Low-carbon lightweight aggregate for 3D printed concrete

By using low-carbon materials and geopolymer bonding technology to prepare lightweight synthetic aggregates, the problem of high carbon emissions caused by high-temperature sintering is solved, the material properties and reliability of 3D printed concrete are improved, and low-carbon and sustainable 3D printing construction is realized.

CN123106049APending Publication Date: 2026-11-17NANO & ADVANCED MATERIALS INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511027154.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-07-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing lightweight aggregates suffer from high carbon emissions due to high-temperature sintering. Furthermore, traditional concrete 3D printing faces challenges such as inconsistent material strength, uneven particle size distribution, high water absorption, and poor interlayer bonding, which affect its performance and reliability in 3D printing applications.

Method used

Lightweight synthetic aggregates are prepared using low-carbon materials such as granulated blast furnace slag and fly ash. High-temperature sintering is avoided by using geopolymer cementing materials. Combined with perlite core material and geopolymer coating layer, lightweight aggregates with low density and controllable particle size are formed. The geopolymer reaction is activated by alkaline activator to form bubbles, thereby reducing the aggregate density.

Benefits of technology

It enables the production of lightweight aggregates with low carbon emissions, improves the extrudability and structural stability of 3D printed concrete, optimizes rheological properties, enhances interlayer bonding and mechanical properties, and supports more efficient and sustainable 3D printing construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106049A_ABST
    Figure CN123106049A_ABST
Patent Text Reader

Abstract

This invention provides a low-carbon emission lightweight aggregate and a 3D-printed concrete composition containing the lightweight aggregate. Firstly, this invention provides a method for preparing a lightweight artificial aggregate for 3D printing. The method includes: mixing 25-70 parts by weight of metakaolin, 15-40 parts by weight of fly ash, 10-70 parts by weight of granulated blast furnace slag, and 0-50 parts by weight of silica fume into a geopolymer encapsulating material; then adding 6-10 parts by weight of closed-cell perlite core material to the mixed encapsulating material. 0.25-0.5 parts by weight of aluminum powder may also be added as a foaming agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to low-carbon lightweight aggregates. More specifically, this invention relates to low-carbon lightweight aggregates for 3D printing. Background Technology

[0002] Aggregate is a granular material widely used in foundations, road base courses, drainage culverts, railway track beds, and concrete fillers. Aggregates can be classified according to density into "common aggregates" (such as granite and basalt) and "lightweight aggregates" (such as pumice and volcanic slag). Common aggregates are typically obtained through mining combined with crushing operations to achieve the desired particle size. However, mining operations can damage the local environment, and mining areas are often located far from population centers that require large quantities of aggregates.

[0003] With increasing concern about the over-exploitation of natural aggregates, synthetic aggregates (including conventional and lightweight aggregates) have been developed as a new source of aggregate materials. Some synthetic aggregates are classified as lightweight aggregates, with a bulk density of less than 1200 kg / m³. Lightweight aggregates are particularly suitable for producing lightweight concrete and other lightweight building products. These products also exhibit excellent thermal insulation and sound insulation properties.

[0004] Current synthetic lightweight aggregates are mainly prepared through sintering processes using materials such as expanded clay and shale. The general steps for sintering lightweight aggregates include: mixing raw materials such as clay with water and additives; forming spherical particles of the desired size through an agglomeration process; then feeding these spherical particles directly into a rotary kiln (or sintering zone) for sintering at 1100-1200℃; and forming lightweight solid particles through particle fusion and structural expansion. However, this preparation method requires burning fuel to drive the kiln, resulting in the emission of large amounts of greenhouse gases and raising environmental concerns. It is estimated that producing one ton of lightweight aggregate emits approximately 0.3 tons of carbon dioxide.

[0005] Despite their numerous advantages, traditional lightweight aggregates still present some challenges, such as inconsistent strength, uneven particle size distribution, and high water absorption. These factors can affect the overall performance of lightweight concrete, therefore, when used in 3D printing applications, precise control over the aggregate composition and processing methods is necessary to achieve the desired mechanical properties and printability.

[0006] 3D printing of concrete (also known as additive manufacturing in the construction industry) has attracted widespread attention due to its potential for rapid construction, reduced material waste, and enhanced design flexibility. However, several challenges hinder the widespread adoption of this technology. For example, printable concrete mixes must strike a good balance between workability and molding stability. The material needs sufficient flowability to be extruded from the nozzle while maintaining shape stability after deposition. This requires precise control over mixing ratios, including the selection of cementitious materials, lightweight aggregates, and admixtures.

[0007] Furthermore, each layer of printed material must be able to support subsequent layers without excessive deformation. If the material is too fluid, it may collapse under its own weight; if it is too viscous, the interlayer bonding will be poor, easily leading to a weak structure. Therefore, optimizing the thixotropic properties of concrete is crucial for achieving structural stability. The extrusion rate, nozzle size, layer height, and printing speed must be precisely synchronized to avoid defects in the printed structure, such as voids, cracks, or uneven layer thickness.

[0008] Unlike traditional cast-in-place concrete, 3D printed concrete is printed layer by layer in a thin-layer manner, which increases the risk of shrinkage cracks due to rapid moisture evaporation. To reduce cracking and maintain the integrity of the printed component, water-reducing agents, anti-shrinkage agents, and appropriate curing techniques must be used.

[0009] The traditional concrete production process uses a large amount of ordinary silicate cement to maintain high strength, resulting in high carbon emissions. Developing and using other low-carbon materials as alternatives (such as geopolymer-based materials) and incorporating recycled materials into the mix can significantly reduce the environmental impact of 3D-printed concrete.

[0010] This invention overcomes the shortcomings of existing technologies by employing an innovative geopolymer binder, thus avoiding the high-temperature sintering process. The lightweight aggregate provided by this invention can improve the performance of 3D printed concrete compositions while achieving sustainable development. Summary of the Invention

[0011] This invention provides a low-carbon emission lightweight aggregate and a 3D-printed concrete composition containing the lightweight aggregate. In a first aspect, this invention provides a method for preparing a lightweight synthetic aggregate for 3D printing. The method includes mixing a geopolymer encapsulating material by weight: 25-70 parts metakaolin, 15-40 parts fly ash, 10-70 parts granulated blast furnace slag, and 0-50 parts silica fume, and then incorporating 6-10 parts closed-cell perlite core material by weight into the mixed encapsulating material. Additionally, 0.25-0.5 parts aluminum powder may be added as a foaming agent.

[0012] The polymer coating material, core material, and foaming agent are mixed in a granulator. An alkaline activator is sprayed during the granulation process to form near-spherical particles, and the particles are then cured to prepare lightweight synthetic aggregate.

[0013] The alkaline activator may be a mixture of potassium silicate and potassium hydroxide, or a mixture of sodium silicate and sodium hydroxide, with a mass concentration of 20-40% and a modulus range of 1.0-1.4.

[0014] The alkaline activator can be sprayed onto the powder at a mass ratio of 0.25-0.35.

[0015] The granulator rotates at a speed of 20-35 revolutions per minute.

[0016] After the granulation process is completed, the granules can be left to stand at room temperature for 24 hours.

[0017] The curing process can be carried out in an oven at 70-80°C for 12-36 hours.

[0018] After curing in the oven, it can continue to cure for 7 days in a water bath at room temperature.

[0019] After curing in a warm water bath, it can be cured again in an oven.

[0020] The aggregate can be screened to a particle size of 0.3 mm to 2.36 mm.

[0021] A 3D concrete printing composition may contain the aforementioned lightweight synthetic aggregate, for example, its dry components include: 14-40 parts by weight of lightweight synthetic aggregate, 19-35 parts by weight of ordinary Portland cement (OPC), 9-15 parts by weight of fly ash, 9-20 parts by weight of granulated blast furnace slag, 1-27 parts by weight of silica fume (SF), and 5-10 parts by weight of sand.

[0022] A 3D concrete printing mortar may include 100 parts by weight of the above-described dry concrete printing composition, plus 2-8 parts by weight of an additive mixture and 13-36 parts by weight of water. The additive mixture may include rheology modifiers, defoamers, water-reducing agents, retarders, and expanding agents.

[0023] The additive mixture comprises: 0.5-2 parts by weight of rheology modifier, 6-24 parts by weight of water-reducing agent, 3.5-10 parts by weight of defoamer, 2.5-3.5 parts by weight of retarder and 60-75 parts by weight of expander. Attached Figure Description

[0024] Embodiments of the invention are described in more detail below with reference to the accompanying drawings, in which:

[0025] Figure 1 The pelleting process of the lightweight synthetic aggregate of the present invention is illustrated schematically.

[0026] Figure 2 A photo was shown, which displayed according to Figure 1 The overall size and appearance of the lightweight synthetic aggregate formed by the process.

[0027] Figure 3 A photo was shown, which displayed Figure 2 The image shows aggregates incorporated into a 3D-printed concrete structure.

[0028] Figure 4 Examples of reactions that may occur in geopolymerization are shown. Detailed Implementation

[0029] This invention relates to a lightweight synthetic aggregate for 3D printing lightweight concrete. The lightweight aggregate incorporates low-carbon materials (such as granulated blast furnace slag (GGBS) and fly ash (PFA)), making it an environmentally friendly and sustainable product. The molding technology of this aggregate does not involve high-temperature sintering, thereby improving energy efficiency and reducing carbon emissions. When the lightweight aggregate is incorporated into 3D printable concrete mixtures, it enhances the extrudability and structural stability of the material, thus optimizing its application in additive manufacturing.

[0030] The lightweight aggregate comprises a perlite core and a lightweight polymer coating. It is made from at least 30% recycled materials by weight to achieve low carbon emissions. The polymer shell is activated by an alkaline activator, generating bubbles within the coating upon reaction with the aluminate components, thereby reducing the aggregate density. The density of this lightweight aggregate can reach 500 kg / m³. 3 Up to 700kg / m 3 between.

[0031] The core of the lightweight aggregate can be perlite. Perlite is a naturally formed volcanic glass, usually formed after obsidian (volcanic glass) is hydrated. Its main characteristic is that when rapidly heated to approximately 850–900°C, it expands to 20 times its original volume due to the water content within its structure, thus forming a lightweight, porous material. The composition of perlite is shown in Table 1 below.

[0032] Table 1: oxides Ingredient percentage (%) <![CDATA[Silicon dioxide (SiO₂)]]> 70–75% <![CDATA[Alumina (Al₂O₃)]]> 12–15% <![CDATA[Potassium oxide (K2O)]]> 3–5% Sodium oxide (Na₂O) 2–4% <![CDATA[Iron oxide (Fe₂O₃)]]> 0.5–2% Magnesium oxide (MgO) 0.1–0.5% Calcium oxide (CaO) 0.5–1.5% <![CDATA[Water (H2O)]]> 2–6% (hydrated state)

[0033] Other core materials include vermiculite (a hydrated magnesium aluminum silicate), pumice, recycled foam glass, and fly ash cenospheres.

[0034] The geopolymer coating can be formed from various geopolymer cementitious materials. The geopolymer cementitious material is an inorganic cementitious material formed by the reaction of aluminosilicate powder and an alkaline activator, creating a rigid three-dimensional polymeric network. Unlike traditional silicate cement, geopolymers rely on polymerization rather than hydration, thus exhibiting higher durability, chemical stability, and lower carbon emissions, thereby enhancing their sustainability.

[0035] Examples of geopolymers include industrial byproducts such as granulated blast furnace slag (GGBS) and fly ash (PFA), which are environmentally friendly alternatives to cement. Granulated blast furnace slag (GGBS) is a byproduct of steelmaking and is primarily composed of calcium oxide, silica, alumina, and magnesium oxide.

[0036] The typical chemical composition of GGBS (by weight percentage) is as follows:

[0037] General range of ingredients

[0038] Calcium oxide (CaO) 30–50%

[0039] 30–40% silicon dioxide (SiO2)

[0040] Alumina (Al2O3) 5–15%

[0041] Magnesium oxide (MgO) 1–10%

[0042] Iron oxide (Fe2O3) 0.5–2%

[0043] Fly ash is a byproduct of coal combustion in thermal power plants. It is rich in silicon dioxide (SiO2) and aluminum oxide (Al2O3) and can also be used as a cementing material for the polymer coating layer of this invention.

[0044] The typical chemical composition (by weight percentage) of fly ash is as follows:

[0045] Composition: F type fly ash, C type fly ash

[0046] Silica (SiO2) 40–60% 30–50%

[0047] Alumina (Al2O3) 15–30% 10–25%

[0048] Calcium oxide (CaO) <10% 10–40%

[0049] Iron oxide (Fe2O3) 5–20% 5–15%

[0050] Magnesium oxide (MgO) 1–5% 1–5%

[0051] Geopolymer materials are cured via an alkaline activation reaction. During alkaline activation, the aluminosilicate component reacts with an alkaline activator (typically sodium hydroxide (NaOH), potassium hydroxide (KOH), and / or sodium silicate (Na₂CO₃)), breaking the silicate and aluminate bonds in the raw material and dissolving it into an active state. The dissolved silicate (SiO₄) and aluminate (AlO₄) ions recombine to form a three-dimensional cross-linked geopolymer network, whose structure is similar to zeolite but amorphous.

[0052] The polymerization reaction produces sodium-based or potassium-based aluminosilicate hydrate gels (NASH or KASH), which gradually solidify into solid materials. Due to its high calcium content, GGBS can also form CSH gels. Figure 4 Examples of reactions that may occur during geopolymerization are shown.

[0053] Other components, such as metakaolin, sand, and silica fume, can also be added to the coating cementitious material. To enhance reactivity with alkaline activators, a small amount of aluminum powder can be added to the coating composition as a foaming agent, with the following reaction:

[0054] 2Al + 6H₂O → 2Al(OH)₃ + 3H₂↑

[0055] Lightweight aggregate preparation process

[0056] The preparation process of lightweight synthetic aggregate includes the following steps:

[0057] Metakaolin, fly ash, granulated blast furnace slag, and aluminum powder are mixed in a certain mass ratio to prepare a geopolymer coating material. The proportion range of each raw material is as follows:

[0058] Composition of encapsulation layers

[0059] Ingredients by weight

[0060] Granulated blast furnace slag 10–70

[0061] fly ash 15–40

[0062] Metakaolin 25–70

[0063] Silica ash 0–50

[0064] Additives 0–5

[0065] A composition for geopolymer coating materials and examples of its properties are shown in Table 2 below:

[0066] Table 2:

[0067] Then, perlite or other core materials are incorporated into the geopolymer encapsulation material at a mass ratio of approximately 1:16 to 1:10.

[0068] The core material and the wrapping material are mixed in a granulator according to the above proportions.

[0069] Figure 1 A schematic diagram of the pelleting section in the lightweight aggregate molding process is shown.

[0070] During the granulation process, an alkaline activator composed of sodium (potassium) silicate, sodium (potassium) hydroxide, and water is sprayed into the mixture to prepare spherical lightweight aggregate particles.

[0071] The spherical particles can be cured at room temperature for about 24 hours, followed by heat curing at 70°C for about 24 hours, and optionally cured in a room temperature water bath for 7 days, and finally dried at about 110°C.

[0072] The alkaline activator used in this process can be a mixture of potassium silicate and potassium hydroxide, or a mixture of sodium silicate and sodium hydroxide, with a mass concentration ranging from 20% to 40% and a modulus of 1.0 to 1.4. During granulation, the activator is sprayed at a mass ratio of 0.25 to 0.35 to ensure uniform polymerization. The granulator speed can be maintained at 20–35 rpm.

[0073] Figure 2 The resulting spherical lightweight aggregate particles are shown.

[0074] 3D Concrete Printing Using Lightweight Polymer Aggregates

[0075] Concrete used for 3D printing differs from traditional cast concrete, requiring specialized design for extrusion and layer-by-layer deposition. The formulation of printable concrete needs precise balancing of flowability and stability to ensure a smooth printing process while preventing deformation or collapse of the printed structure. Replacing traditional aggregates with lightweight aggregates in 3D printed concrete offers several advantages, including reduced density, improved thermal insulation, and enhanced sustainability.

[0076] The lightweight aggregate described in this invention offers significant advantages in 3D printing applications, enabling weight reduction of printed structures without compromising strength. Its controllable particle size distribution ensures good extrudability while maintaining the structural integrity of the printed layers. Furthermore, the geopolymer coating of the aggregate enhances its adhesion to the cementitious matrix, thereby improving the interlayer bonding strength and mechanical properties of the printed component.

[0077] The following improvements can be achieved by replacing traditional aggregates with lightweight synthetic aggregates:

[0078] Rheological property optimization: Lightweight aggregates improve the stability of printing mortar, reduce segregation, and improve fluidity.

[0079] Lower density: Lower density improves material utilization efficiency and saves energy during transportation and handling.

[0080] Sustainability: The use of recycled and low-carbon materials in aggregate production contributes to environmentally friendly construction.

[0081] Improved printing performance: Controlled particle size and surface properties of lightweight aggregates can improve extrusion accuracy and increase printing resolution.

[0082] By integrating these lightweight aggregates into 3D-printed concrete, this invention provides a material that is both structurally feasible and environmentally responsible, enabling more efficient and sustainable construction methods.

[0083] To prepare 3D printed concrete, lightweight aggregates need to be screened to a particle size range of 0.3mm to 2.36mm to ensure an apparent density of 500-700kg / m³. 3 The compressive strength is 1-2 MPa. The selected particle size range ensures that the aggregate meets the extrudability requirements of 3D printing.

[0084] The solid raw materials for 3D printed concrete consist of the following:

[0085] 14-40 parts by weight of lightweight synthetic aggregate,

[0086] 19-35 parts by weight of ordinary Portland cement (OPC),

[0087] 9-15 parts by weight of fly ash (FA),

[0088] 9-20 parts by weight of granulated blast furnace slag (GGBS),

[0089] 1-27 parts by weight of silica fume (SF),

[0090] 5-10 parts by weight of sand.

[0091] To achieve good rheological and printing properties, 3D printed concrete needs to be mixed in the following proportions:

[0092] 100 parts by weight of solid raw materials,

[0093] 2-8 parts by weight of additives,

[0094] 13-36 parts by weight of water.

[0095] Additives include:

[0096] 0.5-2 parts by weight of rheology modifier,

[0097] 6-24 parts by weight of water-reducing agent,

[0098] 3.5-10 parts by weight of defoamer,

[0099] 2.5-3.5 parts by weight of retarder,

[0100] 60-75 parts by weight of expanding agent.

[0101] The prepared 3D printing concrete mortar can be extruded using a frame-type 3D printer. The relevant extrusion parameters are as follows:

[0102] Nozzle diameter: 10–40 mm

[0103] Nozzle movement speed: 30–60 mm per second

[0104] Mortar extrusion rate: 0.5–1.0

[0105] Floor height: 10–40 mm.

[0106] Examples of additives are as follows: rheology modifiers can be thixotropic rheology modifiers based on aluminosilicates; water-reducing agents can be polycarboxylate-based water-reducing agents; defoamers can be composed of a mixture of liquid hydrocarbons, polyethylene glycol, and inorganic carriers; retarders can be polycarboxylic acids and hydroxycarboxylic acids; and expanding agents can be aluminosilicate-based expanding agents.

[0107] By combining lightweight synthetic aggregates with optimized concrete formulations, an extrudable and printable material can be obtained, characterized by its lightweight, structural stability, and environmental friendliness. Its smooth extrusion performance and controllable setting behavior enable high-quality digital construction, significantly reducing the amount of materials and carbon emissions required in traditional concrete construction. Figure 3 A 3D-printed concrete component incorporating lightweight aggregate was demonstrated.

[0108] The foregoing briefly describes several embodiments and detailed features of this disclosure. The embodiments described in this disclosure can be readily used as the basis for designing or modifying other processes and structures to achieve the same or similar purposes and / or obtain the same or similar advantages as those described in the embodiments of this disclosure. Such equivalent constructions do not depart from the spirit and scope of this disclosure, and various changes, substitutions, and modifications can be made without departing from the spirit and scope of this disclosure.

[0109] As used herein, terms such as “approximately,” “substantially,” “essentially,” and “about” are used to describe and explain minute variations. When used in conjunction with an event or situation, the term can refer to a situation where the event or situation occurs precisely, or approximately. As used herein with respect to a given value or range, the term “about” typically means within ±10%, ±5%, ±1%, or ±0.5% of the given value or range. A range can be expressed herein as from one endpoint to another or between two endpoints. Unless otherwise stated, all ranges disclosed in this disclosure include endpoints. The term “substantially coplanar” can refer to two surfaces located within a few micrometers (μm) along the same plane, such as within 10 μm, 5 μm, 1 μm, or 0.5 μm along the same plane. When referring to “substantially” identical values ​​or characteristics, the term can refer to values ​​within ±10%, ±5%, ±1%, or ±0.5% of the average value.

Claims

1. A method for preparing lightweight synthetic aggregate for 3D printing, characterized in that, include: 25-70 parts by weight of metakaolin, 15-40 parts by weight of fly ash, 10-70 parts by weight of granulated blast furnace slag (GGBS) and 0-50 parts by weight of silica fume (SF) are mixed to obtain a geopolymer encapsulation material. Add 6-10 parts by weight of closed-cell perlite core material to the geopolymer encapsulation material; 0.25-0.5 parts by weight of aluminum powder are added to the geopolymer coating material as a foaming agent; The geopolymer encapsulating material, the core material, and the foaming agent are mixed and granulated using a granulator. During the granulation process, an alkaline activator is sprayed to prepare approximately spherical particles; as well as The spherical particles are solidified to obtain the lightweight synthetic aggregate.

2. The method according to claim 1, characterized in that, The alkaline activator is selected from a mixture of potassium silicate and potassium hydroxide, or a mixture of sodium silicate and sodium hydroxide, with a mass concentration of 20-40% and a modulus range of 1.0-1.

4.

3. The method according to claim 1, characterized in that, The alkaline activator is sprayed onto the powder at a mass ratio of 0.25-0.

35.

4. The method according to claim 1, characterized in that, The granulator is said to rotate at a speed of 20-35 revolutions per minute.

5. The method according to claim 1, characterized in that, The process further includes allowing the pellet to stand at room temperature for 24 hours after the pelleting process.

6. The method according to claim 1, characterized in that, The curing process is carried out in an oven at a temperature of 70-80°C for 12-36 hours.

7. The method according to claim 1, characterized in that, The curing process also includes curing in a room temperature water bath for 7 days after curing in the oven.

8. The method according to claim 7, characterized in that, The process further includes curing in an oven after curing in the warm water bath.

9. The method according to claim 1, characterized in that, The method further includes sieving the aggregate to a particle size of 0.3 mm to 2.36 mm.

10. A 3D concrete printing composition, characterized in that, It includes the lightweight synthetic aggregate as described in claim 1.

11. The 3D concrete printing composition according to claim 10, characterized in that, This includes dry components, and the dry components include: 14-40 parts by weight of the lightweight synthetic aggregate according to claim 1; 19-35 parts by weight of ordinary Portland cement (OPC); 9-15 parts by weight of fly ash (PFA); 9-20 parts by weight of granulated blast furnace slag (GGBS); 1-27 parts by weight of silica fume (SF); and 5-10 parts by weight of sand.

12. A 3D concrete printing mortar, characterized in that, include: 100 parts by weight of the concrete printing composition according to claim 11; 2-8 parts by weight of additive mixture; as well as 13-36 parts by weight of water.

13. The 3D concrete printing mortar according to claim 12, characterized in that, The additive mixture includes: 0.5-2 parts by weight of rheology modifier; 6-24 parts by weight of water-reducing agent; 3.5-10 parts by weight of defoamer; 2.5-3.5 parts by weight of retarder; and 60-75 parts by weight of expanding agent.