A low-alkali, crack-resistant cement clinker for pipe gallery with synergistic regulation of mineral phase and micro-expansion and its preparation method
By adjusting the composition and preparation method of cement clinker, the problems of hydration heat release and volume stability were solved, and a low-alkali crack-resistant cement clinker suitable for underground pipe corridors was prepared. It has good early strength and crack resistance and is suitable for underground pipe corridors and concrete water conveyance pipelines.
Patent Information
- Application Number
- CN202611520522.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cement technology struggles to maintain early strength while simultaneously ensuring hydration heat release and volume stability, especially in underground utility tunnels and large-volume underground concrete construction, where it cannot effectively control hydration heat and volume changes.
A method for preparing low-alkali crack-resistant pipe gallery cement clinker was adopted. By adjusting the content of C3A, C3S, MgO, free CaO and alkali, and combining it with raw materials such as low-alkali limestone, silica, red mud and fly ash, cement clinker that meets specific composition requirements was prepared. It was then ground together with limestone, mineral powder and desulfurized gypsum to form a cementitious material suitable for underground pipe galleries.
It achieves effective control of hydration heat release and volume stability while maintaining early strength, making it suitable for underground pipe corridors and concrete water pipelines, and possessing good crack resistance, impermeability resistance and chemical corrosion resistance.
Smart Images

Figure CN123106028A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cement clinker and inorganic cementitious material preparation technology, and relates to a low-alkali crack-resistant cement clinker for pipe gallery with synergistic regulation of mineral phase and micro-expansion and its preparation method. Background Technology
[0002] Underground utility tunnels and large-volume underground concrete applications place specific requirements on the strength, crack resistance, impermeability, and chemical resistance of cementitious materials. Concrete generates heat of hydration during early hardening, and temperature changes and shrinkage affect the structural volume deformation. Furthermore, the construction and demolding of utility tunnel components require a certain early strength; therefore, the clinker composition design must simultaneously consider the heat of hydration and strength development. When used for concrete water pipelines, cementitious materials must also be selected based on the load-bearing capacity, water pressure, and durability requirements of the corresponding products.
[0003] Existing cement technologies control the heat of hydration by adjusting the composition of silicate and aluminate minerals, or regulate volume changes by utilizing the expansion effect of magnesium-containing components. For example, Chinese invention patent application CN102976641A, published on March 20, 2013, describes a micro-expansion medium-heat silicate cement and its production method, involving a low-alumina, high-iron composition and the proportions of MgO, alkali content, and sulfate content. This disclosure indicates that the balance between low heat, micro-expansion, and strength is an existing research direction, and the suitability of cement for specific pipe gallery conditions cannot be determined solely by any one of these indicators.
[0004] For specific low-alkali limestone resources and existing calcination, cooling, and grinding routes, it is necessary to clarify the combined requirements for clinker mineral phases, MgO, free CaO, alkali content, and batching ratios, and to ensure that clinker preparation and finished cement preparation are interconnected at the material level. The challenge is to maintain early strength requirements while also considering hydration heat release and volume stability, rather than simply reducing the content of a single clinker mineral. Summary of the Invention
[0005] This invention proposes a low-alkali, crack-resistant cement clinker for pipe gallery applications. Based on clinker quality, the clinker contains 5.0%–6.5% C3A, 50%–60% C3S, 3.5%–5.0% MgO, no more than 1.20% free CaO, and no more than 0.60% alkali (R2O). The clinker has a saturation ratio (KH) of 0.920±0.020, a silica ratio (n) of 2.30±0.10, and an aluminum ratio (P) of 1.00±0.10.
[0006] The clinker preparation includes raw meal preparation, preheating, rotary kiln calcination, and grate cooling. Based on the total mass of the raw meal, the proportions are: 80.0%–83.5% calcareous material, 10.0%–12.0% silicate corrective material, 3.7%–4.5% ferrous corrective material, and 2.7%–4.6% aluminous corrective material, with the sum of these four types of raw materials being 100%. Low-alkali limestone is used for the calcareous material, silica for the silicate corrective material, red mud for the ferrous corrective material, and fly ash for the aluminous corrective material. These four types of raw materials are metered by a metering system and then fed into a raw meal mill for grinding. The resulting raw meal is preheated and then fed into a rotary kiln. Under a 1700℃ flame, heat exchange brings the material to 1450℃, and calcination is carried out for 30–60 minutes. The clinker is then rapidly cooled to room temperature using a grate cooler.
[0007] Low-alkali limestone shall have a CaO content of not less than 50%, an MgO content of 2.8%–3.2%, and an R2O content of not more than 0.25%. Silica shall have a SiO2 content of not less than 85% and an R2O content of not more than 1.20%. Red mud shall have a Fe2O3 content of not less than 50% and an R2O content of not more than 1.20%. Fly ash used in aluminum corrective materials shall have a loss on ignition of not more than 8.0%, an Al2O3 content of not less than 28.0%, and an R2O content of not more than 0.80%.
[0008] The rotary kiln uses raw coal as fuel. The total moisture content of the raw coal is no more than 13%, the internal moisture content is no more than 4.0%, the ash content is no more than 18.0%, the volatile matter is 30±5%, the calorific value on received basis is no less than 5800 kcal / kg, and the total sulfur content is no more than 0.40%.
[0009] When further preparing pipe gallery cement from the obtained clinker, the following proportions are used based on the total mass of the four ingredients: 89% clinker, 2% limestone, 3% mineral powder, and 6% desulfurized gypsum. These are all weighed together and then ground in a cement mill. The finished product should have limestone with a CaO content of not less than 50% and an Al2O3 content of not more than 1.5%; mineral powder with a moisture content of not more than 1.0%, a loss on ignition of not more than 1.0%, an SO3 content of not more than 1.0%, and a specific surface area of not less than 405 m². 2 / kg, activity index not less than 95%; desulfurized gypsum moisture not greater than 13.0%, SO3 content not less than 38.0%, R2O content not greater than 0.30%, Cl − The content is not greater than 0.20%. The 45µm sieve residue of the cement obtained from co-grinding of the pipe gallery is 7% to 13%, and the specific surface area is 300 to 350 m². 2 / kg.
[0010] Beneficial effects:
[0011] 1. The above technical arrangement links the composition requirements of C3A and C3S with hydration exothermics and early strength, respectively, and considers MgO, free CaO, and volume stability together. The alkali content requirements of low-alkali limestone and corrective raw materials are in the same batching system as the low-alkali target of clinker, avoiding the situation where only the performance name of the finished product is given without corresponding restrictions at the raw material and clinker levels.
[0012] 2. The clinker composition control is integrated with the subsequent 89 / 2 / 3 / 6 finished product batching, providing a clear arrangement for the preparation of cementitious materials for underground pipe corridors and concrete water conveyance products. The historical values listed in the specific implementation method are from the technical disclosure records; however, due to batch relationships and testing limitations, these records are used to illustrate existing data and do not imply that any combination of ranges will produce the same effect, nor do they represent the synergistic effect between micro-expansion and mineral phase control as having been independently verified. Attached Figure Description
[0013] The invention will now be further described with reference to the accompanying drawings.
[0014] Figure 1 This is a schematic diagram of the clinker preparation process, showing the sequence in which four types of raw materials are metered, ground, preheated, calcined, and cooled to obtain cement clinker for the pipe gallery.
[0015] Figure 2 This diagram illustrates the relationship between clinker composition and rate limits, showing the composition requirements and KH, n, and P requirements for the same clinker.
[0016] Figure 3 These are schematic diagrams illustrating the connection between finished cement batching and grinding, showing the batching of clinker, limestone, mineral powder, and desulfurized gypsum, and their applications in finished cement. All three diagrams are schematic representations of technical relationships and do not represent equipment dimensions, spatial installation locations, or actual measured microstructures.
[0017] Figure 4 The hydration heat recording diagrams in Tables 3 and 6 of the specific implementation method represent the 3-day and 7-day hydration heat values in the "original table row 1" column and the "original table row 2" column, respectively.
[0018] Figure 5 The mineral composition records in Tables 2 and 5 are shown in the specific implementation. The four panels represent C3S, C2S, C3A, and C4AF, respectively. Figure 4 and Figure 5 The plotting data are derived from existing records in the table above, without adding test data. Detailed Implementation
[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] Raw material selection and preparation process
[0021] This embodiment uses low-alkali limestone as the main raw material, combined with silica, ferrous, and aluminous corrective materials to prepare pipe gallery cement clinker. The obtained clinker is then ground together with limestone, mineral powder, and desulfurized gypsum to produce pipe gallery cement. The pipe gallery cement is used for underground pipe galleries, underground large-volume concrete, and concrete water pipelines. Raw material metering is performed separately for clinker preparation and finished cement grinding.
[0022] The four types of raw materials used to prepare clinker, by mass percentage, include: 80.0%–83.5% calcareous material, 10.0%–12.0% silicate corrective material, 3.7%–4.5% ferrous corrective material, and 2.7%–4.6% aluminous corrective material. Specifically, low-alkali limestone is used for the calcareous material, silica for the silicate corrective material, high-ferrous red mud for the ferrous corrective material, and fly ash for the aluminous corrective material. These four types of raw materials are used in raw meal preparation, and after grinding and calcination, form the pipe gallery cement clinker.
[0023] The calcareous material uses low-alkali limestone from our own mine, with its CaO content controlled to be no less than 50%, MgO content to be 2.8%–3.2%, and alkali content (R₂O) no greater than 0.25%. This limestone serves as the main raw material for clinker, and its MgO content is also incorporated into the clinker composition design. The clinker batching is based on this low-alkali mineral resource, combining the CaO, MgO, and R₂O specifications of the limestone with the composition requirements of other corrective materials.
[0024] The silica correcting material uses low-alkali, high-silica silica from the Fuping area, with its SiO2 content controlled to be no less than 85% and R2O content no more than 1.20%. When selecting silica materials, both Al2O3 and R2O content are considered to meet the control requirements for alumina and alkali content in clinker batching. Silica, along with the other three types of raw materials, enters the raw meal mill but is not used as a grinding admixture in the finished cement formula.
[0025] The iron-based corrective material used is Shandong red mud, with its Fe2O3 content controlled to be no less than 50% and R2O content no greater than 1.20%. This iron-based material is combined with a batching arrangement that reduces Al2O3 and increases Fe2O3 in the clinker to form the mineral composition of the pipe gallery cement clinker. In this embodiment, red mud is a component of the clinker raw meal, belonging to a different batching stage than the mineral powder added during the grinding of the finished cement.
[0026] The aluminum corrective material uses fly ash from Shang'an Power Plant, with its loss on ignition (LOSS) controlled to be no more than 8.0%, Al2O3 content no less than 28.0%, and R2O content no more than 0.80%. The fly ash used as the aluminum corrective material is mixed with low-alkali limestone, silica, and red mud to form raw meal, and the proportion of the fly ash added is within the range of 2.7% to 4.6% of the aforementioned aluminum corrective material.
[0027] The fuel used is raw coal from Fugu County, Shaanxi Province, with total moisture content controlled to be no more than 13%, internal moisture content no more than 4.0%, ash content no more than 18.0%, volatile matter content 30±5%, calorific value on received basis no less than 5800 kcal / kg, and total sulfur content no more than 0.40%. The raw coal is selected according to the above fuel specifications and is determined separately with the calcareous, siliceous, ferrous, and aluminous materials used to prepare the raw meal.
[0028] During raw meal preparation, a metering system measures the calcium-based, silica-based, ferrous-based, and aluminous-based corrective materials, and these raw materials are then fed together into a raw meal mill for grinding. The resulting raw meal is preheated and then fed into a rotary kiln for calcination. The material obtained from the raw meal mill is used as feed for the rotary kiln calcination process. After calcination in the rotary kiln, the material is cooled to form clinker for cement grinding.
[0029] In the rotary kiln, the raw materials undergo heat exchange under a 1700℃ flame, raising the material temperature to 1450℃, with a calcination time of 30–60 minutes. The calcined material is then rapidly cooled to room temperature using a grate cooler to obtain pipe gallery cement clinker. Here, 1700℃ is the flame temperature, and 1450℃ is the material temperature reached through heat exchange.
[0030] The pipe gallery cement clinker obtained through calcination and cooling is used in the preparation of finished cement. By mass ratio, the finished cement consists of 89% pipe gallery cement clinker, 2% limestone, 3% mineral powder, and 6% desulfurized gypsum. The limestone, mineral powder, and desulfurized gypsum in the finished cement are metered and added together with the clinker during the cement grinding process, and are distinguished from the four types of raw materials in the raw meal preparation process.
[0031] The finished cement uses desulfurized gypsum from Shijiazhuang Shang'an Power Plant, with its moisture content controlled to be no more than 13.0%, SO3 content no less than 38.0%, R2O content no more than 0.30%, and Cl... −The content is no more than 0.20%. The desulfurized gypsum is measured according to the aforementioned finished cement mix ratio and is fed into the cement mill along with clinker, limestone and mineral powder.
[0032] The limestone in the finished cement formula shall have a CaO content of not less than 50% and an Al2O3 content of not more than 1.5%. The limestone accounts for 2% of the finished cement formula, and its batching process is cement grinding; the calcium-based materials used for clinker preparation shall be selected according to the aforementioned low-alkali limestone specifications and raw meal proportions.
[0033] The finished cement formula should have a mineral powder moisture content of no more than 1.0%, a loss on ignition of no more than 1.0%, an SO3 content of no more than 1.0%, and a specific surface area of no less than 405 m². 2 / kg, with an activity index of not less than 95%. The mineral powder is added at 3% of the finished cement formula and is ground together with the clinker, limestone and desulfurized gypsum.
[0034] After each component of the finished cement is separately metered by a metering system, they are fed together into a cement mill for grinding to obtain pipe gallery cement. The 45µm sieve residue of the pipe gallery cement is controlled at 7%–13%, and the specific surface area is controlled at 300–350 m². 2 / kg. The cement grinding stage follows the aforementioned clinker calcination and cooling stage, using the cooled pipe gallery cement clinker as the main grinding material.
[0035] The original technical data also listed the specifications of the fly ash used as a blending material, which was fly ash from Shang'an Power Plant, with its moisture content controlled to be no more than 1.0%, loss on ignition no more than 5.0%, Al2O3 content no less than 28.0%, R2O content no more than 0.80%, f-CaO content no more than 1.0%, and activity index no less than 70%. The specifications of this blending material fly ash are listed separately from those of the aforementioned raw alumina corrective material fly ash.
[0036] The original technical data separately listed the specifications for silica fume used as a composite material, controlling its moisture content to be no more than 1.0%, loss on ignition to be no more than 3.0%, SiO2 content to be no less than 90%, and specific surface area to be no less than 18000 m². 2 / kg, with an activity index of not less than 105%. The aforementioned fixed finished cement mix proportions do not separately list the amounts of fly ash and silica fume added.
[0037] clinker composition and existing records
[0038] The control of C3A content takes into account both hydration heat release and early performance. Original technical data suggests that C3A in clinker hydrates and releases heat rapidly; reducing its content is one measure to reduce hydration heat release. Simultaneously, to meet the early performance requirements for pipe gallery component construction and demolding, its content is maintained within the range of 5.0%–6.5%. The C3S content is controlled at 50%–60% to maintain the clinker composition required for early strength. Therefore, the composition design is not solely aimed at reducing hydration heat, but considers both early strength and hydration heat release simultaneously.
[0039] The designed MgO content is 3.5%–5.0%, and its role in this scheme is based on the hydration expansion effect described in the original technical data, intended to mitigate cracking caused by cement shrinkage. The upper limit for f-CaO is 1.20%, which, together with the clinker ratio, constitutes the composition control requirements. For both of the above two items, the original technical data also stipulated the requirement to maintain volume stability; therefore, the utilization of micro-expansion and the stability requirement are both retained, and the content range itself is not described as the measured expansion amount.
[0040] The R2O control value is no greater than 0.60%, corresponding to the low alkali requirement proposed in the original technical data. The utility tunnel project also involves resistance to seepage and chemical erosion; therefore, low alkali control and mineral composition control are different components of the same clinker scheme. K2O and Na2O in the following chemical composition record are still listed separately; R2O uses the notation from the original technical data, and the calculation method not specified in the original data is not supplemented in this embodiment.
[0041] The clinker ratio is designed as follows: KH = 0.920 ± 0.020, n = 2.30 ± 0.10, P = 1.00 ± 0.10. Simultaneously, requirements are set for f-CaO ≤ 1.20%, R2O ≤ 0.60%, and MgO 3.5%–5.0%. The original technical data linked increasing KH to ensuring early-stage compressive strength of the clinker, and lower P to a batching approach that reduced aluminum content and increased iron content. The mineral composition requirements and ratio requirements are listed separately here to maintain the integrity of the original design.
[0042] The original technical data separately listed the following rate values for general-purpose cement clinker in normal production: KH=0.900±0.020, n=2.40±0.10, P=1.45±0.10, with an upper limit of 1.50% for f-CaO and 5.0% for MgO. This item is a record of the original general-purpose clinker scheme and is explained alongside the control values of KH, n, P, and f-CaO in this scheme; its existence does not mean that all the following records were obtained on the same date, under the same sampling conditions, or in the same test batch.
[0043] The performance design requirements for the clinker in the pipe gallery are as follows: 3-day compressive strength not less than 26.0 MPa, 28-day compressive strength not less than 48.0 MPa, 3-day heat of hydration not greater than 250 kJ / kg, and 7-day heat of hydration not greater than 300 kJ / kg. The original technical data also stipulated a 3-day compressive strength requirement for cement greater than 24.0 MPa. The above clinker performance requirements and the requirements for the produced cement are retained separately to avoid merging the indicators of the two objects into the same set of test records.
[0044] Original records of cement clinker for utility tunnels
[0045] The following tables are compilations of records from the technical briefing. The table numbers only indicate the row numbers in the original tables and do not represent confirmed sample numbers or batch relationships across tables. The values for composition and mineral content are retained from the original data, and the rate values retain their original notations. Records for pipe gallery clinker, general clinker, and cement production are listed separately, and rows from different tables are not combined into a complete production batch.
[0046] Table 1. Record of chemical composition of cement clinker for pipe gallery:
[0047] project Original table, row 1 Original table, row 2 loss 0.21 0.28 <![CDATA[SiO2]]> 21.03 21.18 <![CDATA[Al2O3]]> 4.88 4.91 <![CDATA[Fe2O3]]> 4.52 4.60 CaO 63.84 63.67 MgO 3.90 3.72 <![CDATA[K2O]]> 0.41 0.36 <![CDATA[Na2O]]> 0.24 0.24 <![CDATA[SO3]]> 0.30 0.31 <![CDATA[Cl − ]]> 0.029 0.035 f-CaO 1.04 1.12 KH 0.921 0.910 n 2.24 2.23 P 1.08 1.07
[0048] In Table 1, the MgO values in the two rows are 3.90 and 3.72, f-CaO values are 1.04 and 1.12, KH values are 0.921 and 0.910, n values are 2.24 and 2.23, and P values are 1.08 and 1.07. Both rows simultaneously retain SiO2, Al2O3, Fe2O3, CaO, the alkali component, SO3, and Cl. − This forms the original chemical record corresponding to the aforementioned mineral composition and rate values. Individual components have not been converted to new component values not provided in the original data.
[0049] Original table row number <![CDATA[C3S]]> <![CDATA[C2S]]> <![CDATA[C3A]]> <![CDATA[C4AF]]> Line 1 60.74 14.80 5.27 13.74 Line 2 58.60 16.84 5.21 13.98
[0050] Table 2. Mineral composition record of cement clinker for pipe gallery:
[0051] Table 2 shows C3A values of 5.27 and 5.21, and C4AF values of 13.74 and 13.98. The value for C3S in the first row is 60.74, which is higher than the aforementioned design upper limit of 60%. Therefore, this row is only retained as an independent mineral composition record in the original data and is not listed as an embodiment that fully meets the aforementioned composition range. The original data does not specify the method for obtaining the values in this table, and this embodiment does not supplement it as the result of a specific mineral phase detection method.
[0052] Table 3. Physical property records of cement clinker for pipe gallery:
[0053] project Original table, row 1 Original table, row 2 80µm sieve residue / % 3.2 2.8 <![CDATA[Specific surface area / (m 2 / kg)]]> 344 351 P / % 24.0 23.8 Initial setting / min 202 192 Final setting / min 294 286 Stability qualified qualified Group 1 "Flexural strength" 3d / MPa 5.5 5.7 Group 1 "Flexural strength" 28d / MPa 8.6 8.7 The second group's "flexural strength" 3d / MPa 26.4 27.6 The second group's "flexural strength" was measured at 28 days / MPa. 50.3 51.4 <![CDATA[SO3 / %]]> 2.24 2.16 Heat of hydration 3d / (kJ / kg) 242 248 Heat of hydration 7d / (kJ / kg) 282 298
[0054] Table 3 retains the columns for fineness, specific surface area, P, setting time, stability, strength, and heat of hydration. The original table had two consecutive "flexural strength (MPa)" headers, both containing sub-columns for 3d and 28d. Therefore, in the revised version, only the first and second groups are used to distinguish their positions, without changing the original name of the second group. The P / % symbols in the table are from the original physical property table and are listed separately from the aforementioned rate values P.
[0055] In Table 3, the heat of hydration records for 3 days are 242 and 248 kJ / kg, and for 7 days are 282 and 298 kJ / kg; the condensation records are 202 and 192 min for initial condensation and 294 and 286 min for final condensation. Both rows for stability are marked "qualified". These entries retain their original meaning and are not extended to include volume changes under conditions not recorded in the original data.
[0056] Original records of general-purpose cement clinker:
[0057] Table 4. Record of chemical composition of general-purpose cement clinker:
[0058] project Original table, row 1 Original table, row 2 row 3 of the original table loss 0.33 0.34 0.42 <![CDATA[SiO2]]> 21.69 21.30 21.08 <![CDATA[Al2O3]]> 5.28 5.35 5.20 <![CDATA[Fe2O3]]> 3.59 3.66 3.41 CaO 64.17 64.06 63.71 MgO 2.76 4.25 5.64 <![CDATA[K2O]]> 0.34 0.35 0.40 <![CDATA[Na2O]]> 0.32 0.30 0.25 <![CDATA[SO3]]> 0.34 0.32 0.29 <![CDATA[Cl − ]]> 0.027 0.022 0.038 f-CaO 1.43 1.32 1.24 KH 0.895 0.905 0.914 n 2.44 2.36 2.45 P 1.46 1.46 1.53
[0059] Original table row number <![CDATA[C3S]]> <![CDATA[C2S]]> <![CDATA[C3A]]> <![CDATA[C4AF]]> Line 1 55.18 20.53 7.91 10.91 Line 2 57.11 17.96 7.99 11.14 Line 3 58.51 16.29 8.02 10.37
[0060] Table 5. Mineral Composition Record of General Cement Clinker:
[0061] The chemical composition table and mineral composition table for general-purpose clinker each have three rows of records, all retained in their original order. In Table 4, the value for MgO in the third row is 5.64, and Cl... − The values in the second row are 0.022, and none of them are modified according to the aforementioned design upper limit or the values in adjacent rows. The C3A values in Table 5 are 7.91, 7.99, and 8.02, and the C4AF values are 10.91, 11.14, and 10.37, which are listed as mineral composition data for general clinker.
[0062] Table 6. Physical Properties Record of General-Purpose Portland Cement Clinker:
[0063] project Original table, row 1 Original table, row 2 80µm sieve residue / % 1.8 1.6 <![CDATA[Specific surface area / (m 2 / kg)]]> 349 341 P / % 24.2 24.3 Initial setting / min 122 128 Final setting / min 172 178 Stability qualified qualified Group 1 "Flexural strength" 3d / MPa 5.6 5.8 Group 1 "Flexural strength" 28d / MPa 9.1 9.3 The second group's "flexural strength" 3d / MPa 27.1 28.5 The second group's "flexural strength" was measured at 28 days / MPa. 56.8 57.6 <![CDATA[SO3 / %]]> 2.23 2.27 Heat of hydration 3d / (kJ / kg) 272 268 Heat of hydration 7d / (kJ / kg) 322 318
[0064] The general clinker physical properties table contains only two rows, therefore no corresponding physical property records will be added for it to correspond to the third row of Tables 4 and 5. This table also has two sets of "flexural strength" headers, which will be distinguished as described above. The listed 3-day hydration heats are 272 and 268 kJ / kg, and the 7-day hydration heats are 322 and 318 kJ / kg. These will be kept separately from the hydration heat records of the pipe gallery clinker; no batch-by-batch comparison relationships not recorded in the original data will be constructed based on this.
[0065] Based on the organization of these existing data, the clinker scheme for the utility tunnel simultaneously lists the batching direction, specific rate values, and heat of hydration requirements for lower C3A and higher iron content, while retaining early strength requirements; the general clinker record provides another set of composition and performance data. Since the original tables do not have common batch identifiers, this implementation does not interpret the difference between the two values as an independent contribution of a single component.
[0066] Composition and Product Records of Cement for Pipe Gallery:
[0067] Table 7 Cement mix proportions and technical requirements for utility tunnels:
[0068] project The values recorded Clinker / % 89.0 limestone / % 2.0 Mineral powder / % 3.0 Desulfurized gypsum / % 6.0 LOSS / % ≤3.0 <![CDATA[SO3 / %]]> 2.0~3.0 MgO / % 3.5~5.0 <![CDATA[R2O / %]]> ≤0.60 <![CDATA[Cl − / %]]> ≤0.060 <![CDATA[Specific surface area / (m 2 / kg)]]> 300~350 45µm sieve residue / % 7~13
[0069] In Table 7, LOSS is controlled to be no more than 3.0%, SO3 to 2.0%–3.0%, and MgO to 3.5%–5.0%. Other ranges or upper limits are listed in the original table. The MgO, SO3, and other items in the cement composition table are requirements for cement production and belong to two different material levels compared to the corresponding items in the clinker table.
[0070] Table 8. Technical requirements related to the use of cement in pipe galleries:
[0071] project Original data requirements Early crack resistance time / min ≥1800 <![CDATA[chloride ion diffusion coefficient, original table unit "K×10 -12 m 2 / s"]]> ≤2.50 Sulfate corrosion resistance 14d expansion rate / % ≤0.50 C35 concrete impermeability grade ≥P6 level
[0072] The requirements for the aforementioned applications involve cracking, chloride ion transport, sulfate action, and concrete impermeability. Cracking time is used for the early cracking resistance evaluation listed in the original data; the chloride ion diffusion coefficient and sulfate attack resistance items retain their original table names; the C35 concrete impermeability grade is explicitly stated with the concrete strength grade. The objects and names of the various indicators are not interchangeable.
[0073] Table 9. Record of physical properties of the manufactured cement:
[0074] project The values recorded 45µm sieve residue / % 8.8 <![CDATA[Specific surface area / (m 2 / kg)]]> 344 P / % 25.16 Initial setting / min 159 Final setting / min 227 Stability qualified Group 1 "Flexural strength" 3d / MPa 5.4 Group 1 "Flexural strength" 28d / MPa 8.4 The second group's "flexural strength" 3d / MPa 27.4 The second group's "flexural strength" was measured at 28 days / MPa. 50.2 <![CDATA[SO3 / %]]> 2.15 Heat of hydration 3d / (kJ / kg) 244 Heat of hydration 7d / (kJ / kg) 287
[0075] Table 9 shows a record of the physical properties of the cement produced, including a 45µm sieve residue of 8.8% and a specific surface area of 344 m². 2 / kg, with initial setting time and final setting time of 159 min and 227 min, respectively. The table retains the two original strength columns titled "Flexural Strength," without renaming one of them based on numerical values. The heat of hydration is recorded as 244 kJ / kg at 3 days and 287 kJ / kg at 7 days, listed separately from the aforementioned clinker physical properties table.
[0076] Table 10 Records related to cement production and applications:
[0077] project The values recorded Early cracking time / min 2445 Chloride ion diffusion coefficient 2.41 Sulfate resistance 14d expansion coefficient 0.031 C35 concrete impermeability grade P7 level loss 1.87 MgO 4.34 <![CDATA[K2O]]> 0.52 <![CDATA[Na2O]]> 0.13 <![CDATA[Cl − ]]> 0.044
[0078] Table 10 uses the same item names as the results table: "Early Cracking Time" and "Sulfate Resistance 14d Expansion Coefficient" are distinguished from "Early Cracking Resistance Time" and "Sulfate Resistance 14d Expansion Rate" in the requirements table by retaining the original wording. This results table does not have complete repeating units; therefore, no additional testing caliber is specified for items without units. Table 10 also does not forcibly establish a batch correspondence with any clinker row in Table 1.
[0079] The technical briefing specifies the applications of cement for underground utility tunnels, large-volume underground concrete, and concrete water pipeline products, and outlines requirements for crack resistance, impermeability, chemical corrosion resistance, and strength maintenance. The original documentation also mentions "preparing concrete materials for utility tunnels with a strength grade of 50 MPa or higher"; this record is retained separately from the C35 concrete impermeability test results in Tables 8 and 10, and they are not combined into test results for the same concrete mix proportion.
[0080] When the cement is used in the aforementioned products, its application direction is explained by the material uses and existing technical requirements. The original technical documentation did not list the concrete composition, sample preparation methods, and curing conditions corresponding to all application records. Therefore, the values listed in this embodiment are limited to the recorded objects and items in the disclosure and are not extended to the same performance results obtainable under any concrete mix ratio and any construction environment.
[0081] The materials and indicators in the attached diagram correspond to...
[0082] Figure 1 The four inlets all correspond to the raw material formula. The upper and lower limits of each raw material must be selected from the same total amount of ingredients, and the actual proportions of each item must add up to 100%. It is not permissible to use all upper limits simultaneously, nor is it permissible to supplement any less than 100% of the total amount with another raw material. The four materials converge into a common metering and grinding step, and the grinding output is raw meal, which is then sent to the preheating and rotary kiln for calcination. The connecting lines in the diagram indicate existing material connections; no separate mixing device or specified order of adding the four types of raw materials is required.
[0083] Figure 1 The 1700℃ and 1450℃ in the firing frame correspond to the flame and the material, respectively. They are related through heat exchange, not as the holding temperatures of two separate material sections. 1700℃ is not used as the measurement temperature for the resulting clinker. The fired material is cooled by a grate to obtain clinker, which is... Figure 1 Output and Figure 3 The main input. Raw coal is used to provide the heat source for combustion, and will be explained separately from the aforementioned four types of raw materials; desulfurized gypsum belongs to... Figure 3 Cement grinding and batching, not included Figure 1 The percentage of raw materials.
[0084] Figure 2The composition and rate conditions for the same clinker are divided into two groups. The branches containing C3A, C3S, MgO, free CaO, and R2O retain their respective compositional meanings, while the branches containing KH, n, and P retain their rate value notations. Both sets of conditions refer to the same clinker object; there is no automatic conversion between the remaining conditions from one condition in the diagram. This diagram is a compositional constraint illustration and does not depict total MgO as a periclase microstructure with a specific grain size or distribution.
[0085] Figure 3 Limestone, mineral powder, and desulfurized gypsum are all added to cement batching after clinker calcination and cooling. The 2% limestone content in the finished product and the percentage of calcareous raw materials are different total amounts, although their names are similar, they are still expressed separately. Mineral powder and desulfurized gypsum are not used as raw meal corrective agents. The 45µm sieve residue and specific surface area after cement milling are for finished cement, and do not use the 80µm sieve residue from the clinker physical property record, nor do they use the specific surface area of the mineral powder itself to replace the finished product indicators.
[0086] Figure 3 The end-stage pipe gallery concrete and water pipeline products represent existing applications of the finished cement, and the proportions of aggregate, water, or admixtures are not given in the figure. The cement preparation process therefore terminates at the finished product obtained through co-grinding; the two downstream application boxes do not add molding, curing, or testing steps for specific components. The aforementioned strength, impermeability, and early cracking records are still listed separately for each table item and are not merged into the same product sample due to similar application directions.
[0087] Figure 4 All data used are taken from Tables 3 and 6 of this specific implementation. In the figure, "Table 3 Record 1" and "Table 3 Record 2" are located in the "Original Table Row 1" and "Original Table Row 2" columns of Table 3, respectively; "Table 6 Record 1" and "Table 6 Record 2" are located in the two columns with the same name in Table 6, respectively. The rows for "Hydration Heat 3d / (kJ / kg)" in Table 3 are 242 and 248, respectively, and the rows for "Hydration Heat 7d / (kJ / kg)" are 282 and 298, respectively; the corresponding rows in Table 6 are 272 and 268, and 322 and 318, respectively. Each bar directly represents a value in the corresponding cell, and the two ages of the same record are arranged side by side.
[0088] Figure 4 Values are located using both the table number and the record number within the table. "Record 1" and "Record 2" correspond to the original table row and column saved in the table header; they do not refer to the first or second physical data rows of the transposed table, nor do they indicate newly added samples or repeated tests. The original data did not fully describe the test conditions and sample batches for each record; therefore, paired improvement rates, error bars, or statistical significance are not calculated, and the differences in the bar charts are not interpreted as independent contributions from variations in a particular mineral. Continuous exothermic processes were not plotted between the two ages; therefore, the values in the figure cannot replace the instantaneous exothermic rate curve.
[0089] Figure 5 All data used are taken from Tables 2 and 5 of this specific implementation. "Table 2 Row 1" and "Table 2 Row 2" respectively locate the records in Table 2 with row headings "Row 1" and "Row 2"; "Table 5 Row 1" to "Table 5 Row 3" locate the records with the same names in Table 5, without counting the table headers as data rows. The C3S, C2S, C3A, and C4AF values for each record are directly taken from the corresponding column, resulting in twenty original table values. The four panels each have a vertical axis scale, without normalization, without adding points, and without inferring other minerals from the difference between the listed components and 100%. Figure 5 The table number and Figure 4 Unlike other methods, its record labels do not establish cross-table sample pairing relationships between mineral composition and heat of hydration.
[0090] Figure 5 The record of 60.74% C3S listed in Table 2 is retained. This value is higher than the upper limit of the aforementioned composition range of 50% to 60% C3S, and therefore cannot be interpreted as an example meeting this range simply because it is listed in the clinker record for the pipe gallery. The original data did not specify the analytical or calculation methods used for each mineral value. This figure is used to represent existing composition records and does not rewrite these values as actual phase contents determined by X-ray diffraction, nor does it confirm a synergistic effect between mineral phases and micro-expansion based on differences in the figure.
[0091] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.
Claims
1. A low-alkali, crack-resistant cement clinker for pipe gallery with synergistic regulation of mineral phase and micro-expansion, characterized in that, Based on the mass of the cement clinker, the C3A content is 5.0%–6.5%, the C3S content is 50%–60%, the MgO content is 3.5%–5.0%, the free CaO content is not greater than 1.20%, and the alkali content R2O is not greater than 0.60%.
2. The low-alkali, crack-resistant cement clinker for pipe gallery according to claim 1, characterized in that, The cement clinker has a saturation ratio KH of 0.920±0.020, a silicon content n of 2.30±0.10, and an aluminum content P of 1.00±0.
10.
3. A method for preparing the low-alkali, crack-resistant cement clinker for pipe galleries as described in claim 1, characterized in that, The process includes the following steps: Based on the total mass of the raw meal, 80.0%–83.5% of calcareous material, 10.0%–12.0% of silica correcting material, 3.7%–4.5% of ferrous correcting material, and 2.7%–4.6% of aluminous correcting material are measured, ensuring the sum of the mass percentages of the four materials is 100%. These are then fed into a raw meal mill for grinding to obtain raw meal. The calcareous material is low-alkali limestone, the silica correcting material is silica, the ferrous correcting material is red mud, and the aluminous correcting material is fly ash. The raw meal is preheated and then fed into a rotary kiln. Under a 1700℃ flame, the material temperature is increased to 1450℃ through heat exchange and calcined for 30–60 minutes. It is then rapidly cooled to room temperature using a grate cooler to obtain the cement clinker.
4. The method according to claim 3, characterized in that, The low-alkali limestone has a CaO content of not less than 50%, an MgO content of 2.8% to 3.2%, and an alkali content (R₂O) of not more than 0.25%.
5. The method according to claim 3, characterized in that, The silica has a SiO2 content of not less than 85% and an alkali content (R2O) of not more than 1.20%; the red mud has a Fe2O3 content of not less than 50% and an alkali content (R2O) of not more than 1.20%.
6. The method according to claim 3, characterized in that, The fly ash used in the aluminum corrective material has a loss on ignition of no more than 8.0%, an Al2O3 content of no less than 28.0%, and an alkali content (R2O) of no more than 0.80%.
7. The method according to claim 3, characterized in that, The rotary kiln uses raw coal as fuel for calcination. The raw coal has a total moisture content of no more than 13%, internal moisture content of no more than 4.0%, ash content of no more than 18.0%, volatile matter of 30±5%, calorific value on received basis of no less than 5800 kcal / kg, and total sulfur content of no more than 0.40%.
8. The method according to claim 3, characterized in that, The obtained cement clinker is used as raw material to further prepare pipeline cement. Based on the total mass of the four ingredients for preparing pipeline cement, 89% of the cement clinker, 2% of limestone, 3% of mineral powder and 6% of desulfurized gypsum are weighed together and then fed into a cement mill for grinding to obtain pipeline cement.
9. The method according to claim 8, characterized in that, The limestone used for preparing the pipe gallery cement has a CaO content of not less than 50%, and an Al2O3 content of not more than 1.5%; the mineral powder has a moisture content of not more than 1.0%, a loss on ignition of not more than 1.0%, a SO3 content of not more than 1.0%, a specific surface area of not less than 405 m 2 / kg, and an activity index of not less than 95%; the desulfurization gypsum has a moisture content of not more than 13.0%, a SO3 content of not less than 38.0%, an alkali content R2O of not more than 0.30%, and a Cl − content of not more than 0.20%.
10. The method according to claim 8, characterized in that, The cement for pipe racks obtained by co-grinding has a 45µm sieve residue of 7%–13% and a specific surface area of 300–350 m². 2 / kg.
Citation Information
Patent Citations
Micro-expansive moderate-heat Portland cement and production method thereof
CN102976641A