A coated photovoltaic glass and its preparation method
By constructing a composite coating of acrylic resin and modified silicone resin on the surface of photovoltaic glass, the problem of balancing high light transmittance with impact resistance and flame retardancy is solved, thereby improving the mechanical strength and fire safety of the glass.
Patent Information
- Application Number
- CN202611272117.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photovoltaic glass struggles to balance high light transmittance with impact resistance and flame retardancy. Furthermore, organic coatings are flammable and pose a fire hazard, while traditional inorganic flame retardants reduce light transmittance.
A coating composed of acrylic resin, acrylic-modified silicone resin and composite additives is used to construct a high light transmittance, high hardness and flame retardancy composite coating on the surface of photovoltaic glass through photoinitiated curing technology. The composite additive is prepared by reacting phosphorus oxychloride, hydroxyethyl acrylate and pentaerythritol tetra-3-mercaptopropionate.
It achieves improved hardness and flame retardancy of coating under high light transmittance, avoiding the problems of reduced light transmittance and flammability of coating caused by traditional additives, and enhancing the mechanical strength and fire safety of photovoltaic glass.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic glass technology, specifically to a coated photovoltaic glass and its preparation method. Background Technology
[0002] Photovoltaic glass is the core encapsulation material for solar cell modules, primarily used for physical protection and sealing of photovoltaic cells to ensure long-term stable operation of the modules under complex outdoor climatic conditions. Since solar cell modules typically need to meet outdoor service life requirements of over 25 years, photovoltaic glass, as the outermost protective medium, not only needs to possess extremely high and stable solar transmittance to minimize light refraction and absorption losses and improve the photoelectric conversion efficiency of the cells, but also must have good weather resistance, mechanical strength, and surface chemical stability to resist external ultraviolet radiation, wind and rain erosion, and the adhesion of pollutants.
[0003] However, existing photovoltaic glass still has significant limitations in its impact resistance and flame retardant safety performance when facing increasingly harsh real-world application environments. On the one hand, when subjected to hail, sandstorms, or mechanical stress impacts during installation and maintenance, traditional photovoltaic glass and its surface functional coatings are prone to micro-cracks or localized peeling, leading to a decrease in the coating's mechanical protective strength and even causing glass breakage and module encapsulation failure. On the other hand, the organic protective coatings designed to improve weather resistance or anti-reflective properties are mostly based on flammable resins. When faced with localized hot spot effects in photovoltaic modules, aging wiring, or high-temperature ignition sources induced by electrical short circuits, the coatings are easily ignited and accelerate the spread of fire, posing a significant fire hazard. Simply adding large-particle inorganic flame retardants to improve flame retardancy will significantly reduce the coating's light transmittance due to scattering of solid-phase impurities, making it difficult to effectively balance high light transmittance, strong impact resistance, and high flame retardant performance. Therefore, how to develop a photovoltaic glass that maintains high light transmittance while also possessing excellent impact resistance and flame retardant protection is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a coated photovoltaic glass and a method for its preparation.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A coated photovoltaic glass includes a photovoltaic glass substrate and a coating applied to the surface of the photovoltaic glass substrate. The coating is formed by coating and curing a coating liquid containing the following components in parts by weight: 40-60 parts of acrylic resin, 5-10 parts of acrylic modified silicone resin, 3-6 parts of composite additives, 0.5-1 part of leveling agent, 1-2 parts of photoinitiator, and 20-40 parts of ethyl acetate.
[0006] In the technical solution disclosed in this invention, acrylic resin is used as the film-forming matrix of the coating, providing the most basic physical and mechanical properties of the coating and its adhesion to the glass substrate. The amount of acrylic resin can be selected from 40 parts, 42 parts, 45 parts, 46 parts, 48 parts, 50 parts, 52 parts, 54 parts, 55 parts, 58 parts, and 60 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0007] In the technical solution disclosed in this invention, the siloxane backbone in the acrylic-modified silicone resin can improve the heat resistance and UV aging resistance of the coating. The amount of acrylic-modified silicone resin can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, or 10 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0008] In the technical solution disclosed in this invention, the preparation method of the composite additive is as follows: S1. Add phosphorus oxychloride to anhydrous dichloromethane and stir until homogeneous to obtain a phosphorus oxychloride solution; add hydroxyethyl acrylate, triethylamine, and p-methoxyphenol to anhydrous dichloromethane and mix until homogeneous to obtain a mixture; add the mixture dropwise to the phosphorus oxychloride solution at 0-5℃. After the addition is complete, allow the system to naturally rise to room temperature and stir the reaction. After the reaction is complete, filter, wash, dry, and remove the solvent by vacuum distillation to obtain a viscous liquid product. S2. Under a nitrogen atmosphere, pentaerythritol tetra-3-mercaptopropionate and azobisisobutyronitrile are added to the viscous liquid product, and the mixture is heated to react. After the reaction is completed, the mixture is cooled to room temperature to obtain the composite additive.
[0009] Specifically, in step S1, the molar ratio of phosphorus oxychloride, hydroxyethyl acrylate, triethylamine, and p-methoxyphenol is 0.1:0.30-0.35:0.30-0.35:0.001-0.003.
[0010] Specifically, in step S1, the stirring reaction time is 6-8 hours.
[0011] Specifically, in step S2, the mass ratio of the viscous liquid product, pentaerythritol tetra-3-mercaptopropionate, and azobisisobutyronitrile is 10:0.5-2:0.02-0.05.
[0012] Specifically, in step S2, the temperature of the heating reaction is 55-65℃, and the heating reaction time is 3-5 hours.
[0013] In the technical solution disclosed in this invention, the leveling agent can reduce the surface tension of the coating solution and improve the wetting and spreading ability of the coating on the photovoltaic glass substrate. The amount of leveling agent can be selected from 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, and 1 part, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0014] Preferably, the leveling agent is selected from polyester-modified silicone leveling agents or polyether-modified silicone leveling agents, such as BYK-370, BYK-378 or BYK-UV-3510.
[0015] In the technical solution disclosed in this invention, the photoinitiator absorbs light energy and decomposes under ultraviolet light to generate free radicals, which initiate free radical polymerization and crosslinking of the residual double bonds in the acrylic resin, acrylic-modified silicone resin, and composite additives. The amount of photoinitiator can be selected from 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, and 2 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0016] Preferably, the photoinitiator is selected from photoinitiator 1173 or photoinitiator 184.
[0017] In the technical solution disclosed in this invention, ethyl acetate is used as a diluent solvent to reduce the viscosity of the coating solution system, giving it good flowability and coating processability. The amount of ethyl acetate can be selected from 20 parts, 22 parts, 24 parts, 25 parts, 28 parts, 30 parts, 32 parts, 34 parts, 35 parts, 36 parts, 38 parts, and 40 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0018] The present invention also provides a method for preparing the above-mentioned coated photovoltaic glass, comprising the following steps: mixing acrylic resin, acrylic modified silicone resin, composite additive, leveling agent, photoinitiator and ethyl acetate evenly to obtain a coating solution; then coating the coating solution on one side of the photovoltaic glass substrate, drying it and curing it with ultraviolet light to obtain the coated photovoltaic glass.
[0019] Preferably, the coating amount of the coating solution on one side is 15-30 g / m². 2 .
[0020] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention constructs a composite coating on the surface of photovoltaic glass by compounding an acrylic resin matrix, an acrylic-modified silicone resin, and a phosphorus-sulfur composite additive, and then using photo-initiated curing technology. This coating possesses high light transmittance, high pencil hardness, flame retardancy, and impact resistance. This invention overcomes the problem that traditional inorganic additive flame retardants easily cause light scattering and reduce light transmittance in the coating, while avoiding the defects of physical additive organic flame retardants that easily migrate and reduce coating hardness and adhesion. Under the premise of ensuring that the photovoltaic glass maintains high solar transmittance, it achieves a synergistic improvement in coating surface hardness and flame retardancy.
[0021] (2) The composite additive used in this invention is prepared by a two-step reaction of phosphorus oxychloride, hydroxyethyl acrylate and pentaerythritol tetra-3-mercaptopropionate. Its structure contains phosphate ester flame-retardant functional groups, flexible sulfide bonds and carbon-carbon double bonds that can participate in the photocuring reaction. During the ultraviolet curing process, the composite additive enters the cross-linking network of the resin matrix through double bond bonding, forming a homogeneous and dense network structure. Among them, the phosphate ester structure promotes charring on the coating surface when heated, playing a condensed phase flame-retardant role; the multifunctional cross-linking nodes significantly improve the micro-cross-linking density and pencil hardness of the coating after curing; the flexible sulfide segments in pentaerythritol tetra-3-mercaptopropionate can release the internal stress of the coating, significantly improving the impact toughness of the coating. Furthermore, since the composite additive is a chemically modified liquid component, there is no problem of solid particle scattering, maintaining the high light transmittance of the coating. Detailed Implementation
[0022] The present invention will be further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0023] It should be noted that, unless otherwise specified, all chemical reagents involved in this invention were purchased through commercial channels.
[0024] The acrylic resin used in this embodiment of the invention is AC8003, which is sourced from Guangzhou Qiyuan New Materials Co., Ltd. The acrylic-modified silicone resin is designated JP-R03 and is sourced from Shanghai Kaiyin Chemical Co., Ltd.
[0025] Example 1 A method for preparing coated photovoltaic glass includes the following steps: 50 parts acrylic resin, 8 parts acrylic modified silicone resin, 5 parts composite additive, 0.8 parts leveling agent BYK-UV-3510, 1.5 parts photoinitiator 1173, and 30 parts ethyl acetate were added to a mixing device and stirred at 400 r / min for 30 min to obtain a coating solution. The coating solution was then applied to one side of a photovoltaic glass substrate, with a single-sided coating amount of 20 g / m².2 The glass is dried at 70°C and then cured by irradiation with a high-pressure mercury lamp (with main emission wavelengths including 254nm, 313nm, and 365nm) for 60 seconds to obtain coated photovoltaic glass.
[0026] The preparation method of the composite additive is as follows: S1. Add 0.05 mol of phosphorus oxychloride to 50 mL of anhydrous dichloromethane and stir until homogeneous to obtain a phosphorus oxychloride solution. Add 0.15 mol of hydroxyethyl acrylate, 0.15 mol of triethylamine, and 0.001 mol of p-methoxyphenol to 50 mL of anhydrous dichloromethane and mix until homogeneous to obtain a mixture. At 0 °C, add the mixture dropwise to the phosphorus oxychloride solution. After the addition is complete, allow the system to naturally rise to room temperature and stir for 6 h. After the reaction is complete, filter to remove the solid salt. Wash the filtrate with water, dry it with anhydrous sodium sulfate, and then remove the solvent by vacuum distillation to obtain a viscous liquid product. S2. Under a nitrogen atmosphere, add 1g pentaerythritol tetra-3-mercaptopropionate and 0.03g azobisisobutyronitrile to 10g of viscous liquid product, heat at 60℃ for 4h, and after the reaction is completed, cool to room temperature to obtain the composite additive.
[0027] Example 2 A method for preparing coated photovoltaic glass includes the following steps: 40 parts acrylic resin, 5 parts acrylic-modified silicone resin, 3 parts composite additive, 0.5 parts leveling agent BYK-UV-3510, 1 part photoinitiator 1173, and 20 parts ethyl acetate were added to a mixing device and stirred at 400 rpm for 30 minutes to obtain a coating solution. The coating solution was then applied to one side of a photovoltaic glass substrate, with a single-sided coating amount of 15 g / m². 2 The glass is dried at 70°C and then cured by irradiation with a high-pressure mercury lamp (with main emission wavelengths including 254nm, 313nm, and 365nm) for 60 seconds to obtain coated photovoltaic glass.
[0028] The preparation method of the composite additive is as follows: S1. Add 0.05 mol of phosphorus oxychloride to 50 mL of anhydrous dichloromethane and stir until homogeneous to obtain a phosphorus oxychloride solution. Add 0.15 mol of hydroxyethyl acrylate, 0.15 mol of triethylamine, and 0.001 mol of p-methoxyphenol to 50 mL of anhydrous dichloromethane and mix until homogeneous to obtain a mixture. At 0 °C, add the mixture dropwise to the phosphorus oxychloride solution. After the addition is complete, allow the system to naturally rise to room temperature and stir for 6 h. After the reaction is complete, filter to remove the solid salt. Wash the filtrate with water, dry it with anhydrous sodium sulfate, and then remove the solvent by vacuum distillation to obtain a viscous liquid product. S2. Under a nitrogen atmosphere, add 0.5g pentaerythritol tetra-3-mercaptopropionate and 0.02g azobisisobutyronitrile to 10g of viscous liquid product, heat at 60℃ for 4h, and after the reaction is completed, cool to room temperature to obtain the composite additive.
[0029] Example 3 A method for preparing coated photovoltaic glass includes the following steps: 60 parts acrylic resin, 10 parts acrylic-modified silicone resin, 6 parts composite additive, 1 part leveling agent BYK-UV-3510, 2 parts photoinitiator 1173, and 40 parts ethyl acetate were added to a mixing device and stirred at 400 rpm for 30 minutes to obtain a coating solution. The coating solution was then applied to one side of a photovoltaic glass substrate, with a single-sided coating amount of 30 g / m². 2 The glass is dried at 70°C and then cured by irradiation with a high-pressure mercury lamp (with main emission wavelengths including 254nm, 313nm, and 365nm) for 60 seconds to obtain coated photovoltaic glass.
[0030] The preparation method of the composite additive is as follows: S1. Add 0.05 mol of phosphorus oxychloride to 50 mL of anhydrous dichloromethane and stir until homogeneous to obtain a phosphorus oxychloride solution. Add 0.15 mol of hydroxyethyl acrylate, 0.15 mol of triethylamine, and 0.001 mol of p-methoxyphenol to 50 mL of anhydrous dichloromethane and mix until homogeneous to obtain a mixture. At 0 °C, add the mixture dropwise to the phosphorus oxychloride solution. After the addition is complete, allow the system to naturally rise to room temperature and stir for 6 h. After the reaction is complete, filter to remove the solid salt. Wash the filtrate with water, dry it with anhydrous sodium sulfate, and then remove the solvent by vacuum distillation to obtain a viscous liquid product. S2. Under a nitrogen atmosphere, add 2g of pentaerythritol tetra-3-mercaptopropionate and 0.05g of azobisisobutyronitrile to 10g of viscous liquid product, heat at 60℃ for 4h, and after the reaction is completed, cool to room temperature to obtain the composite additive.
[0031] Comparative Example 1 A method for preparing coated photovoltaic glass includes the following steps: 50 parts acrylic resin, 8 parts acrylic-modified silicone resin, 0.8 parts leveling agent BYK-UV-3510, 1.5 parts photoinitiator 1173, and 30 parts ethyl acetate were added to a mixing device and stirred at 400 rpm for 30 minutes to obtain a coating solution. The coating solution was then applied to one side of a photovoltaic glass substrate, with a single-sided coating amount of 20 g / m². 2The glass is dried at 70°C and then cured by irradiation with a high-pressure mercury lamp (with main emission wavelengths including 254nm, 313nm, and 365nm) for 60 seconds to obtain coated photovoltaic glass.
[0032] Compared with Comparative Example 1, no compound additives were added.
[0033] Comparative Example 2 A method for preparing coated photovoltaic glass includes the following steps: 50 parts acrylic resin, 8 parts acrylic modified silicone resin, 5 parts composite additive, 0.8 parts leveling agent BYK-UV-3510, 1.5 parts photoinitiator 1173, and 30 parts ethyl acetate were added to a mixing device and stirred at 400 r / min for 30 min to obtain a coating solution. The coating solution was then applied to one side of a photovoltaic glass substrate, with a single-sided coating amount of 20 g / m². 2 The glass is dried at 70°C and then cured by irradiation with a high-pressure mercury lamp (with main emission wavelengths including 254nm, 313nm, and 365nm) for 60 seconds to obtain coated photovoltaic glass.
[0034] The preparation method of the composite additive is as follows: 0.05 mol of phosphorus oxychloride was added to 50 mL of anhydrous dichloromethane and stirred until homogeneous to obtain a phosphorus oxychloride solution. 0.15 mol of hydroxyethyl acrylate, 0.15 mol of triethylamine, and 0.001 mol of p-methoxyphenol were added to 50 mL of anhydrous dichloromethane and mixed until homogeneous to obtain a mixture. At 0 °C, the mixture was added dropwise to the phosphorus oxychloride solution. After the addition was complete, the system was allowed to naturally rise to room temperature, and the reaction was stirred for 6 hours. After the reaction was complete, the solid salt was removed by filtration. The filtrate was washed with water, dried over anhydrous sodium sulfate, and then the solvent was removed by vacuum distillation to obtain the composite additive.
[0035] Compared with Example 1, the composite additive did not contain grafted pentaerythritol tetra-3-mercaptopropionate.
[0036] The performance of the coated photovoltaic glasses prepared in Examples 1-3 and Comparative Examples 1-2 of the present invention was tested, as follows: Oxygen index: The oxygen index was tested in accordance with GB / T 2406.2-2009; Light transmittance: The average light transmittance of the coated photovoltaic glass in the wavelength range of 380-1100 nm was measured using a UV-3600 spectrophotometer. Pencil hardness: The hardness of the coated pencil was tested according to the method disclosed in ASTM D 3363-05 (R2011); Impact resistance test: Steel ball impact test (227g steel ball dropped freely from a height of 1m) Post-impact condition: No cracks or damage.
[0037] The test results are shown in Table 1.
[0038] Table 1 Performance test results for different groups As can be seen from the table, Comparative Example 1, which did not add composite additives, had significantly lower flame retardant and impact resistance than Example 1 of the present invention. Comparative Example 2, which did not have pentaerythritol tetra-3-mercaptopropionate grafted into its composite additives, had reduced light transmittance. This was because the ungrafted phosphate ester product had high polarity and poor compatibility with the acrylic resin system, resulting in microphase separation and a decrease in light transmittance. After grafting modification with pentaerythritol tetra-3-mercaptopropionate, the molecular polarity decreased, the compatibility with the resin matrix improved, microphase separation was eliminated, and the light transmittance recovered to 93%.
[0039] Finally, it should be noted that the above embodiments do not limit the present invention in any way. Those skilled in the art can make modifications and improvements based on the present invention. Therefore, any modifications or improvements made without departing from the spirit of the present invention are within the scope of protection claimed by the present invention.
Claims
1. A coated photovoltaic glass, comprising a photovoltaic glass substrate and a coating applied to the surface of the photovoltaic glass substrate, characterized in that, The coating is formed by coating and curing a coating solution containing the following components in parts by weight: 40-60 parts acrylic resin, 5-10 parts acrylic modified silicone resin, 3-6 parts composite additive, 0.5-1 part leveling agent, 1-2 parts photoinitiator, and 20-40 parts ethyl acetate.
2. The coated photovoltaic glass according to claim 1, characterized in that, The preparation method of the composite additive is as follows: S1. Add phosphorus oxychloride to anhydrous dichloromethane and stir until homogeneous to obtain a phosphorus oxychloride solution; add hydroxyethyl acrylate, triethylamine, and p-methoxyphenol to anhydrous dichloromethane and mix until homogeneous to obtain a mixture; add the mixture dropwise to the phosphorus oxychloride solution at 0-5℃. After the addition is complete, allow the system to naturally rise to room temperature and stir the reaction. After the reaction is complete, filter, wash, dry, and remove the solvent by vacuum distillation to obtain a viscous liquid product. S2. Under a nitrogen atmosphere, pentaerythritol tetra-3-mercaptopropionate and azobisisobutyronitrile are added to the viscous liquid product, and the mixture is heated to react. After the reaction is completed, the mixture is cooled to room temperature to obtain the composite additive.
3. The coated photovoltaic glass according to claim 2, characterized in that, In step S1, the molar ratio of phosphorus oxychloride, hydroxyethyl acrylate, triethylamine and p-methoxyphenol is 0.1:0.30-0.35:0.30-0.35:0.001-0.
003.
4. The coated photovoltaic glass according to claim 2, characterized in that, In step S1, the stirring reaction time is 6-8 hours.
5. The coated photovoltaic glass according to claim 2, characterized in that, In step S2, the mass ratio of the viscous liquid product, pentaerythritol tetra-3-mercaptopropionate, and azobisisobutyronitrile is 10:0.5-2:0.02-0.
05.
6. The coated photovoltaic glass according to claim 2, characterized in that, In step S2, the temperature of the heating reaction is 55-65℃, and the heating reaction time is 3-5h.
7. The coated photovoltaic glass according to claim 1, characterized in that, The leveling agent is selected from polyester-modified silicone leveling agents or polyether-modified silicone leveling agents.
8. The coated photovoltaic glass according to claim 1, characterized in that, The photoinitiator is selected from photoinitiator 1173 or photoinitiator 184.
9. The method for preparing coated photovoltaic glass according to any one of claims 1-8, characterized in that, The process includes the following steps: mixing acrylic resin, acrylic-modified silicone resin, composite additives, leveling agents, photoinitiators, and ethyl acetate evenly to obtain a coating solution; then coating the coating solution onto one side of the photovoltaic glass substrate, drying it, and curing it with ultraviolet light to obtain coated photovoltaic glass.