During the melting and cooling process, SiO2 can form a stable three-dimensional random network structure (interconnected [SiO4] tetrahedra), providing a basic framework for the matrix glass-ceramic. It can also improve the chemical stability and mechanical strength of the matrix glass-ceramic, reduce its coefficient of thermal expansion, influence melt viscosity, and regulate the forming and crystallization behavior of the matrix glass-ceramic. For example, the silicon-containing glass components may be 40wt%, 42wt%, 44wt%, 46wt%, 48wt%, or 50wt% by mass percentage, etc.

[0117] The aforementioned aluminum-containing glass components may include Al2O3, etc. Al2O3 can exist simultaneously in tetrahedral and octahedral structures, and the Al content of Al2O3... 3+ It can be tetracoordinated ([AlO4]). - The aluminum oxide tetrahedrons enter the SiO2 network in the form of [SiO4] tetrahedra, connecting with them to make the structure more compact. Therefore, increasing the content of Al2O3 can increase the content of aluminum oxide tetrahedrons, resulting in high-modulus, high-density matrix glass-ceramics.

[0118] Significantly, the aluminum-containing glass component can be selected to be 25wt%-30wt% by mass percentage. For example, the aluminum-containing glass component can be 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, or 30wt% by mass percentage, etc.

[0119] The spinel composition mentioned above may include TO, wherein T may include any one of Mg, Mg and Zn. When the spinel composition is Mg, pure magnesium spinel crystal MgAl2O4 can be formed; when the spinel composition is Mg and Zn, zinc magnesium spinel crystal (Mg,Zn)Al2O4 can be formed.

[0120] Significantly, the spinel component can be selected as 1wt%-10wt% by mass percentage. For example, the spinel component by mass percentage can be 1wt%, 2wt%, 4wt%, 6wt%, 8wt%, or 10wt%, etc.

[0121] It should be noted that during the formation of spinel, spinels with low energy barriers are formed first, followed by spinels with high energy barriers. Since the energy barrier of zinc-magnesium spinel crystals is lower than that of pure magnesium spinel crystals, if the formula contains Zn and Mg, only zinc-magnesium spinel crystals will be formed.

[0122] The aforementioned self-nucleating agent may include XO2, wherein X may include one or more of titanium (Ti) and zirconium (Zr). Ti and / or Zr can directly serve as crystal nuclei, reducing the activation energy of crystal nucleation by providing a heterogeneous interface, allowing crystallization to occur at a lower temperature, thereby inducing controllable crystallization and achieving the transformation from ordinary glass to glass-ceramics. This avoids surface nucleation (non-uniformity) during spontaneous crystallization of the glass, instead achieving uniform nucleation in the bulk phase. For example, the self-nucleating agent may be 1 wt%, 2 wt%, 4 wt%, 6 wt%, 7 wt%, or 8 wt% by mass percentage, etc.

[0123] It should be noted that Zn, Mg, and Al in spinel crystals can all form bonds through O, while the self-nucleating agent only acts as the crystal nucleus to create the lowest energy point, causing other elements to concentrate there and form spinel crystals that are coated on the outer surface of the self-nucleating agent and do not participate in the spinel crystal.

[0124] The aforementioned yttrium-containing modifiers may include Y₂O₃, etc., where Y₂O₃ contains Y 3+ The coordination number is 6 (octahedral), and the YO bond angle is about 90°-110°, which is smaller than that of typical glass network forgings (e.g., the Si-O-Si bond angle in SiO2 is about 144°). The smaller bond angle means that the coordination polyhedron (e.g., [YO6]) is more distorted, which allows the three-dimensional random network structure to aggregate in a smaller shape, promotes more compact atomic packing, regulates the density of the three-dimensional random network structure, and improves the modulus and strength of the matrix glass-ceramic.

[0125] Significantly, the yttrium-containing modifier can be selected in the range of 1wt% to 8wt% by mass, and further, the yttrium-containing modifier can be selected in the range of 1wt% to 5wt% by mass. For example, the yttrium-containing modifier can be 1wt%, 2wt%, 3wt%, 4wt%, or 5wt% by mass, etc.

[0126] As a first example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%.

[0127] As a second example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%.

[0128] As a third example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or Mg,ZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%.

[0129] As a fourth example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%.

[0130] The microcrystalline glass provided in this application embodiment, on the one hand, increases the density and chemical bond energy of the three-dimensional random network structure of the matrix microcrystalline glass by containing atoms such as silicon, aluminum, and yttrium in the glass phase, thereby improving the modulus and bond energy volume density of the matrix microcrystalline glass, and thus significantly improving the intrinsic strength and hardness of the microcrystalline glass; on the other hand, the matrix microcrystalline glass has magnesium spinel crystals or zinc magnesium spinel crystals with higher elastic modulus and hardness as the main crystal phase, which not only ensures optical performance, but also improves the ability to resist the lateral propagation of cracks when facing sharp objects or friction and puncture scenarios. Therefore, the combination of the two factors works together at both the glass body and crystal type levels. When an external force first hits the glass phase of the microcrystalline glass and causes a crack, and the crack then extends inward and comes into contact with the internal spinel crystal, the microcrystalline glass can absorb the crack propagation according to its own crystal vibration, making the crack very shallow and not easily seen by the naked eye. Therefore, the overall scratch resistance of the magnesium aluminum silicon system microcrystalline glass in this application embodiment is higher than that of ordinary lithium aluminum silicon glass with silicon dioxide as the main component and silicate microcrystalline glass with lithium disilicate crystal as the main component in the related technology.

[0131] Therefore, applying the magnesium aluminum silicon system microcrystalline glass of this application embodiment to electronic devices, such as to cover plates, can improve the service life of electronic devices, enhance the aesthetics of cover plates, and improve the overall performance and user experience of electronic devices.

[0132] Optionally, as an achievable method, the matrix microcrystalline glass provided in this application embodiment comprises, by weight percentage, the following components: silicon-containing glass component, 40wt%-50wt%; aluminum-containing glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; yttrium-containing modifier, greater than 0wt% and less than or equal to 8wt%; and flux, 1wt%-5wt%.

[0133] In applications, the flux mentioned above may include one or more of boron trioxide (B2O3) and phosphorus pentoxide (P2O5). For example, the flux may be 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt% by mass percentage, etc.

[0134] As a first example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3 and / or P2O5, 1wt%-5wt%.

[0135] As a second example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3 and / or P2O5, 1wt%-5wt%.

[0136] As a third example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; B2O3 and / or P2O5, 1wt%-5wt%.

[0137] As a fourth example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; B2O3 and / or P2O5, 1wt%-5wt%.

[0138] The microcrystalline glass provided in this application has a high content of both silicon-containing glass components and aluminum-containing glass components. By including a flux in the matrix microcrystalline glass, the flux can lower the melting point of the raw materials during the preparation of the matrix microcrystalline glass, so that the melting temperature is not too high and a good melting effect can be achieved. This is beneficial for industrial production and saves energy and costs, thereby meeting the needs of mass production.

[0139] Optionally, as one possible implementation, the microcrystalline glass provided in this application embodiment comprises, by weight percentage, the following components: silicon-containing glass component, 40wt%-50wt%; aluminum-containing glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; yttrium-containing modifier, greater than 0wt% and less than or equal to 8wt%; and clarifying agent, 0.05wt%-0.7wt%.

[0140] In applications, clarifying agents may include antimony trioxide (Sb₂O₃), etc. For example, the clarifying agent may be 0.05 wt%, 0.1 wt%, 0.3 wt%, 0.5 wt%, or 0.7 wt% by mass percentage, etc.

[0141] As a first example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; Sb2O3, 0.05wt%-0.7wt%.

[0142] As a second example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or Mg,ZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; Sb2O3, 0.05wt%-0.7wt%.

[0143] As a third example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; Sb2O3, 0.05wt%-0.7wt%.

[0144] As a fourth example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; Sb2O3, 0.05wt%-0.7wt%.

[0145] The microcrystalline glass provided in this application embodiment contains a clarifying agent in the matrix glass, which can discharge a large amount of gas generated during the melting process of the matrix glass. For example, small bubbles become large bubbles, and the large bubbles are discharged from the microcrystalline glass, thereby making the microcrystalline glass more uniform, clearer, and more transparent, thus meeting its requirements as a cover plate.

[0146] Optionally, as one possible approach, the microcrystalline glass provided in this application embodiment includes a matrix microcrystalline glass and a first chemical strengthening layer, wherein the first chemical strengthening layer includes a Na / Li exchange layer and the Na / Li exchange layer coats the matrix microcrystalline glass.

[0147] It should be understood that Na / Li exchange layer coated matrix glass-ceramics refers to the entire outer surface of Na / Li exchange layer coated matrix glass-ceramics.

[0148] The matrix microcrystalline glass provided in this application embodiment comprises, by weight percentage, the following components: silicon-containing glass component, 40wt%-50wt%; aluminum-containing glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; yttrium-containing modifier, greater than 0wt% and less than or equal to 8wt%; and first chemical strengthening component, 1wt%-8wt%.

[0149] In applications, the first chemically enhanced component may include R2O, wherein R may include one or more of lithium (Li) and sodium (Na). Exemplarily, the first chemically enhanced component may be 1 wt%, 3 wt%, 5 wt%, 6 wt%, 7 wt%, or 8 wt% by mass percentage, etc.

[0150] As a first example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; Li2O and / or Na2O, 1wt%-8wt%.

[0151] As a second example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; Li2O and / or Na2O, 1wt%-8wt%.

[0152] As a third example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; Li2O and / or Na2O, 1wt%-8wt%.

[0153] As a fourth example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; Li2O and / or Na2O, 1wt%-8wt%.

[0154] The microcrystalline glass provided in this application embodiment can improve the impact resistance of the microcrystalline glass by covering the matrix microcrystalline glass with a first chemical strengthening layer. At the same time, it can also improve the microcrystalline glass's resistance to punctures from rough ground and has high optical properties such as light transmittance.

[0155] Optionally, as one possible approach, the microcrystalline glass provided in this application embodiment includes a matrix microcrystalline glass, a first chemical strengthening layer and a second chemical strengthening layer. The first chemical strengthening layer includes a Na / Li exchange layer, and the second chemical strengthening layer includes a K / Na exchange layer. The Na / Li exchange layer covers the matrix microcrystalline glass, and the K / Na exchange layer covers the Na / Li exchange layer.

[0156] It should be understood that the K / Na exchange layer covering the Na / Li exchange layer means that the K / Na exchange layer covers the entire outer surface of the Na / Li exchange layer.

[0157] The matrix microcrystalline glass provided in this application embodiment comprises, by weight percentage, the following components: silicon-containing glass component, 40wt%-50wt%; aluminum-containing glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; yttrium-containing modifier, greater than 0wt% and less than or equal to 8wt%; first chemical strengthening component, 1wt%-8wt%; and second chemical strengthening component, 1wt%-8wt%.

[0158] In applications, the E in the second chemical fortification component E2O may include one or more of Na and potassium (K). For example, the second chemical fortification component may be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, or 8 wt% by mass percentage, etc.

[0159] As a first example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; and at least one of Li2O, Na2O, and K2O, 1wt%-8wt%.

[0160] As a second example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; and at least one of Li2O, Na2O, and K2O, 1wt%-8wt%.

[0161] As a third example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; and at least one of Li2O, Na2O, and K2O, 1wt%-8wt%.

[0162] As a fourth example, the matrix microcrystalline glass of this application embodiment may include, by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-10wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-5wt%; and at least one of Li2O, Na2O, and K2O, 1wt%-8wt%.

[0163] The microcrystalline glass provided in this application embodiment further improves the high impact resistance of the microcrystalline glass and its resistance to drops from rough ground by covering the first chemical strengthening layer with a second chemical strengthening layer, that is, adding a potassium layer outside the first chemical strengthening layer.

[0164] Optionally, as one possible approach, the microcrystalline glass provided in this application embodiment includes a matrix microcrystalline glass, a first chemical strengthening layer, a second chemical strengthening layer, and a protective layer. The first chemical strengthening layer includes a Na / Li exchange layer, the second chemical strengthening layer includes a K / Na exchange layer, the Na / Li exchange layer covers the matrix glass, the K / Na exchange layer covers the Na / Li exchange layer, and the protective layer covers the K / Na exchange layer.

[0165] It should be understood that the protective layer covering the K / Na exchange layer means that the protective layer covers the entire outer surface of the K / Na exchange layer.

[0166] In applications, the aforementioned protective layer may include film layers with special functions such as anti-fingerprint (AF) layers, and no specific limitations are made here. The material of the AF layer may include perfluoropolyether siloxane structures with anti-fingerprint effects.

[0167] The microcrystalline glass provided in this application embodiment has a protective layer covering the second chemical strengthening layer, which can further reduce the risk of the microcrystalline glass being scratched, bruised, or broken, and the overall performance of the microcrystalline glass is better.

[0168] The following is a specific embodiment of a microcrystalline glass provided in this application.

[0169] The specific formulation of the matrix microcrystalline glass in this application embodiment, based on mass percentage, is as follows: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3 and / or P2O5, 1wt%-5wt%; Sb2O3, 0.05wt%-0.7wt%.

[0170] Figure 5 The image shows the morphology of crack propagation in pure magnesium spinel crystal MgAl2O4 according to an embodiment of this application. Figure 6 The stress-strain simulation curves of pure magnesium spinel crystal MgAl2O4 from embodiments of this application and silicate microcrystalline glass (Li2Si2O5) mainly composed of lithium disilicate crystals in related technologies are shown. Figure 6 In the figure, the horizontal axis represents strain and the vertical axis represents stress, with the unit being GPa.

[0171] like Figure 5 As shown, the pure magnesium spinel crystal MgAl2O4 of this application embodiment can withstand more crack propagation energy after being subjected to puncture energy impact, thus significantly reducing the risk of failure; and even if the crack propagation energy exceeds the withstand range of pure magnesium spinel crystal MgAl2O4, the direction of chemical bond breakage is the direction of penetrating the crystal, i.e., transgranular fracture. Thus, from a visual perspective, the crack is relatively fine. Figure 5 Compared to the crack width w1 in the middle Figure 4 The w02 in it is relatively small. For zinc-magnesium spinel crystal (Mg,Zn)Al2O4, please refer to pure magnesium spinel crystal MgAl2O4; further details will not be provided here.

[0172] like Figure 6 As shown, the MgAl2O4 in this application has a higher resistance to deformation than Li2Si2O5 in related technologies. The MgAl2O4 crystals in the glass-ceramic can effectively absorb crack propagation energy, so that the crack does not extend along the grain boundary, but rather fractures through the grain. Thus, from a visual perspective, the crack is relatively fine.

[0173] Optionally, as an achievable method, the crystallinity of the main crystalline phase of the microcrystalline glass provided in the embodiments of this application is greater than or equal to 45%.

[0174] Significantly, the crystallinity of the main crystalline phase of the glass-ceramic can be selected to be greater than or equal to 50%. For example, the crystallinity of the main crystalline phase of the glass-ceramic can be 50%, 60%, 70%, 80%, or 90%, etc.

[0175] The microcrystalline glass provided in this application has a higher crystallinity of the main crystalline phase, meaning that the main crystalline phase forms a more complete and regular crystal structure. This makes the atomic arrangement inside the microcrystalline glass more compact and orderly, increasing its hardness and thus effectively resisting scratches and friction, reducing scratches or damage. At the same time, the main crystalline phase grows uniformly during the crystallization process, reducing defects and weak areas inside the microcrystalline glass. This allows it to withstand external forces more evenly, making it less prone to stress concentration in local areas that could lead to scratches or damage. Furthermore, high crystallinity means that more atoms are in a stable chemical bond state. Therefore, when subjected to scratches and friction, more energy is required to break these chemical bonds, thus giving the microcrystalline glass better scratch resistance.

[0176] Optionally, as one possible approach, the shape of the main crystalline phase of the microcrystalline glass provided in this application embodiment includes a spherical shape, and the diameter of the sphere includes 10nm-20nm.

[0177] For example, the diameter of the sphere can be 10nm, 12nm, 14nm, 16nm, 17nm, or 20nm, etc.

[0178] The microcrystalline glass provided in this application embodiment has a more uniform and ordered internal structure by making the grain size of pure magnesium spinel or zinc magnesium spinel smaller, which can enhance the hardness of the main crystalline phase. At the same time, the small-diameter pure magnesium spinel or zinc magnesium spinel can make the internal stress distribution of the microcrystalline glass more uniform. In this way, the microcrystalline glass can resist the lateral propagation of cracks when facing sharp objects or friction and puncture scenarios, so that the cracks are very shallow and difficult to propagate laterally. In addition, they are not easily seen by the naked eye, and the microcrystalline glass has better performance.

[0179] Optionally, as one possible approach, the microcrystalline glass provided in this application embodiment has a density greater than or equal to 2.8 g / cm³. 3 .

[0180] Significantly, the density of the microcrystalline glass can be selected to be greater than or equal to 3.0 g / cm³. 3 Furthermore, the density of the microcrystalline glass can be selected to be greater than or equal to 3.1 g / cm³. 3 For example, the density of the microcrystalline glass can be 3.1 g / cm³. 3 3.2g / cm 3 3.3g / cm 3 3.4g / cm 3 3.5g / cm 3 Or 3.0g / cm 3 wait.

[0181] The microcrystalline glass provided in this application has a high density, which can improve its hardness and enhance its scratch resistance. At the same time, the dense structure has a stronger ability to absorb impact energy, which can reduce the risk of breakage when dropped. In addition, the dense structure can also reduce the penetration of corrosive substances and improve acid and alkali resistance, thus making the microcrystalline glass have better overall performance.

[0182] Optionally, as an implementation method, the grayscale value of the microcrystalline glass provided in this application embodiment is less than or equal to 1.5 when rubbed with 1500gf garnet sandpaper.

[0183] In applications, garnet sandpaper can have a mesh size of 220, etc.

[0184] For example, the grayscale value of the microcrystalline glass under 1500gf and 220-grit garnet sandpaper can be 0.5, 0.8, 1.0, 1.2, 1.4 or 1.5, etc.

[0185] It should be noted that 1500gf refers to the load.

[0186] The microcrystalline glass provided in this application embodiment has a small grayscale value under 1500gf garnet sandpaper friction, indicating that under the same friction conditions, the color change of the microcrystalline glass surface is not obvious, its surface remains relatively intact, and there are no large number of scratches or damages caused by friction. In addition, the surface hardness of the microcrystalline glass is high, and at the same time, the internal structure of the microcrystalline glass remains relatively stable and has good wear resistance. Thus, the microcrystalline glass has good scratch resistance.

[0187] Optionally, as an achievable method, the microcrystalline glass provided in this application embodiment has a transmittance of greater than or equal to 88% at a wavelength of 550nm when the thickness is 0.5mm-0.65mm.

[0188] Significantly, the microcrystalline glass can be selected with a transmittance of 91% or greater at a wavelength of 550nm when the thickness is 0.5mm-0.65mm. For example, the transmittance of the microcrystalline glass at a wavelength of 550nm when the thickness is 0.65mm can be 91%, 92%, 93%, 94%, 95%, or 96%, etc.

[0189] The microcrystalline glass provided in this application embodiment has good transmittance at a wavelength of 550nm, with minimal absorption and scattering of light, maintaining the intensity and direction of light propagation, thereby providing a clear and transparent visual effect. Furthermore, after the microcrystalline glass is made into a cover plate, it can be directly placed on the display screen without affecting its normal display function.

[0190] Optionally, as an achievable method, the microcrystalline glass provided in this application embodiment has a reflectivity of less than or equal to 10% at a wavelength of 550nm when the thickness is 0.5mm-0.65mm.

[0191] Significantly, the microcrystalline glass can be selected with a reflectance of less than or equal to 8% at a wavelength of 550nm when the thickness is 0.5mm-0.65mm. For example, the reflectance of the microcrystalline glass at a wavelength of 550nm when the thickness is 0.65mm can be 1%, 2%, 4%, 5%, 6%, or 8%, etc.

[0192] The microcrystalline glass provided in this application has good reflectivity at a wavelength of 550nm, allowing more light to pass through and resulting in excellent optical performance. Therefore, when this microcrystalline glass is applied to a cover plate, the display can be clearer and the colors more realistic. Simultaneously, in strong light environments, it can reduce ambient light interference and improve visual comfort.

[0193] Optionally, as an achievable method, the microcrystalline glass provided in this application embodiment has a haze of less than or equal to 2.0% when the thickness is 0.5mm-0.65mm.

[0194] Significantly, the microcrystalline glass can be selected to have a haze of less than or equal to 0.5% when the thickness is 0.5mm-0.65mm. For example, the haze of the microcrystalline glass when the thickness is 0.5mm-0.65mm can be 0.1%, 0.2%, 0.3%, 5%, 0.4%, or 0.5%, etc.

[0195] The microcrystalline glass provided in this application has low haze, meaning that the internal crystal structure of the microcrystalline glass is uniform and has few defects. Light passing through the microcrystalline glass mainly travels in straight lines with minimal scattering. Therefore, when this microcrystalline glass is applied to a cover plate, it can make the image displayed on the screen sharper and more detailed. At the same time, it can also improve the contrast of the screen, reduce color distortion, reduce fingerprints and oil stains, and maintain long-term light transmittance.

[0196] Optionally, as one possible approach, the Young's modulus of the microcrystalline glass provided in this application embodiment is greater than or equal to 98 GPa.

[0197] Significantly, the Young's modulus of the glass-ceramic can be selected to be greater than or equal to 110 GPa. For example, the Young's modulus of the glass-ceramic can be 110 GPa, 120 GPa, 130 GPa, 140 GPa, 150 GPa, or 160 GPa, etc.

[0198] The microcrystalline glass provided in this application has a large Young's modulus, which gives it high stiffness and resistance to deformation. This allows its surface to withstand greater external forces without easily undergoing plastic deformation, increasing surface hardness and making it less susceptible to scratches or damage from sharp objects. Furthermore, when an object attempts to scratch the microcrystalline glass, the large Young's modulus effectively disperses the external force over a larger area, preventing the force from concentrating at a localized point and causing scratches. In addition, the large Young's modulus enables the microcrystalline glass to resist wear caused by friction, reducing the likelihood of surface scratches and thus maintaining surface smoothness and integrity.

[0199] Optionally, as one possible approach, the microcrystalline glass provided in this application embodiment has a Vickers hardness greater than or equal to 930 HV.

[0200] Significantly, the Vickers hardness of the glass-ceramic can be selected to be greater than or equal to 980 HV. For example, the Vickers hardness of the glass-ceramic can be 980 HV, 990 HV, 1000 HV, 1100 HV, 1200 HV, or 1300 HV, etc.

[0201] The microcrystalline glass provided in this application has a high Vickers hardness, allowing its surface to withstand greater pressure without producing obvious indentations or scratches. Thus, when a sharp object comes into contact with the microcrystalline glass surface, the high Vickers hardness effectively resists the object's penetration, reducing scratches or damage. Simultaneously, the microcrystalline glass surface has a tight atomic bond and a stable structure, resulting in high surface strength that allows it to withstand friction and impact from external objects without easily sustaining damage. Furthermore, it better maintains a smooth surface, reducing scratches caused by wear, extending its service life, and preserving good appearance and performance.

[0202] The preparation method of the microcrystalline glass provided in the embodiments of this application is described in detail below according to the following formula: silicon glass component, 40wt%-50wt%; aluminum glass component, greater than or equal to 25wt%; spinel component, 1wt%-12wt%; self-nucleating agent, 1wt%-8wt%; yttrium modifier, greater than 0wt% and less than or equal to 8wt%.

[0203] like Figure 7 As shown, the method for preparing microcrystalline glass provided in this application includes the following steps:

[0204] S1. Select each component as raw material according to the formula and mix them. After melting all components at high temperature and maintaining the mixture for a period of time, perform cooling and annealing treatments in sequence to obtain matrix glass bricks.

[0205] S2. The matrix glass bricks are subjected to high-temperature nucleation treatment and high-temperature crystallization treatment in sequence to obtain matrix microcrystalline glass.

[0206] The matrix glass-ceramic includes a main crystalline phase and a glass phase. The glass phase encapsulates the main crystalline phase, which includes magnesium spinel crystals or zinc magnesium spinel crystals. The glass phase includes at least silicon atoms, aluminum atoms, and yttrium atoms, and has a three-dimensional random network structure.

[0207] The method for preparing glass-ceramics provided in this application not only produces a glass phase with high silicon and aluminum content and containing yttrium, but also introduces more network forgings and high bond energy components into the matrix glass-ceramics, thereby obtaining glass-ceramics with high modulus, high density, and high hardness. Furthermore, through nucleation and crystallization treatments, highly crystalline, small-sized spinel crystals can be precipitated. The spinel crystals are encapsulated by the glass phase, so when crack propagation encounters the spinel crystals, the spinel crystals offset the crack propagation energy through their intrinsic strength, making it difficult for the crack to propagate further. Moreover, if the crack propagation capacity is greater than the intrinsic strength of the spinel crystals, the crack will propagate along the low bond energy positions of the crystal lattice points rather than laterally, greatly enhancing the scratch resistance of the glass-ceramics. In addition, the nucleation and crystallization temperatures in this preparation method are not high, resulting in low energy consumption and low cost, which is beneficial for industrial production and application.

[0208] The preparation method of the microcrystalline glass provided in the embodiments of this application is described in detail below according to the following formula: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4, 1wt%-12wt%; TiO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3, 1wt%-5wt%; Sb2O3, 0.05wt%-0.7wt%; Li, Na, K, 1wt%-8wt%.

[0209] like Figure 8 As shown, the method for preparing microcrystalline glass provided in this application includes the following steps:

[0210] S11. According to the mass percentage, select 40wt%-50wt% SiO2, 25wt%-30wt% Al2O3, 1wt%-8wt% Li2O, Na2O and K2O, 1wt%-12wt% MgO, 1wt%-8wt% TiO2, 1wt%-5wt% B2O3, 1wt%-8wt% Y2O3, and 0.05wt%-0.7wt% Sb2O3. After preparing the glass raw materials and mixing them for a period of time, place the glass raw materials in a furnace and melt them at 1600℃-1700℃ for a period of time. Then, pour them into a cooled mold to obtain the matrix glass brick.

[0211] In applications, the mixing time can range from 20 to 40 minutes, which ensures that the glass raw materials are mixed as evenly as possible. For example, the mixing time can be 20 minutes, 25 minutes, 30 minutes, 35 minutes, or 40 minutes, etc.

[0212] The melting time can include 5-6 hours. For example, the melting temperature can be 1600℃, 1620℃, 1640℃, 1650℃, 1660℃, or 1700℃, and the melting time can be 5 hours, 5.2 hours, 5.4 hours, 5.6 hours, 5.8 hours, or 6 hours. A melting temperature of 1600℃-1700℃ allows all raw materials to be molten, but this temperature is not excessively high, which is beneficial for industrial production, reduces energy consumption, and lowers costs.

[0213] During the above melting process, SiO2 can form a stable three-dimensional random network structure ([SiO4] tetrahedra are interconnected), and Al2O3... 3+ It can be tetracoordinated ([AlO4]). - Y2O3 enters the SiO2 network in the form of [SiO4] tetrahedrons, connecting with them to make the three-dimensional random network structure more compact, with higher modulus and greater density. At the same time, Y2O3 can also participate in the three-dimensional random network structure, making the three-dimensional random network structure more compact, with higher modulus and greater density.

[0214] In applications, the cooled mold can include a cooled metal mold, such as a cooled iron plate. The reason for immediately cooling the molten raw material is that: under heat treatment at 1600℃-1700℃, the glass raw material undergoes a solid-state reaction. For example, the oxygen-oxygen bonds in the silicon-oxygen tetrahedra of SiO2 break, and the oxygen-oxygen bonds in Al2O3 break, reconnecting by sharing a single oxygen atom as a bridging bond, forming a three-dimensional random network structure. However, no chemical reaction occurs, leaving the glass raw material with only the three-dimensional random network structure of the glass phase. This structure is metastable. When followed by rapid cooling, the three-dimensional random network structure does not have time to transform into a lower-energy crystal and remains as a three-dimensional random network structure, forming a matrix glass brick.

[0215] It should be noted that if no flux is added to the raw materials, the melting temperature needs to be adjusted to a higher level, such as 1800℃ or above, to completely melt the glass raw materials, which is difficult to achieve in industrial production. Therefore, in the embodiments of this application, with both Al and Si contents being high, a flux is also added, which allows the glass raw materials to be molten at 1600℃-1700℃, which is beneficial for industrial production and application.

[0216] S12. Place the matrix glass brick in an annealing furnace and anneal it at 500℃-600℃ for a period of time, then cool it with the furnace to obtain the matrix glass.

[0217] In applications, annealing time can range from 12 to 16 hours. For example, annealing temperatures can be 500°C, 520°C, 540°C, 560°C, 580°C, or 600°C, and annealing times can be 12, 13, 14, 15, or 16 hours. Because the three-dimensional irregular network structure of the matrix glass brick contains significant thermal stress, annealing raises the matrix glass brick to a certain temperature. This prevents the three-dimensional irregular network structure from being destroyed (i.e., from remelting) and releases the stress within the structure through the thermal field, making it less prone to brittle fracture.

[0218] The shape of the substrate glass brick can include cuboids, cubes, etc. When the substrate glass brick is cuboid, the dimensions of the cuboid can be 250mm × 250mm × 500mm.

[0219] S13. Place the matrix glass at 600℃-690℃ for nucleation treatment for a period of time, and then raise the temperature to 700℃-850℃ at a certain heating rate for crystallization treatment for a period of time to obtain matrix microcrystalline glass.

[0220] It should be noted that adding a nucleating agent can lower the nucleation temperature. Without a nucleating agent, the minimum nucleation temperature could reach 750℃, resulting in high energy consumption and hindering industrial production and application. Clearly, the nucleation temperature can be selected from 650℃ to 690℃; for example, the nucleation temperature could be 650℃, 660℃, 670℃, 680℃, or 690℃. The nucleation time can range from 3 hours to 5 hours; for example, the nucleation time could be 3 hours, 4 hours, or 5 hours.

[0221] Too rapid a heating rate can lead to uneven crystallization or nucleation, while too slow a rate results in poor controllability of the crystallization and nucleation degrees. Therefore, in this embodiment, the heating rate from nucleation to crystallization can be set to 10℃ / min-15℃ / min. For example, the heating rate can be 10℃ / min, 11℃ / min, 12℃ / min, 13℃ / min, 14℃ / min, or 15℃ / min. By heating the nucleation process to the crystallization process at a suitable rate, both the crystallization and nucleation processes can be relatively uniform, and the controllability of the degree of crystallization and nucleation is also better.

[0222] Significantly, the crystallization temperature can be selected from 750℃ to 800℃, and the crystallization time can be selected from 3h to 5h. For example, the crystallization temperature can be 750℃, 760℃, 770℃, 780℃, 790℃ or 800℃, etc., and the crystallization time can be 3h, 4h or 5h, etc.

[0223] Since higher temperatures result in higher nucleation efficiency, this application first selects 600℃-690℃ to increase nucleation. After a period of time, nucleation tends to saturate, and then the temperature is raised to 700℃-850℃. Mg, Al, and O gather around the nucleating agent and are arranged in a periodic and orderly manner according to the crystal structure. Then they gather and grow, making the crystal grow larger and larger. This allows for better control of the crystal size and the acquisition of a matrix microcrystalline glass with more main crystalline phases, fewer impurity crystalline phases, and greater transparency, resulting in a purer crystal phase.

[0224] The method for preparing glass-ceramics provided in this application has two aspects. First, in terms of preparing the glass phase, a glass phase with high silicon and aluminum content and containing yttrium is obtained, which can improve the density and chemical bond energy of the three-dimensional random network structure of the glass phase. That is, more network forgings and high bond energy components are introduced into the matrix glass-ceramics, resulting in glass-ceramics with high modulus, high density and high hardness. Second, in terms of preparing the crystal, nucleation and crystallization treatments are performed sequentially. The nucleating agent becomes the lowest energy point in the glass phase. Driven by the thermal force of the internal thermal field of the matrix glass-ceramics, other ions and / or atoms migrate and gather near the nucleating agent. By raising the temperature, highly crystalline, small-sized spinel crystals can be precipitated, and the spinel crystals are encapsulated by the glass phase. When a crack propagates and encounters a spinel crystal, the spinel crystal's intrinsic strength counteracts the crack propagation energy, making further propagation difficult. Furthermore, if the crack propagation potential exceeds the intrinsic strength of the spinel crystal, the crack will propagate along the lower bond energy positions of the crystal lattice points rather than laterally, significantly enhancing the scratch resistance of the glass-ceramic. In addition, this preparation method uses relatively low nucleation and crystallization temperatures, resulting in low energy consumption and low cost, which is beneficial for industrial production and application.

[0225] Alternatively, as one possible approach, such as Figure 9 As shown, after step S2, the preparation process of the microcrystalline glass provided in this application embodiment includes the following steps:

[0226] S3. Perform at least one surface treatment on the matrix glass-ceramic to obtain the initial glass-ceramic.

[0227] In applications, surface treatment may include computer numerical control (CNC) processing, polishing and grinding of the substrate glass crystal according to actual process requirements, until the surface of the substrate glass crystal is smooth and transparent, thus obtaining the initial glass crystal.

[0228] It should be noted that the initial microcrystalline glass can also be used as a cover plate at this time, so it should be cut into the corresponding cover plate size according to the actual required size.

[0229] S4. Perform at least one chemical strengthening treatment on the initial glass-ceramic to obtain glass-ceramic.

[0230] Since the atomic radii of Li, Na, and K atoms increase sequentially, a chemical strengthening process can be achieved by selecting an atomic radius in the salt solution that is larger than the atomic radius of the atoms in the initial microcrystalline glass.

[0231] The chemical strengthening treatment can include a primary chemical strengthening treatment, specifically, placing the initial glass-ceramic in a sodium-containing molten salt for a primary chemical strengthening treatment to form a Na / Li exchange layer, thus obtaining a primary strengthened glass-ceramic.

[0232] Alternatively, the chemical strengthening treatment may include two chemical strengthening treatments. Specifically, the initial glass-ceramic is placed in a sodium-containing molten salt for a first chemical strengthening treatment to form a Na / Li exchange layer, resulting in a first-strengthened glass-ceramic. Then, the first-strengthened glass-ceramic is placed in a potassium-containing molten salt for a second chemical strengthening treatment to form a K / Na exchange layer, resulting in the glass-ceramic.

[0233] In applications, sodium-containing molten salts can include any one of pure sodium nitrate (NaNO3), or a mixture of NaNO3 and potassium nitrate (KNO3). When the sodium-containing molten salt is a mixture of NaNO3 and KNO3, the mass percentage of NaNO3 in the mixture is greater than or equal to 60 wt% and less than 100 wt%. For example, the mass percentage of NaNO3 in the mixture can be 60 wt%, 70 wt%, 80 wt%, or 90 wt%. Therefore, mixed salts containing K and Na can significantly improve strengthening efficiency and enhance the performance of glass-ceramics through mechanisms such as lowering process temperature, regulating ion exchange kinetics, optimizing stress distribution, and adapting glass composition, while also balancing process stability and economic efficiency.

[0234] The primary chemical strengthening temperature can include 350℃-450℃, and the primary chemical strengthening time can include 0.1h-5h. For example, the primary chemical strengthening temperature can be 350℃, 370℃, 390℃, 400℃, 420℃, or 450℃, and the primary chemical strengthening time can be 0.1h, 1h, 2h, 3h, 4h, or 5h. By controlling the primary chemical strengthening time and temperature, the risk of over-strengthening leading to a decrease in the mechanical properties of the glass-ceramic can be reduced.

[0235] In applications, potassium-containing molten salts can include any of pure KNO3, NaNO3, and mixed salts of KNO3. When the potassium-containing molten salt is a mixed salt of NaNO3 and KNO3, the mass percentage of KNO3 in the mixed salt is greater than or equal to 80 wt% and less than 100 wt%. For example, the mass percentage of KNO3 in the mixed salt can be 80 wt%, 85 wt%, 90 wt%, or 95 wt%, etc. Therefore, mixed salts containing K and Na can significantly improve strengthening efficiency and enhance the performance of glass-ceramics through mechanisms such as reducing process temperature, regulating ion exchange kinetics, optimizing stress distribution, and adapting glass composition, while balancing process stability and economy.

[0236] The secondary chemical strengthening temperature can include 350℃-450℃, and the secondary chemical strengthening time can include 0.1h-2h. For example, the secondary chemical strengthening temperature can be 350℃, 370℃, 390℃, 400℃, 420℃, or 450℃, and the secondary chemical strengthening time can be 0.1h, 0.5h, 1h, 1.5h, or 2h. By controlling the time and temperature of the secondary chemical strengthening, the risk of over-strengthening leading to a decrease in the mechanical properties of the glass-ceramic can be reduced.

[0237] It should be noted that, in step S3, the cover plate can be cut to the required size first, and then at least one surface treatment can be performed. Alternatively, in step S3, at least one surface treatment can be performed first, and then the cover plate can be cut to the required size first. No specific limitation is made here.

[0238] In addition, in step S4, the cover plate is first cut to the required size according to the actual needs, and then at least one chemical strengthening treatment is performed. Alternatively, in step S4, at least one chemical strengthening treatment can be performed first, and then the cover plate is cut to the required size according to the actual needs. No specific limitation is made here.

[0239] The method for preparing microcrystalline glass provided in this application involves replacing atoms with larger atomic radii in the original microcrystalline glass with atoms with smaller atomic radii in a salt solution. For example, Na replaces Li, K replaces Li and / or Na. During this process, compressive stress is attached to the surface of the matrix microcrystalline glass to form at least one compressive stress layer. The compressive stress layer can resist the impact force generated during impact, further improving the scratch resistance of the microcrystalline glass. In addition, it is simple to implement and conducive to industrial production and application.

[0240] Alternatively, as one possible approach, such as Figure 10 As shown, after step S4 above, the preparation process of the microcrystalline glass provided in this application embodiment includes the following steps:

[0241] S5. A protective layer is formed on the outer surface of the first chemically reinforced layer or the second chemically reinforced layer to obtain microcrystalline glass.

[0242] It should be noted that after step S5, the cover plate can be cut to the corresponding size according to the actual needs, depending on the actual application.

[0243] The method for preparing microcrystalline glass provided in this application, by forming a protective layer, can further reduce scratches, abrasions, or breakage of microcrystalline glass. Microcrystalline glass has good performance and is also simple and easy to implement, which is conducive to industrial production and application.

[0244] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0245] Examples S1 to S6 of this application provide different compositions, different melting parameters, and different annealing parameters for the prepared microcrystalline glass, as shown in Table 1 below.

[0246] Table 1

[0247]

[0248]

[0249] It should be noted that Examples S1 to S3 of this application mainly characterize the effect of the difference between Al and Y on the three-dimensional random network density of glass-ceramics, while Examples S4 to S6 of this application mainly characterize the effect of the difference in the ratio of Mg and Zn on the crystal type of glass-ceramics.

[0250] Various heat treatments were performed on Embodiments S1 and S2 of this application as shown in Table 1 above, and the heat treatment parameters are shown in Table 2 below.

[0251] Table 2

[0252]

[0253]

[0254] As shown in Table 2, for the same glass-ceramic, the crystallinity of the glass-ceramic increases with the increase of nucleation temperature and nucleation time; the crystal size of the glass-ceramic increases slightly with the increase of crystallization temperature and crystallization time, but is still relatively small; with the increase of nucleation and crystallization temperature and time, the density of the glass-ceramic increases, the transmittance at 550 nm decreases, the refractive index at 550 nm increases, the b-value becomes more negative (the color becomes more bluish), the haze increases but is still within a small range, the Young's modulus increases, and the hardness increases.

[0255] Various heat treatments were performed on Embodiments S3 and S4 of this application as shown in Table 1 above, and the heat treatment parameters are shown in Table 3 below.

[0256] Table 3

[0257]

[0258]

[0259] As shown in Table 3, for the same glass-ceramic, the crystallinity of the glass-ceramic increases with the increase of nucleation temperature and nucleation time; the crystal size of the glass-ceramic increases slightly with the increase of crystallization temperature and crystallization time, but is still relatively small; with the increase of nucleation and crystallization temperature and time, the density of the glass-ceramic increases, the transmittance at 550 nm decreases (except for S3-3 which is devitrified), the refractive index at 550 nm increases (except for S3-3 which has an excessively large value), the b-value becomes more negative (the color becomes more bluish), the haze increases but is still within a small range, the Young's modulus increases, and the hardness increases.

[0260] It should be noted that Example S3-3 used a longer crystallization time and a higher crystallization temperature, which is exactly at the point where the crystal growth rate is the largest. The crystal grows rapidly, which leads to a surge in the crystal content in the glass-ceramic, a significant increase in scattering, glass devitrification, and a tendency to become ceramic.

[0261] Various heat treatments were performed on Embodiments S5 and S6 of this application as shown in Table 1 above, and the heat treatment parameters are shown in Table 4 below.

[0262] Table 4

[0263]

[0264]

[0265]

[0266] As shown in Table 4, for the same glass-ceramic, the crystallinity of the glass-ceramic increases with the increase of nucleation temperature and nucleation time; the crystal size of the glass-ceramic increases slightly with the increase of crystallization temperature and crystallization time, but is still relatively small; with the increase of nucleation and crystallization temperature and time, the density of the glass-ceramic increases, the transmittance at 550 nm decreases (except for S6-3 which is devitrified), the refractive index at 550 nm increases (except for S6-3 which has an excessively large value), the b-value becomes more negative (indicating a more bluish color), the haze increases but remains within a small range, the Young's modulus increases, and the hardness increases.

[0267] It should be noted that Example S6-3 used a longer crystallization time and a higher crystallization temperature, which is exactly at the point where the crystal growth rate is the largest. The crystal grows rapidly, which leads to a surge in the crystal content in the glass-ceramic, a significant increase in scattering, glass devitrification, and a tendency to become ceramic.

[0268] The relevant performance tests and results of the glass in the embodiments and comparative examples of this application are given in Tables 1 to 4 below:

[0269] 1. Grayscale value testing and calculation:

[0270] Figure 11 A schematic diagram of a grayscale value test according to an embodiment of this application is shown.

[0271] like Figure 11 As shown, a microcrystalline glass 1 is placed on a horizontal platform 21, and garnet sandpaper 22 is placed in a portion of the microcrystalline glass 1 away from the horizontal platform 21. A linear abrasion tester 23 is placed on the horizontal platform 21 and located on one side of the microcrystalline glass 1. The linear abrasion tester 23 includes a first rod 231, one end of which is in contact with the garnet sandpaper 22, and the other end of which is away from the garnet sandpaper 22 and has a weight load 24 placed on it. The first rod 231 can reciprocate along the dashed arrow.

[0272] During the test, the first rod 231 rubs back and forth along the dotted arrow. The scratches on the surface of the microcrystalline glass 1 are captured by an automated optical inspection (AOI) imaging system. Then, the weighted average is calculated to determine the grayscale value.

[0273] The load can be different loads such as 500gf, 750gf, 1000gf, 1250gf, and 1500gf.

[0274] The sandpaper is 220-grit garnet sandpaper. The shape of the garnet sandpaper can be cuboid or cube. When the garnet sandpaper is cube-shaped, the size of the garnet sandpaper can be 20×20mm.

[0275] The friction stroke can be 40mm, the friction thread can be 20mm-50mm, the friction area size of the garnet sandpaper can be 20mm×(40-70)mm, the friction speed can be 40cycle / min-60cycle / min, and the number of cycles can be 10-20 round trips.

[0276] After rubbing with garnet sandpaper 22, the scratches on the surface can be clearly shown under the AOI imaging system. At the same time, after calculating the grayscale value of each pixel in the selected area of ​​the photo using software, the weighted average is taken to obtain the final grayscale value, as shown in Table 5 below.

[0277] It should be noted that the grayscale value ranges from 0 to 255, where 0 represents pure black and 255 represents pure white. The more obvious the scratch in a certain location, the whiter it will appear, and the higher the grayscale value will be.

[0278] Table 5

[0279]

[0280]

[0281] It should be noted that Examples S1, S2, S3, S4, S5 and S6 are all precursor glasses that have not undergone two-step heat treatment.

[0282] Furthermore, since the microcrystalline glass in Examples S3-3 and S6-3 was devitrified, and AOI testing requires transparent glass to detect surface scratches, there is no data.

[0283] As shown in Table 5, the grayscale values ​​of the microcrystalline glass in this application embodiment under 1500gf load of garnet sandpaper friction are all less than or equal to 1.5, which is much lower than the grayscale values ​​of ordinary lithium aluminum silicon glass with silicon dioxide as the main component under 1500gf load of garnet sandpaper friction, and the grayscale values ​​of silicate microcrystalline glass with lithium disilicate crystal as the main component under 1500gf load of garnet sandpaper friction. This indicates that the microcrystalline glass in this application embodiment has very good scratch resistance.

[0284] Based on the above, Example S5-3 showed the lowest grayscale value under 1500gf load garnet sandpaper friction, indicating that the microcrystalline glass has the best scratch resistance.

[0285] 2. The microstructure of the scratches after rubbing with garnet sandpaper under a 1500gf load, as described in Embodiment S5-3 of this application, was obtained by scanning with a 3D profilometer. Figure 12Furthermore, by scanning the microstructure of the scratches on ordinary lithium aluminum silicon glass (mainly silica) after rubbing with garnet sandpaper under a 1500 gf load using a 3D profilometer, the following results were obtained. Figure 13 .

[0286] Figure 12 and Figure 13 Upon comparison, it can be seen that the microcrystalline glass in embodiment S5-3 of this application has very slight and shallow scratches, indicating excellent scratch resistance, while the ordinary lithium aluminum silicon glass with silicon dioxide as the main component in the related technology has severe scratches, indicating poor scratch resistance.

[0287] It should be understood that the above description is merely to help those skilled in the art better understand the embodiments of this application, and is not intended to limit the scope of the embodiments of this application. Those skilled in the art can obviously make various equivalent modifications or variations based on the examples given above, or combinations of any two or more of the above embodiments. Such modifications, variations, or combinations also fall within the scope of the embodiments of this application.

[0288] It should also be understood that the above description of the embodiments of this application focuses on highlighting the differences between the various embodiments. Any similarities or differences not mentioned can be referred to each other. For the sake of brevity, they will not be repeated here.

[0289] It should also be understood that the methods, situations, categories, and classifications of embodiments in this application are for the convenience of description only and should not constitute a special limitation. Various methods, categories, situations, and features in embodiments can be combined without contradiction.

[0290] It should also be understood that, in the various embodiments of this application, unless otherwise specified or in case of logical conflict, the terms and / or descriptions between different embodiments are consistent and can be referenced by each other, and the technical features in different embodiments can be combined to form new embodiments according to their inherent logical relationships.

[0291] Finally, it should be noted that the above descriptions are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions within the technical scope disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A microcrystalline glass, characterized in that, include: The matrix microcrystalline glass comprises a main crystalline phase and a glass phase, wherein the glass phase encapsulates the main crystalline phase, the main crystalline phase comprises magnesium spinel crystals or zinc magnesium spinel crystals, and the glass phase comprises at least silicon atoms, aluminum atoms and yttrium atoms, and the glass phase has a three-dimensional random network structure.

2. The microcrystalline glass according to claim 1, characterized in that, The microcrystalline glass comprises the following components by weight percentage: Silicon glass component, 40wt%-50wt%; Aluminum glass component, greater than or equal to 25 wt%; Spinel component, 1wt%-12wt%; Self-nucleating agent, 1wt%-8wt%; Contains yttrium modifier, greater than 0 wt% and less than or equal to 8 wt%.

3. The microcrystalline glass according to claim 2, characterized in that, The microcrystalline glass, by weight percentage, also includes the following components: Flux, 1wt%-5wt%.

4. The microcrystalline glass according to claim 2 or 3, characterized in that, The microcrystalline glass, by weight percentage, also includes the following components: Clarifying agent, 0.05wt%-0.7wt%.

5. The microcrystalline glass according to any one of claims 2 to 4, characterized in that, The silicon-containing glass component includes silicon dioxide; The aluminum-containing glass component includes aluminum oxide; The spinel component includes TO, wherein T includes any one of magnesium, magnesium and zinc; The self-nucleating agent includes XO2, wherein X includes at least one of titanium and zirconium; The yttrium-containing modifier includes yttrium trioxide; The flux includes at least one of boron trioxide and phosphorus pentoxide; The clarifying agent includes antimony trioxide.

6. The microcrystalline glass according to any one of claims 1 to 5, characterized in that, The glass-ceramic further includes a first chemical strengthening layer, which includes a Na / Li exchange layer that coats the matrix glass-ceramic.

7. The microcrystalline glass according to claim 6, characterized in that, The matrix glass-ceramic, by weight percentage, also includes the following components: The first chemical strengthening component, 1 wt%-8 wt%, comprises R2O, wherein R comprises at least one of lithium and sodium.

8. The microcrystalline glass according to claim 6, characterized in that, The microcrystalline glass further includes a second chemical strengthening layer, which includes a K / Na exchange layer that covers the Na / Li exchange layer.

9. The microcrystalline glass according to claim 8, characterized in that, The matrix glass-ceramic, by weight percentage, also includes the following components: The second chemical fortifying component, 1 wt%-8 wt%; the second chemical fortifying component includes E2O, wherein E includes at least one of sodium and potassium.

10. The microcrystalline glass according to any one of claims 1 to 9, characterized in that, The microcrystalline glass comprises the following components by weight percentage: SiO2, 40wt%-50wt%; Al2O3, 25wt%-30wt%; MgAl2O4 or MgZnAl2O4, 1wt%-12wt%; TiO2 and / or ZrO2, 1wt%-8wt%; Y2O3, 1wt%-8wt%; B2O3 and / or P2O5, 1wt%-5wt%; Sb₂O₃, 0.05wt%-0.7wt%.

11. The glass-ceramic according to any one of claims 1 to 10, characterized in that, The crystallinity of the main crystalline phase is greater than or equal to 45%.

12. The microcrystalline glass according to any one of claims 1 to 10, characterized in that, The main crystalline phase has a spherical shape, and the diameter of the sphere is between 10 nm and 20 nm.

13. The microcrystalline glass according to any one of claims 1 to 10, characterized in that, The density of the microcrystalline glass is greater than or equal to 2.8 g / cm³. 3 .

14. The microcrystalline glass according to any one of claims 1 to 10, characterized in that, The grayscale value of the microcrystalline glass under rubbing with 1500gf garnet sandpaper is less than or equal to 1.

5.

15. The glass-ceramic according to any one of claims 1 to 10, characterized in that, The microcrystalline glass, with a thickness of 0.5mm-0.65mm, has a transmittance of greater than or equal to 88% at a wavelength of 550nm.

16. The microcrystalline glass according to any one of claims 1 to 10, characterized in that, The microcrystalline glass, with a thickness of 0.5mm-0.65mm, has a reflectivity of less than or equal to 10% at a wavelength of 550nm.

17. The microcrystalline glass according to any one of claims 1 to 10, characterized in that, The microcrystalline glass has a haze of less than or equal to 2.0% when its thickness is 0.5mm-0.65mm.

18. The glass-ceramic according to any one of claims 1 to 10, characterized in that, The Young's modulus of the microcrystalline glass is greater than or equal to 98 GPa.

19. The glass-ceramic according to any one of claims 1 to 10, characterized in that, The Vickers hardness of the microcrystalline glass is greater than or equal to 930 HV.

20. An electronic device, characterized in that, Includes a glass component, wherein the glass component is a microcrystalline glass as described in any one of claims 1 to 19.

21. A method for preparing microcrystalline glass, characterized in that, include: The silicon-containing glass component, aluminum-containing glass component, spinel component, self-nucleating agent and yttrium-containing regulator are mixed as raw materials. After the raw materials are melted at a certain temperature and held for a period of time, they are then subjected to cooling treatment and annealing treatment in sequence to obtain matrix glass bricks. The matrix glass brick is subjected to nucleation and crystallization treatments in sequence to obtain matrix microcrystalline glass; wherein, the matrix microcrystalline glass includes a main crystalline phase and a glass phase, the glass phase encapsulates the main crystalline phase, the main crystalline phase includes magnesium spinel crystals or zinc magnesium spinel crystals, the glass phase includes at least silicon atoms, aluminum atoms and yttrium atoms, and the glass phase has a three-dimensional random network structure.

22. The method for preparing microcrystalline glass according to claim 21, characterized in that, The process involves mixing silicon-containing glass components, aluminum-containing glass components, spinel components, self-nucleating agents, and yttrium-containing modifiers as raw materials. After melting the raw materials at a certain temperature and maintaining this temperature for a period of time, the mixture is then subjected to sequential cooling and annealing treatments to obtain matrix glass bricks, including: According to the mass percentage, 40wt%-50wt% of SiO2, greater than or equal to 25wt% of Al2O3, 1wt%-12wt% of MgO or MgO and ZnO, 1wt%-8wt% of TiO2 and / or ZrO2, 1wt%-8wt% of Y2O3, 1wt%-5wt% of B2O3 and / or P2O5, and 0.05wt%-0.7wt% of Sb2O3 are selected as raw materials and mixed for a period of time. The raw materials are then melted at 1600℃-1700℃ for a period of time and then poured into a cooled mold to obtain the matrix glass brick. The step of sequentially performing nucleation and crystallization treatments on the matrix glass brick to obtain matrix microcrystalline glass includes: The matrix glass bricks are annealed at 500℃-600℃ for a period of time and then cooled to obtain matrix glass. The matrix glass is nucleated at 600℃-690℃ for a period of time, and then crystallized at 700℃-850℃ for a period of time to obtain the matrix microcrystalline glass.

23. The method for preparing microcrystalline glass according to claim 22, characterized in that, The raw materials, selected by weight percentage, consist of 40wt%-50wt% SiO2, ≥25wt% Al2O3, 1wt%-12wt% MgO or MgO and ZnO, 1wt%-8wt% TiO2 and / or ZrO2, 1wt%-8wt% Y2O3, 1wt%-5wt% B2O3 and / or P2O5, and 0.05wt%-0.7wt% Sb2O3. After mixing for a period of time, the raw materials are melted at 1600℃-1700℃ for a period of time, and then poured into a cooled mold to obtain the matrix glass brick. According to the mass percentage, 40wt%-50wt% of SiO2, greater than or equal to 25wt% of Al2O3, 1wt%-12wt% of MgO or MgO and ZnO, 1wt%-8wt% of TiO2 and / or ZrO2, 1wt%-8wt% of Y2O3, 1wt%-5wt% of B2O3 and / or P2O5, 0.05wt%-0.7wt% of Sb2O3, and 1wt%-8wt% of Li2O, Na2O and K2O are selected as raw materials and mixed for a period of time. The raw materials are then melted at 1600℃-1700℃ for a period of time and then poured into a cooled mold to obtain the matrix glass brick. After nucleating the matrix glass at 600℃-690℃ for a period of time, and then crystallizing it at 700℃-850℃ for a period of time to obtain the matrix microcrystalline glass, the preparation method further includes: The matrix glass-ceramic is subjected to at least one surface treatment to obtain an initial glass-ceramic; The initial glass-ceramic is subjected to at least one chemical strengthening treatment to obtain the glass-ceramic.