Steel slag-based low-calcium carbon-fixing cement, its preparation method and application
By calcining low-calcium carbon-fixing clinker from steel slag, silica tailings, lithium slag, and fluorite, and adding quicklime and basalt fiber, the problems of low steel slag utilization and easy cracking of low-calcium carbon-fixing cement are solved, achieving efficient steel slag reuse and carbon dioxide sequestration.
Patent Information
- Application Number
- CN202611523565.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have low steel slag utilization rates, and low-calcium carbon-fixing cement is prone to cracking and brittleness during carbonization, posing safety hazards. At the same time, they have failed to effectively achieve large-scale treatment of steel slag and carbon dioxide sequestration.
Low-calcium carbon-fixing clinker is produced by calcining steel slag, silica tailings, lithium slag, and fluorite, and quicklime, nano-calcium carbonate, and basalt fiber are added. The mineral phase composition is reconstructed at high temperature to optimize the composition and improve the high-value utilization of steel slag and the mineralization and sequestration of carbon dioxide.
It achieves efficient and high-value utilization of steel slag, reduces carbon emissions, improves the strength and toughness of low-calcium cement, solves the cracking problem during carbonization, and enhances the carbon dioxide sequestration effect.
Abstract
Description
Technical Field
[0001] This invention relates to the field of cement-based building materials technology, and in particular to a steel slag-based low-calcium carbon-fixing cement, its preparation method, and its application. Background Technology
[0002] Steel slag, a major byproduct of converter steelmaking, not only occupies valuable land resources due to its large accumulation, but also pollutes the environment with the leaching of free CaO, free MgO, and heavy metals contained within it. Existing steel slag utilization technologies mainly focus on physical activation, chemical activation, and thermal activation. These methods can only partially improve performance, resulting in low steel slag utilization rates.
[0003] The main chemical components of steel slag are CaO, SiO2, Al2O3, Fe2O3, and MgO, which in principle meet the requirements for the types of compounds in cement raw materials. Some research has been conducted on using steel slag to replace some natural raw materials in the calcination of cement clinker. However, in practical applications, the chemical composition of steel slag itself significantly limits its application in traditional cement. Existing technologies CN1096997A discloses the use of industrial by-products containing calcium silicate, gypsum, and fluorite as mineralizers, with a dosage of 5-20% as raw materials to prepare silicate cement clinker. CN109851242A discloses the preparation of steel slag with active cement clinker by mixing pulverized steel slag, clay, and quicklime in a mass ratio of 45:(12-18):(37-43) and calcining at 1300-1450℃. CN111320400A discloses the preparation of steel slag, bauxite, and lime in a mass ratio of 74- A process involving high-temperature firing of 83%:2-6%:11-24% of calcium-aluminum reconstructed steel slag can completely or partially replace cement. CN118359390A discloses adding 15-55% of a conditioning agent to molten steel slag at high temperatures to eliminate harmful free calcium oxide and convert MgO into a large amount of inactive inert minerals, thus preparing cement clinker. However, the steel slag utilization rate in the above process is as high as 80% or more, indicating that there is still considerable room for improvement in steel slag utilization, and the environmental benefits of carbon sequestration are not taken into account.
[0004] Low-calcium cement's main components are dicalcium γ-silicate, tricalcium disilicate, and monocalcium silicate. It features low hydration activity and high carbonation activity, making it an effective material for carbon dioxide sequestration. The production of low-calcium cement products can achieve carbon reduction and sequestration through a dual pathway: during the calcination stage, the low calcium content reduces carbonate consumption to control carbon emissions; during the curing and use stage, the active components absorb and fix CO2 through carbonation reactions. This synergistic effect ensures product performance while enabling the resource utilization of CO2. Its low-calcium characteristics also significantly improve its tolerance to steel slag, providing theoretical support for the large-scale, high-value utilization of steel slag.
[0005] The carbonation and hardening process of low-calcium cement depends on CO2 diffusion. The difference in the degree of carbonation inside and outside the product will lead to uneven internal stress distribution, which in turn will cause cracking. At the same time, the main carbonation products of low-calcium carbon-fixing cement are calcium carbonate and silica gel. The uneven content of these two products can easily make the sample extremely brittle and prone to flaking cracks, which poses a safety hazard in actual use.
[0006] Therefore, developing an integrated method that enables the high-value utilization of steel slag and the preparation of high-strength, low-calcium cement, by reconstructing the mineral phase composition at high temperatures and optimizing the composition of low-calcium carbon-fixing cement, can solve the dual challenges of large-scale steel slag treatment and low-calcium cement carbonization, and has significant environmental and economic value. Summary of the Invention
[0007] To address the problems existing in the prior art, this invention provides a steel slag-based low-calcium carbon fixation cement. It uses steel slag as the main material, adds silica tailings, lithium slag and fluorite to produce low-calcium carbon fixation clinker, restructures the steel slag, and adds quicklime, nano-calcium carbonate and basalt fiber to achieve high-value utilization of steel slag, while simultaneously achieving the mineralization and sequestration of carbon dioxide.
[0008] Specifically, the steel slag-based low-calcium carbon-fixing cement of the present invention is composed of the following raw materials in parts by weight: 92-97 parts of low-calcium carbon-fixing clinker, 2-3 parts of quicklime, 0.1-0.5 parts of nano-calcium carbonate, and 0.5-3.0 parts of basalt fiber.
[0009] The low-calcium carbon-fixing clinker is made by calcining, rapidly cooling, and grinding 90-95% steel slag, 3-5% silica tailings, 2-4% lithium slag, and 0-2% fluorite by weight.
[0010] This invention utilizes steel slag, silica tailings, lithium slag, and fluorite sintering to prepare low-calcium carbon-fixing clinker, with steel slag accounting for over 90%, representing a breakthrough in existing technologies. Silica tailings and lithium slag reconstruct the mineral phases of the steel slag, eliminating the need for the addition of calcium and aluminum raw materials. The resulting clinker has a low calcium-silicon ratio, which helps reduce carbon emissions and is more suitable for carbonization curing.
[0011] This invention incorporates a small amount of quicklime, whose main component is CaO, which rapidly transforms into calcium hydroxide upon contact with water, providing an alkaline environment for the matrix. During the carbonization process, CO2 dissolves in water to form H₂. + With CO3 2- The environment was acidic. The introduction of CaO made the initial pH of the sample alkaline, which promoted the ultra-early carbonation reaction of low-calcium carbon-fixing cement.
[0012] This invention adds trace amounts of nano-calcium carbonate as a seed nucleating agent, which can significantly accelerate the nucleation and growth rate of carbonation products by providing abundant heterogeneous nucleation sites for low-calcium carbon-fixing cement, thereby shortening the carbonation reaction induction period and achieving a highly efficient improvement in the ultra-early strength of low-calcium cement.
[0013] Preferably, the calcination temperature is 1300-1350℃, and the calcination time is 0.5-1.5h. This invention, using steel slag, silica tailings, lithium slag, and fluorite in a specific ratio, lowers the melting point of the raw materials, making it easier to form a liquid phase at high temperatures. The addition of lithium slag and fluorite improves the calcinability of the clinker and promotes the formation and reconstruction of calcium silicate minerals under multi-liquid phase conditions. Furthermore, the RO phase in the steel slag will experience crystal structure destruction at 1300℃, undergoing dissolution or decomposition. Simultaneously, the metal ions in the RO phase can replace Ca during the clinker calcination process. 2+ It enters the interior of the crystal lattice, introduces defects into the mineral, and enhances the activity of low-calcium cement clinker minerals.
[0014] Basalt fiber possesses excellent mechanical properties, good durability, and high-temperature resistance, while also exhibiting good compatibility with cement-based materials. Furthermore, the interfacial bonding strength between the fiber and low-calcium carbon-fixing materials is significantly enhanced, inhibiting interfacial delamination, improving sample toughness, and ensuring the stability of low-calcium carbon-fixing cement.
[0015] Preferably, the rapid cooling is achieved by air cooling.
[0016] Preferably, the grinding is performed using a ball mill.
[0017] Preferably, 0.01%-0.03% of grinding aid by weight of clinker is added before grinding.
[0018] Preferably, the grinding aid is an alcohol amine-based grinding aid.
[0019] Preferably, the low-calcium carbon-fixing clinker has a particle size ≤60μm.
[0020] Preferably, the basalt fiber is treated with an alkaline solution and then further treated with a silane coupling agent. The basalt fiber is activated by alkaline treatment, and then its surface is modified with a silane coupling agent, which significantly enhances the surface activity of the fiber. The Si-O-Si bonds on the fiber surface break, generating a large number of active hydroxyl groups (-OH), which facilitates the continued reaction.
[0021] This invention also relates to a method for preparing the above-mentioned steel slag-based low-calcium carbon-fixing cement, specifically comprising the following steps:
[0022] 1) Weigh each ingredient according to its weight.
[0023] 2) Mix all the ingredients evenly to obtain the final product.
[0024] This invention also relates to the application of the above-mentioned steel slag-based low-calcium carbon-fixing cement in the preparation of cement-based building materials.
[0025] Preferably, the preparation of cement-based building materials includes a carbonization process.
[0026] This invention has the following technical advantages:
[0027] 1. This invention uses steel slag as the main raw material to produce low-calcium carbon-fixing clinker, significantly increasing the proportion of raw materials in the steel slag and enabling high-value reuse of the steel slag.
[0028] 2. This invention utilizes the low-calcium properties of clinker produced from steel slag, silica tailings, lithium slag, and fluorite, which significantly reduces carbon emissions and is more suitable for carbonization curing.
[0029] 3. The high-strength low-calcium cement prepared by the components of this invention has the advantages of low calcination temperature and simple sintering process. The low-calcium cement has simple batching and low cost while having ultra-high mechanical properties. Detailed Implementation
[0030] To characterize the technical effect of this invention, cement was prepared and its performance was tested. During the test, cement was prepared and a neat paste was made with a water-cement ratio of 0.15. The neat paste was then pressed into cylinders with a diameter of 20 mm and a height of 20 mm. Carbonization was carried out for 24 hours under conditions of 55% humidity, 25°C, and 90% CO2 concentration. Then, the strength was tested on a universal testing machine with a pressure of 100 N / s.
[0031] Example 1
[0032] The cement is composed of the following raw materials in parts by weight: 95 parts of low-calcium carbon-fixing clinker, 2 parts of quicklime, 0.3 parts of nano-calcium carbonate, and 2 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 93% steel slag, 4% silica tailings, 2% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0033] The cement's 24-hour carbonation strength was tested to be 148.2 MPa.
[0034] Example 2
[0035] The cement is composed of the following raw materials in parts by weight: 96 parts of low-calcium carbon-fixing clinker, 2.5 parts of quicklime, 0.2 parts of nano-calcium carbonate, and 1.5 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 92% steel slag, 3% silica tailings, 4% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0036] The cement's carbonation strength after 24 hours was tested to be 144.6 MPa.
[0037] Comparative Example 1
[0038] The cement is composed of the following raw materials in parts by weight: 95 parts of low-calcium carbon-fixing clinker, 2 parts of quicklime, 0.3 parts of nano-calcium carbonate, and 2 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 93% steel slag and 7% silica tailings at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0039] The cement's 24-hour carbonation strength was tested to be 111.8 MPa.
[0040] Comparative Example 2
[0041] The cement is composed of the following raw materials in parts by weight: 95 parts of low-calcium carbon-fixing clinker, 2 parts of quicklime, 0.3 parts of nano-calcium carbonate, and 2 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 93% steel slag, 4% bauxite, 2% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0042] The cement's 24-hour carbonation strength was tested to be 127.5 MPa.
[0043] Comparative Example 3
[0044] The cement is composed of the following raw materials in parts by weight: 95 parts of low-calcium carbon-fixing clinker, 2 parts of quicklime, 0.3 parts of nano-calcium carbonate, and 2 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 82% steel slag, 10% limestone, 5% red mud, 2% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0045] The cement's 24-hour carbonation strength was tested to be 116.0 MPa.
[0046] Comparative Example 4
[0047] The cement is composed of the following raw materials in parts by weight: 97 parts of low-calcium carbon-fixing clinker, 0.3 parts of nano-calcium carbonate, and 2 parts of basalt fiber. The low-calcium carbon-fixing clinker is made by calcining 93% steel slag, 4% silica tailings, 2% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0048] The cement's 24-hour carbonation strength was tested to be 108.4 MPa.
[0049] Comparative Example 5
[0050] The cement is composed of the following raw materials in parts by weight: 95 parts of low-calcium carbon-fixing clinker and 4.3 parts of quicklime. The low-calcium carbon-fixing clinker is made by calcining 93% steel slag, 4% silica tailings, 2% lithium slag, and 1% fluorite at 1350℃ for 1 hour, followed by rapid cooling and grinding to a particle size ≤60μm.
[0051] The cement's carbonation strength after 24 hours was tested to be 121.1 MPa.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A steel slag-based low-calcium carbon-fixing cement, characterized in that, It is composed of the following raw materials in parts by weight: 92-97 parts low-calcium carbon-fixing clinker, 2-3 parts quicklime, 0.1-0.5 parts nano-calcium carbonate, and 0.5-3.0 parts basalt fiber. The low-calcium carbon-fixing clinker is made by calcining, rapidly cooling, and grinding 90-95% steel slag, 3-5% silica tailings, 2-4% lithium slag, and 0-2% fluorite by weight.
2. The steel slag-based low-calcium carbon-fixing cement according to claim 1, characterized in that, The calcination temperature is 1300-1350℃, and the calcination time is 0.5-1.5h.
3. The steel slag-based low-calcium carbon-fixing cement according to claim 1, characterized in that, The rapid cooling process uses air cooling.
4. The steel slag-based low-calcium carbon-fixing cement according to claim 1, characterized in that, The grinding process uses a ball mill.
5. The steel slag-based low-calcium carbon-fixing cement according to claim 4, characterized in that, Add 0.01%-0.03% of grinding aid by weight of clinker before grinding.
6. The steel slag-based low-calcium carbon-fixing cement according to claim 5, characterized in that, The grinding aid is an alcohol amine-based grinding aid.
7. The steel slag-based low-calcium carbon-fixing cement according to claim 1, characterized in that, The low-calcium carbon-fixing clinker has a particle size ≤60μm.
8. The method for preparing steel slag-based low-calcium carbon-fixing cement according to any one of claims 1-7, characterized in that, Includes the following steps: 1) Weigh each ingredient according to its weight. 2) Mix all the ingredients evenly to obtain the final product.
9. The application of the steel slag-based low-calcium carbon-fixing cement according to any one of claims 1-7 in the preparation of cement-based building materials.
10. The application according to claim 10, characterized in that, The preparation of cement-based building materials includes a carbonization process.
Citation Information
Patent Citations
Method for quick burning silicate cement clinker at low temp.
CN1096997A
Method for modifying steel slag
CN109851242A