A gradient ultrathin glass based on surface pre-modification, its preparation method and application
By performing regional pre-modification treatment on the surface of ultrathin glass and using etching accelerators and etching decelerators to form a gradient thickness structure, the problems of large equipment investment, high cost and low yield in the existing technology are solved, and high-performance gradient ultrathin glass preparation is realized, which is suitable for devices such as foldable screens.
Patent Information
- Application Number
- CN202611236127.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing gradient ultrathin glass suffer from problems such as large equipment investment, complex production line modification, high production costs, low product yield, and unstable performance, making it difficult to meet the high optical and mechanical requirements of foldable screen cover glass.
By performing regional pre-modification treatment on the surface of ultrathin glass, etching accelerators and etching decelerators are used to form gradient thickness structures in different regions. Combined with the overall HF etching process, the thickness differentiation design of the bending zone, transition zone and fixed zone is achieved.
This technology enables the production of ultra-thin glass with a thinner bending zone and a thicker fixed zone, improving production adaptability and product yield, reducing modification costs, ensuring the optical and mechanical properties of the glass, and extending its service life.
Smart Images

Figure CN123106006A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of glass material processing technology, specifically relating to a gradient ultrathin glass based on surface pre-modification, its preparation method, and its application. Background Technology
[0002] As foldable screen devices evolve towards lighter weight, higher durability, and narrower bezels, the performance requirements for cover glass, as a core protective and display component, continue to upgrade. Currently, foldable screen cover glass has gone through two major technology stages: CPI and UTG. Among them, UTG has become the mainstream choice for more than 95% of foldable screen devices on the market due to its high light transmittance, strong wear resistance, and excellent flexibility.
[0003] UTG employs a uniform thickness structure across the entire glass pane, and its manufacturing process is relatively mature. Ultra-thinning is primarily achieved through HF chemical etching or overflow pull-down methods, followed by chemical strengthening and functional coating processes for mass production. However, UTG has inherent technical limitations: to meet the flexible bending requirements of the central bending zone, the entire glass pane needs to be made thin, resulting in insufficient rigidity in the side fixing areas and poor drop and impact resistance. Furthermore, repeated opening and closing of the bending zone can easily lead to micro-crack propagation and fatigue whitening, severely limiting the lifespan and market competitiveness of foldable screen devices.
[0004] To address the aforementioned pain points, the industry has proposed gradient ultra-thin glass (UFG, Ultra Fine Glass / Uneven-thickness Glass). Its core feature is that the central bending area is thin and the two side fixing areas are thick, with a smooth and gradual transition in thickness. This ensures both the extreme flexibility and long bending life of the bending area and improves the rigidity and impact resistance of the two side fixing areas, making it the next-generation core upgrade direction for foldable screen cover glass.
[0005] Currently, existing UFG manufacturing methods are mainly divided into two categories: one is the one-step forming method, which directly draws or rolls glass sheets with gradient thicknesses by precisely controlling the temperature field and melt flow rate of the melting furnace mold. This method has extremely high technical barriers and huge equipment investment (hundreds of millions to billions of yuan). Even small fluctuations in temperature and flow rate during the production process can lead to abnormal thickness gradients, making it difficult to control the yield above 60%. Only a few international giants (such as Corning and Schott) can achieve small-batch production, and the cost remains high, making it difficult to meet the mass production needs of domestic enterprises. The other is the back-end partitioned etching method, which modifies the existing HF etching tank and adds a partitioned spray system and gradient mask mechanism to perform differentiated etching on different areas of the glass to achieve thickness gradients. However, this method requires large-scale modification of the existing UTG etching production line, with a modification cycle of 3-6 months and high modification costs. It is also prone to defects such as mask erosion, edge steps, and uneven thickness transitions, which cause stress concentration in UFG products, making them prone to cracking when bent, further reducing product yield and reliability.
[0006] In addition, existing technologies also include solutions for local etching control through surface coating and protective adhesive coating. However, such solutions often use materials such as photoresist and oil-based resin, which are difficult to completely clean and remove after etching, leaving impurities. This not only contaminates the subsequent chemical strengthening salt bath, leading to glass strengthening failure and later spontaneous breakage, but also affects the subsequent functional coating process, resulting in a decline in the optical performance of the glass and failing to meet the high optical and mechanical requirements of foldable screen cover glass.
[0007] In summary, existing UFG preparation methods generally suffer from core defects such as large equipment investment, complex production line modification, high production costs, low product yield, and unstable performance. The industry urgently needs a UFG preparation method that can fully reuse existing UTG etching processes, has low modification costs, high yield, and stable product performance to solve industry pain points and promote the large-scale mass production and popularization of UFG. Summary of the Invention
[0008] The purpose of this invention is to provide a gradient ultrathin glass based on surface pre-modification and its preparation method. By performing regional pre-modification treatment on the surface of the ultrathin glass and controlling the etching rate of different regions, the glass forms a gradient thickness structure with bending regions, transition regions and fixed regions.
[0009] The present invention also aims to provide an application of gradient ultrathin glass based on surface pre-modification in foldable screen phones, smartwatches, automotive flexible screens and rollable screens.
[0010] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0011] This invention provides a method for preparing gradient ultrathin glass based on surface pre-modification, the method comprising the following steps:
[0012] 1) The original glass sheet is cleaned and dried to obtain a cleaned original glass sheet;
[0013] 2) The cleaned glass sheet is sprayed in sections and then dried to obtain the coated glass;
[0014] 3) Perform HF etching on the coated glass;
[0015] 4) The product from step 3) is subjected to a demolding process to obtain the gradient ultrathin glass based on surface pre-modification;
[0016] In step 2), the cleaned glass sheet is divided into at least two fixed areas and a bending area between the fixed areas along the center line. A transition area is provided between the fixed areas and the bending areas. The partitioned spraying refers to spraying an etching accelerator on the bending areas and an etching decelerator on the fixed areas.
[0017] In step 1), the thickness of the glass substrate is 100-200 μm, the surface roughness Ra≤0.1 nm, and the light transmittance≥92%.
[0018] According to a specific embodiment of the present invention, preferably, in step 1), the cleaning is one or more of ultrasonic cleaning or pure water rinsing.
[0019] In step 2), the etching accelerator is selected from any of the following:
[0020] A hydrochloric acid aqueous solution is formed by mixing concentrated hydrochloric acid and pure water in a volume ratio of 1:10 to 1:15.
[0021] Or a citric acid aqueous solution formed by mixing citric acid and pure water in a mass ratio of 1:20-1:30;
[0022] The etching accelerator has a pH value of 1.0-2.0.
[0023] In step 2), the etching decelerator is selected from any of the following:
[0024] A silane hydrophobic treatment solution is formed by mixing water-based silane hydrophobic agent stock solution and pure water at a volume ratio of 1:30-1:40;
[0025] Alternatively, it can be an aqueous solution of polyvinyl alcohol formed by mixing polyvinyl alcohol and pure water in a mass ratio of 1:50 to 1:60.
[0026] The aqueous silane hydrophobic agent is an octyltrimethoxysilane oligomer with a number-average molecular weight of 1500–2500 g / mol; the polyvinyl alcohol has a weight-average molecular weight of 31000–50000 g / mol.
[0027] In step 2), the transition zone is composed of at least one continuous sub-region divided along the direction from the bending zone to the fixing zone. Each sub-region is sprayed with a composite etching solution composed of etching accelerator and etching decelerator in different proportions. The volume ratio of etching accelerator to etching decelerator gradually transitions from a high proportion of etching accelerator to a low proportion of etching accelerator along the direction from the bending zone to the fixing zone. The volume ratio of etching accelerator to etching decelerator ranges from 1:1 to 5.
[0028] According to a specific embodiment of the present invention, preferably, in step 2), the drying temperature is 50-80°C.
[0029] The coating amount for the fixed zone, bending zone, and transition zone is 1-50 mg / cm³, calculated based on the solute of the etching decelerator and / or etching accelerator. 2 .
[0030] In step 3), the etching temperature of the HF etching process is 45-50℃, the etching time is 2000-3000s, and the HF acid mass concentration is 7wt%-10wt%.
[0031] In step 4), the stripping process refers to cleaning with pure water and alkaline solution, wherein the cleaning temperature is 35-45℃, the pure water cleaning time is 10-20s, the alkaline solution cleaning time is 10-20s, the pH of the alkaline solution is 10-12, and the alkali used is sodium hydroxide.
[0032] A gradient ultrathin glass based on surface pre-modification prepared by the above preparation method includes a bending region, a transition region and a fixing region; the thickness of the bending region is 30-40 μm, the thickness of the fixing region is 70-90 μm, and the width of the transition region is 4-6 mm.
[0033] Application of the aforementioned gradient ultrathin glass based on surface pre-modification in foldable screen phones, smartwatches, automotive flexible screens, or rollable screens.
[0034] Compared with the prior art, the present invention has the following advantages:
[0035] 1. This invention achieves regional thickness control of the glass by setting differentiated surface coatings in different functional areas of the original glass sheet, enabling different areas to have different HF etching response capabilities. Specifically, an etching accelerator is sprayed in the bending area to increase the number of active sites on the glass surface and promote the reaction between HF and the glass network structure; an etching decelerator is sprayed in the fixed area to form a surface protection effect and reduce the HF etching rate. Through the above control method, the thickness of the bending area in the prepared gradient ultrathin glass is 30-40 μm, and the thickness of the fixed area is 70-90 μm, realizing the differentiated design of thickness in different areas.
[0036] 2. The present invention sets a transition zone between the bending zone and the fixing zone, and sprays a composite etching control liquid with a gradually changing ratio of etching accelerator and etching decelerator along the direction from the bending zone to the fixing zone, so that the etching rate of the glass surface in the transition zone gradually changes, avoiding the formation of abrupt structures between regions of different thicknesses.
[0037] 3. This invention, by employing surface pre-modification combined with the overall HF etching process, enables different regions of the glass to achieve differentiated etching under the same etching conditions, eliminating the need for regional adjustments to the HF etching equipment parameters and improving the adaptability of the gradient ultrathin glass preparation process.
[0038] 4. This invention selects a removable surface pre-modified material as the etching control layer, and then uses pure water and alkaline solution for cleaning and demolding after etching, so that the surface pre-modified layer can be effectively removed, reducing the impact of residues on subsequent glass processing.
[0039] 5. The gradient ultrathin glass prepared by this invention has the structural characteristics of thin bending region and thick fixed region, and the bending performance and structural support performance are synergistically optimized by matching the thickness of different regions. Attached Figure Description
[0040] Figure 1 A schematic diagram of the pre-coating zones for the original glass sheet. Detailed Implementation
[0041] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0042] Unless otherwise specified, all test materials and reagents used in the following examples are commercially available.
[0043] Example 1
[0044] A method for preparing gradient ultrathin glass based on surface pre-modification specifically includes the following steps:
[0045] 1) Select an ultra-thin glass sheet with a thickness of 150μm, a surface roughness Ra of 0.08nm and a light transmittance of 93%. Use pure water to ultrasonically clean it for 15min to remove oil and impurities from the glass surface. Then dry it at 60℃ for 10min to obtain the cleaned glass sheet.
[0046] 2) Divide the cleaned glass sheet into two fixed areas and a bending area between the two fixed areas along the center line, and set a transition area between the fixed area and the bending area. The width of the middle bending area is 20mm. Spray an etching accelerator; the etching accelerator is a hydrochloric acid aqueous solution formed by mixing concentrated hydrochloric acid and pure water at a volume ratio of 1:12, with a pH value of 1.5.
[0047] The width of the fixed areas on both sides is 40mm, and an etching decelerator is sprayed on them. The etching decelerator is a silane hydrophobic treatment solution formed by mixing n-octyltrimethoxysilane oligomer and pure water at a volume ratio of 1:35. The number average molecular weight of the n-octyltrimethoxysilane oligomer is 2000g / mol.
[0048] The transition zone has a width of 5mm on one side and is divided into five continuous sub-regions along the direction from the bending zone to the fixing zone. Each sub-region is 1mm wide. Each sub-region is sprayed with a composite etching control liquid composed of etching accelerator and etching decelerator. The volume ratio of the etching accelerator to the etching decelerator gradually transitions from a higher accelerator ratio near the bending zone to a lower accelerator ratio near the fixing zone, with ratios of 1:1, 1:2, 1:3, 1:4 and 1:5, respectively.
[0049] The coating amount for each area is 20 mg / cm³, calculated based on the solute in the etching accelerator and / or etching decelerator. 2 After spraying, the glass is dried in a 60°C environment for 15 minutes to form a pre-modified coating on the surface.
[0050] 3) The coated glass substrate was subjected to HF etching at a temperature of 48°C, an HF acid concentration of 8 wt%, and an etching time of 2500 s.
[0051] 4) After etching, the glass is cleaned with pure water and sodium hydroxide alkaline solution. The pure water cleaning temperature is 40℃ and the cleaning time is 15s. Then, it is cleaned with sodium hydroxide solution with pH 11 for 15s. Finally, it is rinsed with pure water to obtain gradient ultrathin glass based on surface pre-modification.
[0052] The gradient ultrathin glass based on surface pre-modification prepared in this embodiment has a bending zone thickness of 35μm, a fixed zone thickness of 85μm on both sides, a transition zone width of 5mm, a smooth and gradual thickness change, and a thickness fluctuation of ±1.5μm; a light transmittance of 93%, a haze of 0.3%, and no residue, pitting, or microcracks on the surface; a bending radius of 0.4mm, and no fatigue whitening or microcracks after 1.2 million bending tests; a surface compressive stress of 950MPa on both fixed zones, and an impact strength of 320MPa.
[0053] Example 2
[0054] A method for preparing gradient ultrathin glass based on surface pre-modification specifically includes the following steps:
[0055] 1) Select an ultra-thin glass sheet with a thickness of 120μm, a surface roughness Ra of 0.07nm and a light transmittance of 94%. Use pure water to ultrasonically clean it for 12 minutes to remove oil and impurities from the glass surface. Then dry it at 65℃ for 8 minutes to obtain the cleaned glass sheet.
[0056] 2) Divide the cleaned glass sheet into two fixed areas and a bending area between the two fixed areas along the center line, and set a transition area between the fixed area and the bending area. The width of the middle bending area is 18mm. Spray an etching accelerator; the etching accelerator is a hydrochloric acid aqueous solution formed by mixing citric acid and pure water at a volume ratio of 1:25, with a pH value of 1.8.
[0057] The width of the fixed areas on both sides is 38mm, and an etching decelerator is sprayed on them. The etching decelerator is formed by mixing polyvinyl alcohol and pure water at a volume ratio of 1:55, and the weight average molecular weight of the polyvinyl alcohol is 40000g / mol.
[0058] The transition zone has a width of 4mm on one side and is divided into four continuous sub-regions along the direction from the bending zone to the fixed zone. Each sub-region is 1mm wide. Each sub-region is sprayed with a composite etching control liquid composed of etching accelerator and etching decelerator. The volume ratio of the etching accelerator to the etching decelerator gradually transitions from a higher accelerator ratio near the bending zone to a lower accelerator ratio near the fixed zone, with ratios of 1:1, 1:2, 1:3 and 1:4, respectively.
[0059] The coating amount for each area is 20 mg / cm³, calculated based on the solute in the etching accelerator and / or etching decelerator. 2 After spraying, the glass is dried in a 60°C environment for 15 minutes to form a pre-modified coating on the surface.
[0060] 3) The coated glass substrate was subjected to HF etching at a temperature of 48°C, an HF acid concentration of 8 wt%, and an etching time of 2500 s.
[0061] 4) After etching, the glass is cleaned with pure water and sodium hydroxide alkaline solution. The pure water cleaning temperature is 40℃ and the cleaning time is 15s. Then, it is cleaned with sodium hydroxide solution with pH 11 for 15s. Finally, it is rinsed with pure water to obtain gradient ultrathin glass based on surface pre-modification.
[0062] The gradient ultrathin glass based on surface pre-modification prepared in this embodiment has a bending zone thickness of 32μm, a fixed zone thickness of 78μm on both sides, and a transition zone thickness fluctuation of ±1.2μm; light transmittance of 94%, haze of 0.25%; bending radius of 0.35mm, bending life of 1.3 million cycles; surface compressive stress of 920MPa on both sides of the fixed zone, and impact strength of 310MPa.
[0063] Example 3
[0064] A method for preparing gradient ultrathin glass based on surface pre-modification specifically includes the following steps:
[0065] The difference between this embodiment and Embodiment 1 is that the etching accelerator is changed to concentrated hydrochloric acid and pure water diluted at a volume ratio of 1:10, pH=1.0; the etching decelerator is changed to be obtained by mixing n-octyltrimethoxysilane oligomer and pure water at a volume ratio of 1:30, and the rest is the same as in Embodiment 1.
[0066] The gradient ultrathin glass based on surface pre-modification prepared in this embodiment has a bending zone thickness of 33 μm, a fixed zone thickness of 88 μm on both sides, a transition zone width of 5 mm, a smooth and gradual thickness change, and a thickness fluctuation of ±1.6 μm; a light transmittance of 93%, a haze of 0.3%, and no residue, pitting, or microcracks on the surface; a bending radius of 0.4 mm, and no fatigue whitening or microcracks after 1.2 million bending tests; a surface compressive stress of 970 MPa on both fixed zones, and an impact strength of 325 MPa.
[0067] Comparative Example 1
[0068] A method for preparing gradient ultrathin glass by conventional UFG laser-assisted etching includes the following steps:
[0069] 1) Select an ultra-thin glass sheet with a thickness of 120μm, a surface roughness Ra of 0.07nm and a light transmittance of 94%. Use pure water to ultrasonically clean it for 12 minutes to remove oil and impurities from the glass surface. Then dry it at 65℃ for 8 minutes to obtain the cleaned glass sheet.
[0070] 2) Subsequently, the glass bending area was pretreated by laser-induced modification. The UFG glass was internally modified by a femtosecond laser with a wavelength of 1030 nm, a pulse width of 300 fs, a repetition frequency of 100 kHz, an average laser power of 220 mW, a scanning speed of 95 mm / s, and a Bezier beam with a focal depth of 200 μm.
[0071] 3) The glass substrate after laser pre-modification is immersed in hydrofluoric acid etching solution for wet etching. The etching solution is a 7% hydrofluoric acid aqueous solution, the etching temperature is 45 ℃, and the etching time is 35 min. After etching, the glass substrate is removed, washed with pure water and dried to obtain gradient ultrathin glass treated with laser-assisted etching.
[0072] The gradient ultrathin glass prepared in this comparative example, after conventional UFG laser-assisted etching, has a bending zone thickness of 33.5 μm, a fixed zone thickness of 78 μm on both sides, and a transition zone thickness fluctuation of ±2.8 μm; light transmittance of 93.7% and haze of 0.68%; a limiting bending radius of 0.52 mm and a reciprocating bending life of 610,000 cycles; a surface compressive stress of 835 MPa on both fixed zones and an impact strength of 246 MPa.
[0073] Comparative Example 2
[0074] A method for preparing ultrathin glass specifically includes the following steps:
[0075] The only difference between this comparative example and Example 1 is that step 2 in Example 1 is omitted.
[0076] The resulting ultrathin glass has a uniform overall thickness of 80μm, no partitioned structure, and a thickness fluctuation of ±2.1μm across the entire surface. It has a light transmittance of 93.4% and a haze of 0.57%. The bending radius is 1.0mm, the bending life is 360,000 cycles, the overall surface compressive stress is 760MPa, and the impact strength is 212MPa.
[0077] Test Example 1
[0078] The ultrathin glasses prepared in Examples 1-3 and Comparative Examples 1-2 were tested for thickness and thickness uniformity, optical properties, bending properties, surface compressive stress and impact resistance.
[0079] Thickness and thickness uniformity tests were conducted using a non-contact optical thickness gauge. Multiple test points were selected in the bending zone, transition zone, and fixed zone for thickness measurement. The maximum deviation of each test point in the transition zone from the fitted gradual thickness curve was used as the thickness fluctuation in the transition zone to evaluate the uniformity and continuity of thickness changes between different regions. For structures with uniform thinning across the entire surface, the thickness fluctuation at different locations on the board surface was tested.
[0080] Optical performance testing was conducted using a transmittance / haze meter to measure the visible light transmittance and haze of each sample. Before testing, the glass surface was cleaned, and the presence of residues, pitting, microcracks, or other surface defects was observed.
[0081] Bending performance testing was conducted using an ultra-thin glass reciprocating bending test device. The bending radius of the sample was gradually reduced, and the minimum bending radius at which the glass remained intact without breakage or obvious cracks was used as the bending radius evaluation index. Reciprocating bending cycles were performed under the corresponding bending conditions, and the number of cycles at which the sample developed cracks, fatigue whitening, or failure was used as the bending life evaluation index.
[0082] The surface compressive stress was tested using a glass surface stress tester. Multiple locations were selected on both sides of the fixed area for measurement and the average value was taken. For Comparative Example 2 without partition structure, test locations were selected evenly on the glass surface for measurement.
[0083] Impact resistance was assessed using specimens of the same specifications under identical test conditions. The impact strength was calculated based on the critical load at which the specimens failed. The test results are shown in Table 1 below.
[0084] Table 1
[0085]
[0086] The test results above show that the gradient ultrathin glasses based on surface pre-modification prepared in Examples 1-3 can all form a thinner bending zone and a thicker fixing zone, with a continuous thickness transition between the bending zone and the fixing zone. Among them, the thickness of the transition zone in Examples 1 and 3 is smooth and gradual, and no obvious surface residues, pitting, or microcracks were observed.
[0087] Compared to Comparative Example 1, which uses conventional UFG laser-assisted etching, Examples 1-3 show less thickness fluctuation in the transition region. This indicates that by performing differentiated surface pre-modification on different regions before HF etching, the connection between etching rates in different regions can be improved, resulting in a smoother thickness gradient between the bending region, transition region, and fixed region. Simultaneously, Examples 1-3 exhibit lower haze, indicating that the regionalized pre-modification and subsequent etching process did not significantly adversely affect the optical properties of the glass.
[0088] Regarding bending performance, the bending radii of Examples 1-3 were all smaller than those of Comparative Examples 1 and 2, while their reciprocating bending life was significantly higher than that of the two comparative examples. This may be because a thinner bending zone reduces the tensile strain on the outer surface of the glass during bending, while the continuous thickness variation in the transition zone alleviates stress concentration at the connection between the bending zone and the fixed zone, thereby reducing the likelihood of crack initiation and propagation during repeated bending.
[0089] Furthermore, while maintaining a small bending radius, Examples 1-3 still exhibit high surface compressive stress and impact resistance in their fixed areas. Compared to Comparative Example 2, which involves uniform thinning across the entire area, this invention only significantly thins the area bearing the main bending deformation, while maintaining a relatively large thickness in the fixed area. Therefore, it can balance the flexibility of the bending area with the mechanical support and impact resistance of the fixed area.
[0090] The above results indicate that by performing regional surface pre-modification on ultrathin glass and using etching accelerators, etching decelerators, and a composite etching solution in the transition zone to regulate the HF etching rate in different regions, a gradient thickness structure that continuously changes from the bending region to the fixed region can be formed. This approach maintains good light transmittance while reducing the bending radius, improving cyclic bending durability, and maintaining the mechanical strength of the fixed region.
[0091] It should be noted that the above embodiments are merely some preferred embodiments of the present invention, and not all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0092] The above description of the embodiments is intended to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a gradient ultrathin glass based on surface pre-modification, characterized in that, The preparation method includes the following steps: 1) The original glass sheet is cleaned and dried to obtain a cleaned original glass sheet; 2) The cleaned glass sheet is sprayed in sections and then dried to obtain the coated glass; 3) Perform HF etching on the coated glass; 4) The product from step 3) is subjected to a demolding process to obtain the gradient ultrathin glass based on surface pre-modification; In step 2), the cleaned glass sheet is divided into at least two fixed areas and a bending area between the fixed areas along the center line. A transition area is provided between the fixed areas and the bending areas. The partitioned spraying refers to spraying an etching accelerator on the bending areas and an etching decelerator on the fixed areas.
2. The production method according to claim 1, characterized by, In step 1), the thickness of the glass substrate is 100-200 μm, the surface roughness Ra≤0.1 nm, and the light transmittance≥92%.
3. The preparation method according to claim 1, characterized in that, In step 2), the etching accelerator is selected from any of the following: A hydrochloric acid aqueous solution is formed by mixing concentrated hydrochloric acid and pure water in a volume ratio of 1:10 to 1:
15. Or a citric acid aqueous solution formed by mixing citric acid and pure water in a mass ratio of 1:20-1:30; The etching accelerator has a pH value of 1.0-2.
0.
4. The method of claim 1, wherein, In step 2), the etching decelerator is selected from any of the following: A silane hydrophobic treatment solution is formed by mixing water-based silane hydrophobic agent stock solution and pure water at a volume ratio of 1:30-1:40; Alternatively, it can be an aqueous solution of polyvinyl alcohol formed by mixing polyvinyl alcohol and pure water in a mass ratio of 1:50 to 1:
60. The aqueous silane hydrophobic agent is an octyltrimethoxysilane oligomer with a number-average molecular weight of 1500–2500 g / mol; the polyvinyl alcohol has a weight-average molecular weight of 31000–50000 g / mol.
5. The preparation method according to claim 1, characterized in that, In step 2), the transition zone is composed of at least one continuous sub-region divided along the direction from the bending zone to the fixing zone. Each sub-region is sprayed with a composite etching solution composed of etching accelerator and etching decelerator in different proportions. The volume ratio of etching accelerator to etching decelerator gradually transitions from a high proportion of etching accelerator to a low proportion of etching accelerator along the direction from the bending zone to the fixing zone. The volume ratio of etching accelerator to etching decelerator ranges from 1:1 to 10.
6. The method of claim 1, wherein, The spray amount of the fixed area, the bending area and the transition area is 1-50 mg / cm calculated from the etching decelerator and / or etching accelerator solute 2 .
7. The preparation method according to claim 1, characterized in that, In step 3), the etching temperature of the HF etching process is 45-50℃, the etching time is 2000-3000s, and the HF acid mass concentration is 7wt%-10wt%.
8. The preparation method according to claim 1, characterized in that, In step 4), the stripping process refers to cleaning with pure water and alkaline solution, wherein the cleaning temperature is 35-45℃, the pure water cleaning time is 10-20s, the alkaline solution cleaning time is 10-20s, the pH of the alkaline solution is 10-12, and the alkali used is sodium hydroxide.
9. A gradient ultrathin glass based on surface pre-modification prepared by the preparation method according to any one of claims 1-8, characterized in that, It includes a bending zone, a transition zone, and a fixing zone; the thickness of the bending zone is 30-40μm, the thickness of the fixing zone is 70-90μm, and the width of the transition zone is 4-6mm.
10. The application of a surface-premodified gradient ultrathin glass as described in claim 9 in foldable screen phones, smartwatches, automotive flexible screens, or rollable screens.