A method for prehydration treatment of steel slag and a method for preparing steel slag-based aerogel composite materials.

By pre-hydrating steel slag and performing directional freeze-drying, a steel slag-based aerogel composite material with high compressive strength, low thermal conductivity, and good sound absorption properties was prepared, solving the multifunctional requirements of building insulation materials and the problem of high-value utilization of steel slag.

CN123106027APending Publication Date: 2026-11-17SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611436909.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing building insulation materials suffer from problems such as limited functionality, poor fire resistance, or insufficient mechanical strength. Furthermore, steel slag has a low comprehensive utilization rate, occupies space when stored, and poses a risk of heavy metal leakage, making it difficult to achieve the integration of heat insulation, sound absorption, and load-bearing capacity.

Method used

By pre-hydrating steel slag to generate CSH gel and calcium hydroxide hydration products on its surface, the interfacial bonding between the organic and inorganic phases is enhanced. The slag is then compounded with a polyvinyl alcohol solution and combined with a directional freeze-drying process to prepare a steel slag-based aerogel composite material.

Benefits of technology

The prepared aerogel material has high compressive strength, low thermal conductivity and good sound absorption performance, realizing the transformation of steel slag into a high-value functional material. It has the characteristics of integrated load-bearing, heat insulation and sound absorption, and is suitable for building insulation and industrial kiln insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106027A_ABST
    Figure CN123106027A_ABST
Patent Text Reader

Abstract

This invention discloses a method for pre-hydrating steel slag and a method for preparing steel slag-based aerogel composite materials. The pre-hydration method involves mixing steel slag powder with water and stirring at 20-60℃ for 1-4 hours to pre-hydrate it. The pre-hydrated product is then dried to obtain pre-hydrated steel slag powder. This pre-hydrated steel slag powder is mixed with a PVA solution to obtain a composite slurry, which is then directionally frozen using an ice template method. The product is then freeze-dried to obtain the aerogel composite material. This invention improves the interfacial compatibility between steel slag and the organic polymer network by surface activation during pre-hydration. The aerogel composite material exhibits a compressive strength exceeding 128 MPa (90% strain), a thermal conductivity as low as 0.329 W / (m·K), and a peak sound absorption coefficient of 0.74 in the frequency range of 175-6300 Hz, thus transforming steel slag from a "low-value filler material" into a "high-performance functional material."
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for treating solid waste and a method for preparing aerogel, and more particularly to a method for treating steel slag and a method for preparing steel slag-based aerogel composite materials. Background Technology

[0002] Currently, building-wide energy consumption accounts for a significant proportion of total societal energy consumption, with heat loss from the building envelope being a major contributing factor. Current energy-saving standards are continuously tightening requirements for wall heat transfer coefficients, but traditional insulation materials generally suffer from limitations such as single functionality, poor fire resistance, or insufficient mechanical strength. Organic insulation boards like EPS and XPS have low limiting oxygen indices, and their burning droplets can easily ignite secondary fires; rock wool and glass wool have good sound absorption properties, but their tensile and compressive strengths are extremely low, making them unsuitable for load-bearing components; while lightweight concrete combines fire resistance and lightweight properties, its strength and thermal conductivity are inversely related, with strength often falling below 1 MPa at low densities, making it difficult to meet engineering load-bearing requirements.

[0003] Steel slag is a major solid waste generated by the steel industry, with an annual production exceeding 130 million tons. The comprehensive utilization rate is approximately 30%, and the cumulative stockpile exceeds 1.8 billion tons, posing a land occupation risk and the risk of heavy metal leakage. The main oxide composition of steel slag belongs to the CaO-SiO2-Al2O3-Fe2O3 system, similar to silicate cement, containing potentially active minerals such as tricalcium silicate (C3S) and dicalcium silicate (C2S). However, it has higher iron and magnesium content and contains RO phases and phases uncommon in cement, such as free calcium oxide and free magnesium oxide, providing a chemical basis for its role as a cementitious framework. However, the hydration volume expansion rates of free calcium oxide and free magnesium oxide in steel slag reach 98% and 148%, respectively, leading to substandard volume stability in traditional steel slag building materials. Furthermore, its surface multiphase composition is chemically heterogeneous, resulting in severe debonding at the interface with organic polymers, limiting its application in high-performance composite materials.

[0004] Promoting the transformation of steel slag from "low-value filler" to "high-value functional material" and developing integrated green building materials with heat insulation, sound absorption and load-bearing capacity are common needs in the current construction industry for energy conservation, emission reduction and solid waste resource utilization. Summary of the Invention

[0005] Purpose of the invention: The purpose of this invention is to provide a method for prehydrating steel slag that can enhance the interfacial bonding and cross-linking between the organic and inorganic phases;

[0006] Another objective of this invention is to provide a method for preparing a steel slag-based aerogel composite material that integrates load-bearing, heat insulation, and sound absorption.

[0007] Technical solution: The prehydration treatment method for steel slag described in this invention involves mixing steel slag powder with water and stirring at a temperature of 20~60℃ for 1~4 hours to carry out prehydration; drying the prehydrated product and sieving it to obtain prehydrated steel slag powder.

[0008] The mass ratio of steel slag powder to water is 1:(1.5~2.5), that is, the liquid-solid ratio is (1.5~2.5):1.

[0009] The preferred temperature range is 20~60℃, excluding 20℃ and 60℃; the prehydration time is 1~4h, excluding 1h. More preferably, prehydration is carried out at 40℃.

[0010] The stirring speed is 200~300 rpm.

[0011] The specific process of the pre-hydration treatment is as follows: steel slag powder is mixed with water and stirred in a constant temperature water bath at 20~60℃ for 1~4 hours to carry out pre-hydration, so that a hydration product layer containing calcium silicate gel and calcium hydroxide is generated in situ on the surface of the steel slag particles; after the pre-hydration is completed, the wet steel slag is dried to a moisture content of no more than 0.2%, sieved, and pre-hydrated steel slag powder is obtained.

[0012] The preparation method of the above-mentioned steel slag-based aerogel composite material includes the following steps:

[0013] (1) The prehydrated steel slag powder prepared by the above method is mixed and stirred with polyvinyl alcohol solution to obtain a composite slurry;

[0014] (2) Pour the composite slurry into a mold and use the ice template method for directional freezing;

[0015] (3) The product obtained by directional freezing is freeze-dried to obtain a steel slag-based aerogel composite material.

[0016] In step (1), the mass ratio of the prehydrated steel slag powder to the polyvinyl alcohol solution is (0.8~1.2):1.

[0017] In step (1), the mass fraction of the polyvinyl alcohol solution is 8-12%.

[0018] In step (1), the stirring speed is 300~500 rpm and the stirring time is 4~6 min.

[0019] In step (2), the directional freezing time is 20 to 30 minutes.

[0020] In step (3), the drying vacuum degree is 4~10 Pa and the total drying time is 2~4 days.

[0021] In step (2), the bottom of the mold is a 5 mm thick brass plate, and the sides are made of 5 mm thick polytetrafluoroethylene.

[0022] Invention Principle: Common steel slag prehydration treatments primarily aim to consume free calcium oxide and magnesium oxide in steel slag, reducing the risk of expansion during subsequent hydration of cement-based materials. However, the prehydration method in this application, besides reducing the volume stability risks of steel slag, more importantly generates hydration products such as CSH gel and calcium hydroxide on the steel slag surface, increasing surface hydroxyl groups and calcium ions as active sites. This leads to more hydrogen bonding and ion coordination with PVA molecular chains, enhancing the interfacial bonding and cross-linking between the organic and inorganic phases. Under the prehydration conditions of this application, steel slag is premixed with water to form a certain amount of hydration products, which are then dried to produce steel slag powder. This powder is then compounded with an organic polymer and pore-forming is performed to prepare an aerogel. This "prehydration-drying" pretreatment pre-dissolves free calcium oxide and magnesium oxide, eliminating their expansion risks and reducing the volume stability risks caused by subsequent hydration expansion. Furthermore, this invention does not use any chemical cross-linking materials.

[0023] Specifically, this invention pre-hydrates steel slag, preferentially converting free calcium oxide and magnesium oxide on its surface into calcium hydroxide and magnesium hydroxide, significantly reducing the risk of volume expansion. Simultaneously, the CSH gel and calcium hydroxide generated during pre-hydration form a functionalized shell rich in hydroxyl groups and calcium ions on the particle surface, improving surface chemical uniformity. Based on this, the pre-hydrated steel slag is composited with a polyvinyl alcohol (PVA) solution. The hydroxyl groups on the PVA molecular chains form a hydrogen bond network with the hydroxyl groups on the steel slag surface and coordinate with calcium ions in the shell, constructing an organic-inorganic three-dimensional interface coupling network. This structure retains the high rigidity of the steel slag skeleton while introducing the toughness of the PVA network, achieving efficient stress transfer and energy dissipation.

[0024] Subsequently, a directional freezing process was employed, utilizing a temperature gradient to induce the directional growth of ice crystals, displacing the solid components into the interstices of the ice crystals to form a layered porous structure. After freeze-drying, the ice crystals sublimate, yielding a high-porosity aerogel. The low thermal conductivity of air and the complex heat conduction paths within the high porosity result in a low thermal conductivity coefficient for the material; the porous structure induces viscous loss and structural scattering of sound waves, enhancing the material's sound absorption performance; and the inorganic-organic three-dimensional interwoven framework ensures that the material maintains sufficient load-bearing capacity under lightweight and porous conditions.

[0025] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects:

[0026] (1) By combining the prehydrated steel slag of the present invention with a polyvinyl alcohol (PVA) organic network and using a directional freeze-drying process, the prepared aerogel has a compressive strength of over 128 MPa, realizing the transformation of steel slag from a "low-value filler material" to a "high-performance functional material". At the same time, it endows the material with multifunctional coordinated characteristics of low thermal conductivity, high sound absorption and load-bearing capacity.

[0027] (2) The aerogel prepared by the present invention exhibits certain sound absorption properties in the frequency range of 175~6300 Hz. Under the preferred conditions of a prehydration temperature of 40℃ and a prehydration time of 4 h, a significant sound absorption coefficient peak of 0.74 appears at 800 Hz, and a second sound absorption peak is formed at about 4200 Hz with a sound absorption coefficient of about 0.30, indicating that the material has good sound energy absorption capabilities in the mid-low frequency range and a certain high frequency range.

[0028] (3) The thermal conductivity of the aerogel prepared by the present invention can be as low as 0.329 W / (m·K), which is better than that of traditional concrete and comparable to that of lightweight concrete, and can provide a certain thermal insulation function for building envelope.

[0029] (4) This invention uses steel slag as an inorganic skeleton raw material to realize the high-value utilization of bulk industrial solid waste. It mainly relies on physical and chemical action, directional freezing and freeze drying, without the need for high-temperature sintering. The process is simple and has the feasibility of large-scale production. Attached Figure Description

[0030] Figure 1 The image shows the microstructure of the steel slag-based aerogel composite material obtained in Example 4.

[0031] Figure 2 Load curves for the compressive strength test of aerogel composite materials in Examples 1-6;

[0032] Figure 3 The results are the sound absorption coefficient test results of the aerogel composite materials in Examples 1-6;

[0033] Figure 4 The results show the thermal conductivity of the aerogel composite materials in Examples 1-6. Detailed Implementation

[0034] The present invention will now be described in further detail.

[0035] Example 1

[0036] A method for preparing a steel slag-based aerogel functional material includes the following steps:

[0037] (1) Steel slag powder was mixed with deionized water at a liquid-to-solid ratio of 2:1 and pre-hydrated in a constant temperature water bath at 20℃ with a stirring speed of 250 rpm for 1 hour. After pre-hydration, the wet steel slag was dried at 40℃ until the moisture content was no more than 0.2%, crushed and passed through a 400-mesh sieve to obtain pre-hydrated steel slag powder.

[0038] (2) Dissolve polyvinyl alcohol (PVA) powder in deionized water to prepare a PVA solution with a mass fraction of 10%. Weigh the prehydrated steel slag powder and PVA solution at a mass ratio of 1:1, and mix and stir at 400 rpm for 5 min at room temperature to obtain a uniform composite slurry.

[0039] (3) Pour the composite slurry into a mold with a brass heat-conducting plate at the bottom. The bottom of the mold is in close contact with liquid nitrogen. directional freeze for 30 minutes to completely freeze the slurry.

[0040] (4) Demold the frozen sample and transfer it into a freeze dryer. Dry it for 3 days under a vacuum of 4~10 Pa to obtain steel slag-based aerogel functional material.

[0041] The following performance tests were performed on the obtained aerogel material: compressive strength test; thermal conductivity test; sound absorption coefficient test, with a test frequency range of 175~6300 Hz.

[0042] Example 2

[0043] The only difference from Example 1 is that in step (1), the mixture is stirred for 4 hours for pre-hydration treatment.

[0044] Example 3

[0045] The only difference from Example 1 is that in step (1), the temperature of the constant temperature water bath is 40°C.

[0046] Example 4

[0047] The only difference from Example 3 is that in step (1), the mixture is stirred for 4 hours for pre-hydration treatment.

[0048] Example 5

[0049] The only difference from Example 1 is that in step (1), the temperature of the constant temperature water bath is 60°C.

[0050] Example 6

[0051] The only difference from Example 5 is that in step (1), the mixture is stirred for 4 hours for pre-hydration treatment.

[0052] All raw materials used in the above embodiments were commercially available products. The steel slag was sourced from Nanjing, Jiangsu Province, and the PVA was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. The deionized water used in the experiments was obtained from an ultrapure water system.

[0053] Morphological characteristics

[0054] The microstructure of the steel slag-based aerogel composite material obtained in Example 4 was observed using a scanning electron microscope, and the results are as follows: Figure 1 As shown, a layered porous structure is formed inside the material, with pore sizes mainly distributed between 100 and 500 μm. The pore wall framework is continuous and intact, with a rough surface and a large number of fine particles attached, and no obvious collapse or through cracks are observed. This porous structure is formed by the growth of ice crystals displacing solid components during directional freezing. The interconnected pores provide channels for sound waves to enter the material and undergo viscous loss, while the continuous and intact composite pore wall framework provides load-bearing support for the material.

[0055] Performance testing

[0056] (1) Compressive strength test

[0057] The compressive strength test was conducted according to "JGJ / T70-2023 Test Methods for Basic Properties of Building Mortar". The test specimen size was 13 mm × 13 mm × 13 mm. During the entire loading process, the specimen was loaded uniformly and continuously at a rate of 1 mm / min until the strain reached 90%, and the maximum load was recorded. The results are as follows: Figure 2As shown, the load on each sample continuously increased with displacement during compression, and the curves did not show a sudden drop, indicating that the material exhibited a gradual compaction characteristic under compression and did not undergo brittle failure. Example 1 had the lowest maximum load, approximately 21,500 N; while Examples 2-6 all had maximum loads of approximately 69,000-70,000 N, an increase of approximately 3.2 times compared to Example 1, indicating that increasing the prehydration temperature or extending the prehydration time can significantly improve the material's load-bearing capacity. Comparing Examples 1, 3, and 5 with the same prehydration time (1 h), after increasing the prehydration temperature from 20℃ to 40℃ and 60℃, the maximum load increased from approximately 21,500 N to approximately 70,000 N and 69,500 N, respectively. Furthermore, the curves of Examples 3 and 5 were generally located to the left of Example 1, with Example 5 having the smallest displacement required to reach the same load and the highest compressive stiffness. This indicates that increasing the prehydration temperature promoted the formation of hydration products on the steel slag surface, enhanced the organic-inorganic interface bonding, and improved load transfer efficiency. Comparing Examples 2, 4, and 6 with the same prehydration time (4 h), the maximum loads of the three are similar. Example 4 has the smallest displacement required to reach the maximum load (approximately 10.7 mm) and the steepest curve slope, exhibiting the highest compressive stiffness. The curves of Examples 2 and 6 are almost identical, indicating comparable stiffness. In summary, the material exhibits optimal load-bearing performance when the prehydration time is 4 h and the prehydration temperature is 40℃. Appropriate prehydration treatment enables the steel slag and PVA network to form a continuous and uniform organic-inorganic interpenetrating structure, effectively dispersing and transferring the load.

[0058] (2) Sound absorption performance test

[0059] The sound absorption performance was tested using the dual-microphone transfer function method from the standard GB / T 18696.2-2002 (ISO 10534-2:1998), specifically in the section "Measurement of Sound Absorption Coefficient and Acoustic Impedance in Acoustic Impedance Tubes - Part 2: Transfer Function Method". The sample was machined into a cylinder with a diameter of 28 mm and a thickness of 50 mm, matching the impedance tube. After being embedded in the impedance tube port, random noise was emitted by a loudspeaker, and the sound pressure signal was collected by two microphones. The incident and reflected waves were separated using the transfer function method, and the normal incident sound absorption coefficient of the sample was calculated. The sound absorption performance was statistically analyzed within the frequency range of 175–6300 Hz. The results are as follows: Figure 3As shown, under the conditions of prehydration temperature of 20℃ or 60℃, and prehydration at 40℃ for 1 h (i.e., Examples 1, 2, 3, 5, and 6), the samples basically did not form obvious sound absorption peaks in the frequency range of 175~6300 Hz, with most frequency bands having a sound absorption coefficient of only 0.02~0.10. However, under the conditions of prehydration temperature of 40℃ and prehydration time of 4 h (i.e., Example 4), the sample showed an obvious sound absorption peak at about 800 Hz, with a peak sound absorption coefficient of 0.74, which is about 6 times that of the other examples, and a second sound absorption peak (about 0.30) appeared at about 4200 Hz. The above results indicate that prehydration temperature and time have a synergistic effect on sound absorption performance. Only under suitable prehydration conditions (40℃, 4 h) can the interfacial bonding between steel slag and PVA network be improved, the porous structure formed by directional freezing be more regular, and the material can produce obvious sound absorption effect in the mid-to-low frequency range. When the prehydration temperature is too low or too high, or the prehydration time is insufficient, it is difficult to obtain significant sound absorption performance.

[0060] (3) Thermal insulation performance test

[0061] The thermal insulation performance was tested according to GB / T 32064-2015 "Temperature Conductivity and Thermal Diffusivity of Building Materials - Transient Plane Heat Source Test Method". The thermal conductivity of the steel slag-based aerogel composite material was determined based on an infinite medium model. The test atmosphere was air, the temperature range was room temperature, the specific temperature point was 25℃, and the test was performed in triplicate. The results are as follows: Figure 4 As shown, the steel slag-based aerogel composite material prepared in Example 4 has a thermal conductivity as low as 0.329 W / (m·K), which is only about 1 / 7 of that of ordinary concrete (2.3 W / (m·K)) and comparable to lightweight concrete, exhibiting excellent thermal insulation performance. This is attributed to the pre-hydration treatment improving the interfacial bonding between the steel slag and the PVA network, the layered porous structure formed by directional freezing effectively blocking the heat conduction path, and the still air within the pores further weakening heat transfer.

[0062] The thermal conductivity of the remaining embodiments ranges from 0.348 to 0.465 W / (m·K), with Embodiment 6 having a thermal conductivity of 0.348 W / (m·K), second only to Embodiment 4. Embodiments 1 and 2 have relatively higher thermal conductivity, at 0.465 and 0.455 W / (m·K), respectively. The differences in thermal conductivity among the groups are consistent with the evolution of pore structure: when the degree of prehydration is optimized, a layered pore structure with high porosity and small pore size is formed inside the material, which significantly prolongs the solid-phase heat transfer path and inhibits gas-phase heat transfer, thus reducing the thermal conductivity; conversely, when the pore structure is not sufficiently porous or the interfacial bonding is weak, the proportion of solid-phase heat transfer increases, and the thermal conductivity increases.

[0063] In summary, the steel slag-based aerogel composite material prepared by combining prehydrated steel slag powder obtained under suitable prehydration conditions with PVA achieves a low thermal conductivity while possessing both load-bearing capacity and sound absorption properties, demonstrating the advantages of integrated structure and function. It has good application prospects in building insulation, industrial kiln insulation and other fields.

Claims

1. A method for pre-hydration treatment of steel slag, characterized in that, Steel slag powder is mixed with water and stirred at a temperature of 20~60℃ for 1~4 hours to carry out prehydration; the prehydrated product is dried and sieved to obtain prehydrated steel slag powder.

2. The method for pre-hydration treatment of steel slag according to claim 1, characterized in that, The mass ratio of the steel slag powder to water is 1:(1.5~2.5).

3. The method for pre-hydration treatment of steel slag according to claim 1, characterized in that, The stirring speed is 200~300 rpm.

4. The method for pre-hydration treatment of steel slag according to claim 1, characterized in that, The specific process of prehydration is as follows: steel slag powder is mixed with water and placed in a constant temperature water bath at 20~60℃. The mixture is stirred for 1~4 hours to carry out prehydration, so that a hydration product layer containing calcium silicate gel and calcium hydroxide is generated in situ on the surface of the steel slag particles.

5. A method for preparing a steel slag-based aerogel composite material, characterized in that, Includes the following steps: (1) The prehydrated steel slag powder prepared by the method of claim 1 is mixed and stirred with a polyvinyl alcohol solution to obtain a composite slurry; (2) Pour the composite slurry into a mold and use the ice template method for directional freezing; (3) The product obtained by directional freezing is freeze-dried to obtain a steel slag-based aerogel composite material.

6. The method for preparing the steel slag-based aerogel composite material according to claim 5, characterized in that, In step (1), the mass ratio of the prehydrated steel slag powder to the polyvinyl alcohol solution is (0.8~1.2):

1.

7. The method for preparing the steel slag-based aerogel composite material according to claim 5, characterized in that, In step (1), the mass fraction of the polyvinyl alcohol solution is 8-12%.

8. The method for preparing the steel slag-based aerogel composite material according to claim 5, characterized in that, In step (2), the directional freezing time is 20 to 30 minutes.

9. The method for preparing the steel slag-based aerogel composite material according to claim 5, characterized in that, In step (1), the stirring speed is 300~500 rpm and the stirring time is 4~6 min.

10. The method for preparing the steel slag-based aerogel composite material according to claim 5, characterized in that, In step (3), the vacuum degree of the drying is 4~10 Pa, and the total drying time is 2~4 days.