Aerogel thermal insulation materials and their preparation methods

Aerogel insulation materials were prepared by physical stirring and foaming process, which solved the problems of limited product shape and poor thermal stability, and achieved high-efficiency thermal insulation performance and long life of aerogel materials.

CN123106067APending Publication Date: 2026-11-17GONG YI VAN RES INNOVATION COMPOSITE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611349912.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aerogel insulation materials suffer from limitations in product form, poor thermal stability and insulation performance, and short service life.

Method used

Aerogel insulation materials are prepared using a physical mixing foaming process. The foam is formed by mixing binder, foam stabilizer, reinforcing fiber and water. Aerogel powder is added and then cold-pressed and dried, avoiding the use of chemical foaming agents.

Benefits of technology

It improves the thermal stability and service life of aerogel insulation materials, enhances their mechanical properties and formability, and is more environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106067A_ABST
    Figure CN123106067A_ABST
Patent Text Reader

Abstract

This application provides an aerogel thermal insulation material and its preparation method. The preparation method of the aerogel thermal insulation material includes: firstly, mixing 6%-8% of binder, 1%-2% of foam stabilizer, 0.5%-2% of reinforcing fiber, and 85%-95% of water by weight to obtain a mixed slurry; then, physically stirring and foaming the mixed slurry to form a foam body; next, adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam body and mixing evenly to form an aerogel foam mixture; finally, cold-pressing and drying the aerogel foam mixture. The aerogel composite material prepared by this method has improved thermal stability and service life, and is more environmentally friendly; it also has good mechanical properties, formability, and excellent thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of aerogel technology, and in particular to an aerogel thermal insulation material and its preparation method. Background Technology

[0002] Aerogels are considered ideal insulation materials due to their extremely high porosity and extremely low thermal conductivity. However, pure aerogel materials suffer from poor mechanical properties, high brittleness, and difficulty in molding, which limits their large-scale application.

[0003] Existing technologies mainly address this issue through two approaches: one is to combine aerogel with fiber mats (such as glass fiber mats and ceramic fiber mats) to prepare flexible fiber-reinforced aerogel mats, but the product shape is limited, making it difficult to prepare irregularly shaped parts, and the bonding strength between the reinforcing fibers and aerogel is limited; the other is to combine aerogel with foaming polymers (such as polyurethane, phenolic resins, polyimide, etc.) to form foaming polymer / aerogel composite materials, but this approach may affect the thermal stability and service life of aerogel insulation materials, and the aerogel is easily damaged during the composite process, leading to a decrease in thermal insulation performance. Summary of the Invention

[0004] The aerogel thermal insulation material and its preparation method provided in this application aim to solve the problems of limited product form, poor thermal stability and thermal insulation performance, and short service life of existing aerogel thermal insulation materials.

[0005] To solve the above-mentioned technical problems, one technical solution adopted in this application is: to provide a method for preparing an aerogel thermal insulation material, comprising: Mix 6%-8% binder, 1%-2% foam stabilizer, 0.5%-2% reinforcing fiber, and 85%-95% water by weight to obtain a mixed slurry; The mixed slurry is physically stirred and foamed to form a foam body; Add 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mix evenly to form an aerogel foam mixture; The aerogel foam mixture is cold-pressed and dried.

[0006] In one specific embodiment, the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture includes: The aerogel powder is added to the foam in small amounts multiple times; and after each addition, the foam is stirred and extruded for a certain period of time.

[0007] In one specific embodiment, the step of stirring and pressing the foam for a certain period of time after each addition includes: The foam body is stirred at low speed and then extruded by roller pressing and repeated multiple times; wherein the stirring speed of the low speed stirring is 300-500 r / min, the stirring time is 1-2 min, and the roller pressing time is 30 s-1 min.

[0008] In one specific embodiment, the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture includes: The aerogel powder is formed by in-situ doping with a light-blocking agent; the aerogel powder includes a light-blocking agent-doped silica composite aerogel; and / or... After the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture, the method further includes: A light-blocking agent is added to the aerogel foam mixture; the aerogel powder comprises silica aerogel. The mass ratio of silicon dioxide to the light-blocking agent is 6:4-8:2.

[0009] In one specific embodiment, the aerogel powder includes aerogel particles with a particle size of 5-50 μm and aerogel particles with a particle size of 50-100 μm; and the mass fraction of aerogel particles with a particle size of 5-50 μm is 60%-80%.

[0010] In one specific embodiment, the step of physically stirring and foaming the mixed slurry includes: The mixed slurry is foamed by gradually increasing the stirring speed; wherein the stirring speed increases gradually between a first stirring speed and a second stirring speed; the first stirring speed is 500-700 r / min, the second stirring speed is 1100-1300 r / min; the gradient of stirring speed is 200-400 r / min, and the stirring time of each gradient is 2-3 min.

[0011] In one specific embodiment, the foam density of the foam body is 0.08–0.12 g / cm³; the average diameter of the foam body is less than or equal to 200 μm.

[0012] In one specific embodiment, the step of cold-pressing and drying the aerogel foam mixture includes: The aerogel foam mixture is pressurized by gradually increasing the pressure, and after depressurization, the mold is kept closed for 3-5 minutes before demolding; wherein the pressurization pressure is gradually increased between a first pressure and a second pressure; the first pressure is 0.4-0.6 MPa, and the second pressure is 1.4-1.6 MPa; the pressurization time is 1-3 minutes; and the pressure gradient is 0.2-0.5 MPa. The aerogel foam mixture is dried under normal pressure; wherein the drying temperature is 55-65℃ and the drying time is 5-7h.

[0013] In one specific embodiment, the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture further includes: The surface of the aerogel powder was modified and pretreated using 0.2%-1% silane coupling agent.

[0014] In one specific embodiment, the reinforcing fiber comprises long fibers and short fibers in a mass ratio of 6:4 to 8:2; the long fibers have a length of 4-8 mm, and the short fibers have a length of 2-4 mm.

[0015] In one specific embodiment, the step of uniformly mixing 6%-8% of binder, 1%-2% of foam stabilizer, 0.5%-2% of reinforcing fiber, and 85%-95% of water by weight to obtain a mixed slurry specifically includes: A mixed solution is obtained by mixing 6%-8% of the adhesive, 1%-2% of the foam stabilizer, and 85%-95% of the water by weight. The reinforcing fiber, at a mass percentage of 0.5%-2%, is added to the mixed solution and stirred until homogeneous to obtain the mixed slurry.

[0016] To solve the above-mentioned technical problems, another technical solution adopted in this application is: providing a method for preparing an aerogel thermal insulation material, comprising: A mixed slurry is provided; the mixed slurry includes a solvent, a binder, a foam stabilizer, and a reinforcing material, but does not contain a foaming agent; The mixed slurry is stirred and foamed to form a foam body; Aerogel powder is added to the foam and mixed to form an aerogel foam mixture; The aerogel foam mixture is cold-pressed and dried.

[0017] To solve the above-mentioned technical problems, another technical solution adopted in this application is: to provide an aerogel thermal insulation material, wherein the aerogel thermal insulation material is prepared by the preparation method of aerogel thermal insulation material as described in any one of the above-mentioned methods.

[0018] To solve the above-mentioned technical problems, another technical solution adopted in this application is: to provide an aerogel thermal insulation material, wherein the aerogel thermal insulation material does not contain a foaming agent; by mass percentage, the aerogel thermal insulation material comprises the following components: 8%-14% binder, 1%-3% foam stabilizer, 0.5%-1.5% reinforcing fiber and 80%-90% aerogel powder.

[0019] The beneficial effects of this application's embodiments are as follows: Unlike existing technologies, this application provides a method for preparing aerogel thermal insulation materials. This method involves first uniformly mixing 6%-8% binder, 1%-2% foam stabilizer, 0.5%-2% reinforcing fiber, and 85%-95% water by weight to obtain a mixed slurry. Then, the mixed slurry is physically stirred and foamed to form a foam body. Next, 17-21 parts by weight of aerogel powder are added to 33-37 parts by weight of the foam body and mixed uniformly to form an aerogel foam mixture. Finally, the aerogel foam mixture is cold-pressed and dried. By using a physical stirring foaming process instead of chemical foaming, the adverse effects of residual chemical foaming agents on the aerogel thermal insulation material are eliminated, effectively improving the thermal stability and service life of the aerogel thermal insulation material, and making it more environmentally friendly. Attached Figure Description

[0020] Figure 1 This is a schematic flowchart illustrating the preparation method of the aerogel thermal insulation material provided in the first embodiment of this application; Figure 2 This is a schematic flowchart illustrating the preparation method of the aerogel thermal insulation material provided in the second embodiment of this application; Figure 3 This is a schematic diagram of the structure of an aerogel insulation material provided in an embodiment of this application. Detailed Implementation

[0021] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0022] The terms "first," "second," and "third" in this application are for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first," "second," or "third" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified. All directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of this application are only used to explain the relative positional relationships and movements between components in a specific orientation (as shown in the figures). If the specific orientation changes, the directional indications also change accordingly. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or device that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products, or devices.

[0023] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0024] Aerogels are considered ideal insulation materials due to their extremely high porosity and extremely low thermal conductivity. However, pure aerogel materials suffer from poor mechanical properties, high brittleness, and difficulty in molding, which limits their large-scale application. Existing technologies mainly address this through two approaches: one is to composite aerogels with fiber mats (such as glass fiber mats and ceramic fiber mats) to prepare flexible fiber-reinforced aerogel mats, but the product shape is limited, making it difficult to prepare irregularly shaped parts, and the bonding strength between the reinforcing fibers and aerogels is limited; the other is to composite aerogels with foaming polymers (such as polyurethane, phenolic resins, polyimide, etc.) to form foamed polymer / aerogel composite materials, but this method relies on chemical foaming agents or surfactants, increasing costs and environmental burden. Foaming agent residues may affect thermal stability and lifespan, and the aerogel is easily damaged during the composite process, leading to a decrease in insulation performance.

[0025] Based on this, the present application provides a method for preparing aerogel composite materials. The aerogel composite materials prepared by this method have improved thermal stability and service life, and are more environmentally friendly; they also have good mechanical properties, formability, and excellent thermal insulation properties.

[0026] The present application will now be described in detail with reference to the accompanying drawings and embodiments.

[0027] See Figure 1 , Figure 1 This is a schematic flowchart illustrating the preparation method of the aerogel thermal insulation material provided in the first embodiment of this application. This application provides a method for preparing an aerogel thermal insulation material. The specific steps of this method may include: Step S1: Mix 6%-8% of binder, 1%-2% of foam stabilizer, 0.5%-2% of reinforcing fiber, and 85%-95% of water by weight to obtain a mixed slurry.

[0028] In the specific implementation process, the binder, foam stabilizer, and water can be mixed evenly to form a mixed solution before adding the reinforcing fibers. This liquid-to-solid mixing method allows the reinforcing fibers to be more evenly dispersed in the viscous medium composed of the binder and foam stabilizer, avoiding fiber agglomeration. Specifically, step S1 may include: Step S11: Mix 6%-8% of the adhesive, 1%-2% of the foam stabilizer, and 85%-95% of the water by mass percentage to obtain a mixed solution.

[0029] The binder is used to form a polymer matrix network to provide continuous phase support, thereby improving the mechanical properties of the aerogel insulation material and reducing its brittleness. The binder also encapsulates and bonds the aerogel powder to prevent powder shedding. Specifically, the mass percentage of the binder can be any value from 6%, 6.5%, 7%, 7.5%, and 8%; preferably, the mass percentage of the binder is 7%.

[0030] Foam stabilizers have high viscosity properties and are used to stabilize bubbles in subsequent foaming steps, preventing bubbles from breaking or merging during the foaming process. Specifically, the mass percentage of the foam stabilizer can be any value among 1%, 1.2%, 1.5%, 1.8%, and 2%; preferably, the mass percentage of the foam stabilizer is 1.5%.

[0031] Water is used as a solvent to uniformly disperse the binder and foam stabilizer in the mixed solution. Specifically, the mass percentage of water can be any value among 85%, 88%, 90%, 91%, 92%, and 95%; preferably, the mass percentage of water is 91%.

[0032] The binder can specifically include polyvinyl alcohol (PVA), and the foam stabilizer can include sodium carboxymethyl cellulose (CMC). PVA provides film-forming properties and primary adhesive strength, while CMC provides thickening and foam-stabilizing effects. Thus, by employing a two-component system of "PVA + sodium carboxymethyl cellulose," the system can generate bubbles through physical stirring without containing a foaming agent. The high viscosity of CMC stabilizes these bubbles, improving their stability and allowing the foam to disperse more aerogel powder.

[0033] Step S12: Add 0.5%-2% by weight of reinforcing fiber to the mixed solution and stir evenly to obtain a mixed slurry.

[0034] In this process, reinforcing fibers act as a reinforcing skeleton, providing crack resistance and reducing shrinkage deformation during subsequent drying. Furthermore, the reinforcing fibers, combined with binders and foam stabilizers, endow the aerogel insulation material with excellent mechanical properties and moldability, overcoming the drawbacks of pure aerogel such as high brittleness and difficulty in molding. The reinforcing fibers can specifically include glass fibers, quartz fibers, or ceramic fibers. Specifically, the mass percentage of reinforcing fibers can be any value from 0.5%, 0.8%, 1%, 1.5%, and 2%; this avoids excessive reinforcing fiber content affecting the thermal insulation performance of the aerogel insulation material, while also preventing insufficient reinforcing fiber content from reducing the toughness of the aerogel insulation material and making it prone to cracking.

[0035] Specifically, the reinforcing fibers can include long fibers and short fibers in a mass ratio of 6:4 to 8:2. Long fibers primarily provide skeletal support, offering the main tensile strength and inhibiting macroscopic crack propagation; short fibers fill the gaps formed by the long fibers, increasing the contact points and frictional resistance between fibers, which helps to evenly distribute stress, thereby further improving the skeletal strength and crack resistance of the aerogel insulation material. Furthermore, the combination of long and short fibers also helps to further reduce the shrinkage deformation of the aerogel insulation material during the drying process, resulting in better dimensional stability and a lower risk of cracking.

[0036] The specific mass ratio of long fibers to short fibers can be any of 6:4, 7:3, or 8:2. This means that in reinforcing fibers, the mass percentage of long fibers is between 60% and 80%, while the mass percentage of short fibers is between 20% and 40%.

[0037] In the specific implementation process, long fibers can be added to the mixed solution for preliminary dispersion first, and then short fibers can be added for mixing; or long and short fibers can be premixed and then added to ensure uniform distribution in the matrix.

[0038] Specifically, the length of long fibers is 4-8 mm, and the length of short fibers is 2-4 mm. It is understandable that excessively long fibers may lead to agglomeration and processing difficulties, while excessively short fibers cannot form effective long-range connections. Controlling the length of reinforcing fibers within this specific range can balance processing flowability and the mechanical properties of the final material.

[0039] Specifically, the length of the long fibers can be any value among 4mm, 5mm, 6mm, 7mm, and 8mm; the length of the short fibers can be any value among 2mm, 2.5mm, 3mm, 3.5mm, and 4mm.

[0040] Step S2: Physically stir and foam the mixed slurry to form a foam body.

[0041] Physical mixing foaming refers to the process of introducing air into the mixed slurry through mechanical shearing force to form foam, rather than relying on chemical foaming agents. By replacing chemical foaming with physical mixing foaming technology, the adverse effects of residual chemical foaming agents on aerogel insulation materials are eliminated, effectively improving the thermal stability and service life of aerogel insulation materials, and making them more environmentally friendly.

[0042] Furthermore, the foam formed by physical stirring and foaming creates micron-sized air bubbles during the subsequent drying process, which, together with the nano-sized aerogel pores, form a hierarchical porous structure, further improving the thermal insulation efficiency and resulting in a final product with excellent thermal insulation performance. Specifically, during the drying process, some of the foam collapses to form an open-cell structure, while the remaining foam retains to form a closed-cell structure.

[0043] In the specific implementation process, step S2 may include: Step S21: The mixed slurry is foamed by gradually increasing the stirring speed.

[0044] The stirring speed increases sequentially between the first stirring speed and the second stirring speed, where the first stirring speed is the initial speed of the foaming process and the second stirring speed is the final speed.

[0045] Specifically, the first stirring speed is 500-700 r / min; this speed range is sufficient to introduce air to form initial bubble nuclei, while avoiding excessive shear force that would cause premature rupture or coalescence of bubbles in the viscous slurry composed of polyvinyl alcohol and sodium carboxymethyl cellulose. The first stirring speed is any value among 500 r / min, 550 r / min, 600 r / min, 650 r / min, and 700 r / min.

[0046] The second stirring speed is 1100-1300 r / min; this speed range provides sufficient shear force to further refine the bubbles, making the bubble diameter smaller, thereby forming a dense and uniform foam structure. The second stirring speed is any value among 1100 r / min, 1150 r / min, 1200 r / min, 1250 r / min, and 1300 r / min.

[0047] The stirring speed gradient is 200-400 r / min; this allows the stirring speed to transition from low to high in a segmented, stepwise manner, thus avoiding the impact of abrupt speed changes on the foam structure and ensuring that the bubbles are stably encapsulated by the polymer matrix during growth. Specifically, the stirring speed gradient can be any value among 200 r / min, 250 r / min, 300 r / min, 350 r / min, and 400 r / min.

[0048] In addition, by controlling the stirring time of each gradient to 2-3 minutes, polyvinyl alcohol and sodium carboxymethyl cellulose in the mixed slurry have sufficient time to respond to changes in shear force, further stabilizing the bubble walls and improving the overall stability of the foam.

[0049] For example, in the specific implementation process, the mixed slurry can be initially stirred at a first stirring speed of 600 r / min for 3 minutes to form bubble nuclei in the mixed slurry; then, the mixed slurry containing bubble nuclei can be further stirred at a stirring speed of 1000 r / min for 3 minutes to refine the bubbles; finally, a second stirring speed of 1200 r / min can be used for stirring for 3 minutes to make the bubble diameter smaller, thereby forming a dense and uniform foam structure.

[0050] Thus, by gradually increasing the stirring speed during foaming, the bubbles are subjected to controllable shear forces during formation, which helps to form a bubble structure with smaller diameter and more uniform distribution, avoiding bubble rupture or uneven size caused by sudden speed changes. This precise speed control allows the subsequently introduced aerogel powder to be more evenly dispersed in the stable foam skeleton, reducing local agglomeration, which helps to lower the thermal conductivity of the aerogel insulation material and improve its insulation uniformity.

[0051] In practical implementation, the foam density of the foam body is 0.08–0.12 g / cm³, ensuring that the foam skeleton has suitable strength and porosity. This avoids structural collapse due to excessively low density or molding difficulties due to excessively high density, and facilitates the uniform dispersion of the subsequent aerogel powder. Specifically, the foam density of the foam body can be any value among 0.08 g / cm³, 0.09 g / cm³, 0.1 g / cm³, 0.11 g / cm³, and 0.12 g / cm³.

[0052] Specifically, the foam density can be calculated by measuring the mass of the raw material and the volume of the foam formed in the measuring instrument, and then substituting the values ​​into the density calculation formula.

[0053] The average diameter of the foam is less than or equal to 200 μm. This results in a finer and more uniform distribution of bubbles within the foam, reducing localized stress concentration and helping to maintain the integrity of the material structure during cold pressing, thus reducing the risk of cracking. Specifically, the average foam diameter can be any value among 50 μm, 100 μm, 150 μm, and 200 μm. It can be understood that the average foam diameter refers to the arithmetic mean of the diameters of all bubbles in the foam.

[0054] Specifically, the average diameter of the foam can be controlled by adjusting the stirring speed; for example, the average diameter of the foam can be further reduced by increasing the second stirring speed, or the average diameter of the foam can be increased by decreasing the second stirring speed.

[0055] The fine and uniform bubble structure also allows the aerogel powder to be more evenly dispersed in the micron-sized bubble pores, avoiding the agglomeration of aerogel, thereby further improving the uniformity of the internal thermal insulation structure of the aerogel thermal insulation material, resulting in a more stable thermal insulation performance and mechanical properties in the final product.

[0056] Step S3: Add 17-21 parts by weight of aerogel powder to 33-37 parts by weight of foam and mix evenly to form an aerogel foam mixture.

[0057] Specifically, the aerogel powder can be silica aerogel, used as the core thermal insulation filler. By adopting a process sequence of first forming a foam skeleton and then introducing the aerogel powder, the structural damage to the aerogel powder during the vigorous foaming process is reduced, the integrity of its nanoporous structure is maintained, and the thermal insulation performance is effectively improved.

[0058] Specifically, the aerogel powder can be any of 17, 18, 19, 20, or 21 parts by weight. The foam can be any of 33, 34, 35, 36, or 37 parts by weight; preferably, the foam is 35 parts by weight.

[0059] Specifically, aerogel powder can include aerogel particles with a particle size of 5-50 μm and aerogel particles with a particle size of 50-100 μm. That is, aerogel powder includes two types of aerogel particles: the first type consists of small particles with a particle size in the range of 5-50 μm, and the second type consists of large particles with a particle size in the range of 50-100 μm. This allows the small particles to effectively fill the gaps between the large particles, thereby increasing the packing density of the aerogel in the composite material and thus helping to reduce macroscopic pore defects inside the material.

[0060] It is understandable that small particles, due to their smaller size and larger specific surface area, can more tightly wrap around large particles and fill the macroscopic gaps between them, while large particles form the main thermal insulation skeleton, preventing the material from becoming overly dense.

[0061] Among them, the mass fraction of aerogel particles with a particle size of 5-50μm is 60%-80%, that is, the mass fraction of aerogel particles with a particle size of 50-100μm is 20%-40%. This allows the material to maintain sufficient porosity to exert the aerogel nano-insulation effect while optimizing the contact network between particles, making the aerogel particles more uniformly distributed in the matrix. This is conducive to forming a continuous and stable insulation barrier, reducing the local thermal bridging effect caused by particle agglomeration or excessively large pores, thereby further reducing the overall thermal conductivity of the material and improving the insulation uniformity.

[0062] Preferably, the mass fraction of aerogel particles with a particle size of 5-50 μm is 70%, that is, the mass fraction of aerogel particles with a particle size of 50-100 μm is 30%.

[0063] Specifically, in the first type of aerogel particles, the particle size of small particles is normally distributed in the range of 5-50 μm; in the second type of aerogel particles, the particle size of large particles is normally distributed in the range of 50-100 μm.

[0064] In the specific implementation process, step S3 may include: Step S31: Aerogel powder is formed by in-situ doping with a light-blocking agent; the aerogel powder includes a light-blocking agent-doped silica composite aerogel.

[0065] In-situ doping with opaque agents refers to the process of directly introducing opaque agents as dopants into the precursor solution of aerogel during the preparation of aerogel powder. Subsequently, through conventional aerogel preparation processes such as sol-gel and supercritical drying, the opaque agent particles are uniformly dispersed and fixed inside the nanoporous framework of silica aerogel, forming opaque agent-doped silica composite aerogel.

[0066] It is understandable that the uniform distribution of the light-blocking agent within the nanopores helps to maximize the infrared absorption path at the microscale, thereby improving the overall heat insulation efficiency. Thus, by in-situ doping with the light-blocking agent, the aerogel composite material further enhances its ability to block infrared radiation heat while suppressing heat conduction and convection.

[0067] The mass ratio of silica to the opacifier is 6:4-8:2. This helps to maintain the low thermal conductivity of the aerogel matrix while providing optimal infrared absorption enhancement, avoiding increased density and thermal conductivity due to excessive opacifier. Specifically, the mass ratio of silica to opacifier can be any of 6:4, 7:3, or 8:2. Preferably, the mass ratio of silica to opacifier is 7:3.

[0068] Specifically, the light-blocking agent can be a material with high infrared absorption and scattering capabilities, such as silicon carbide and carbon black; these materials can effectively block the penetration of infrared radiation, thereby reducing the heat transfer of the material. Among them, silicon carbide is preferred as the light-blocking agent.

[0069] Step S32: Add aerogel powder to the foam in small amounts multiple times; and stir and press the foam for a certain period of time after each addition.

[0070] In the specific implementation process, the method of adding aerogel powder in small batches multiple times refers to adding the total amount of 17 to 21 parts of aerogel powder in multiple batches in sequence, for example, it can be added in 4 to 5 times, in order to avoid the local accumulation and agglomeration of aerogel powder caused by adding it all at once, so that the aerogel powder is more evenly dispersed in the foam, which is conducive to forming a continuous and stable thermal insulation network.

[0071] After each addition, the foam is stirred and extruded for a certain period of time. This mechanical force further disrupts the van der Waals forces between the aerogel powders, promoting their embedding into the micron-sized pores of the foam framework. This results in greater dispersion of the aerogel powder within the foam and reduced agglomeration. Stirring aims to initially disperse the aerogel powder within the foam framework, while extrusion forces the foam to deform using external mechanical force. Utilizing the viscoelasticity and interconnectivity of the foam's internal pores, the aerogel powder is pressed into the foam framework, further breaking up any potential agglomerates. Specifically, the stirring and extrusion time can be any value from 4 minutes, 5 minutes, or 6 minutes.

[0072] In the specific implementation process, the foam can be stirred and extruded in the following way: the foam is stirred at low speed and then extruded by roller pressing and repeated multiple times. This ensures that the aerogel powder is evenly dispersed and deeply compacted each time it is added, which helps to eliminate local concentration gradients and makes the aerogel distribution inside the final aerogel insulation material more uniform. This reduces the heat conduction channels caused by agglomeration, which helps to further reduce the overall thermal conductivity of the material.

[0073] The low-speed stirring is conducted at a speed of 300-500 r / min, ensuring that the shear force generated during stirring is within a moderate range. This helps protect the foam skeleton structure formed by polyvinyl alcohol and sodium carboxymethyl cellulose, thus maintaining the porous morphology and gas retention capacity of the foam. Specifically, the low-speed stirring speed can be any value among 300 r / min, 350 r / min, 400 r / min, 450 r / min, and 500 r / min.

[0074] The low-speed stirring time is 1-2 minutes to ensure that the aerogel powder has sufficient time to transition from the surface to the interior of the foam, achieving a macroscopically uniform distribution. Specifically, the low-speed stirring time can be any value among 1 minute, 1.5 minutes, and 2 minutes.

[0075] The rolling time is 30s-1min; this allows the aerogel powder to be fully embedded in the micron-sized pores of the foam skeleton under mechanical extrusion, reducing the free state of aerogel particles in the matrix. Specifically, the rolling time can be any value among 30s, 40s, 45s, 50s, and 1min.

[0076] In the specific implementation process, before step S3, the following may be included: pre-treating the surface of the aerogel powder with 0.2%-1% silane coupling agent.

[0077] Among them, silane coupling agents are a class of compounds containing organic functional groups and hydrolyzable groups. Their molecular structure usually contains two different reactive groups: one end is a hydrolyzable alkoxy or chlorine group, which can undergo condensation reaction with hydroxyl groups on the surface of inorganic materials; the other end is an organic functional group, such as amino, epoxy, vinyl, etc., which can undergo chemical reaction or physical entanglement with organic polymers.

[0078] During pretreatment, the silanol groups on the surface of the aerogel powder undergo a condensation reaction with the hydrolysis products of the silane coupling agent, forming a monolayer or multilayer organic film on the surface of the aerogel particles. This enhances the interfacial bonding between the aerogel powder and the polymer matrix composed of polyvinyl alcohol, sodium carboxymethyl cellulose, and reinforcing fibers during subsequent mixing and molding. The improved interfacial bonding results in more uniform stress transmission within the composite material, reducing the generation of microcracks caused by interfacial debonding, thereby improving the overall structural integrity and mechanical strength of the material.

[0079] Specifically, KH-550 (γ-aminopropyltriethoxysilane) can be selected as the silane coupling agent. The concentration of the silane coupling agent can be any value among 0.2%, 0.5%, 0.8%, and 1%; preferably, the concentration of the silane coupling agent is...

[0080] Of course, in other embodiments, a physical mixing method can also be used, that is, after the foam is formed, a separate light-blocking agent powder is added to the aerogel foam mixture containing silica aerogel powder. Specifically, after step S3, the method may further include: adding a light-blocking agent to the aerogel foam mixture; the aerogel powder comprising silica aerogel.

[0081] Specifically, the opacifier powder can be uniformly dispersed in the aerogel foam mixture using high-speed shear stirring or ultrasonic dispersion methods, ensuring that the opacifier particles coat or adhere to the surface and pore inlets of the silica aerogel particles. Specifically, the opacifier powder is added after the foam has been fully dispersed and coated with the aerogel powder to avoid the opacifier absorbing water and affecting the foam volume, thus preventing insufficient dispersion of the aerogel powder.

[0082] Step S4: Cold press the aerogel foam mixture and dry it.

[0083] Specifically, cold pressing refers to applying pressure to an aerogel foam mixture at room temperature or low temperature to shape it. A 100mm x 100mm mold can be used to cold press the aerogel foam mixture at a temperature of 10-35℃. Specifically, the cold pressing temperature can be any value from 10℃, 15℃, 20℃, 25℃, 30℃, or 35℃.

[0084] The drying process is used to remove moisture from the aerogel foam mixture to form micron-sized air bubbles.

[0085] In the specific implementation process, step S4 may include: Step S41: Pressurize the aerogel foam mixture by gradually increasing the pressure, and keep the mold closed for 3-5 minutes after depressurization before demolding; wherein, the pressure is gradually increased between the first pressure and the second pressure.

[0086] Specifically, the method of gradually increasing pressure refers to increasing the pressure from the first pressure to the second pressure in stages. After depressurization, the mold is kept closed for 3 to 5 minutes before demolding. This utilizes the constraint of the mold to allow the aerogel insulation material to slowly relax under residual stress, reducing cracking or deformation caused by elastic rebound and improving the structural integrity and dimensional stability of the product.

[0087] The first pressure is 0.4-0.6 MPa. This low-pressure stage is mainly used for preliminary compaction of the mixture, allowing the aerogel powder to initially adhere to the polymer matrix in the foam, while avoiding the possibility of the fragile aerogel powder breaking due to high pressure. Specifically, the first pressure can be any value among 0.4 MPa, 0.45 MPa, 0.5 MPa, 0.55 MPa, and 0.6 MPa.

[0088] The second pressure is 1.4-1.6 MPa; this high-pressure stage is used for final shaping, eliminating most macroscopic pores and improving the material density uniformity and surface smoothness. Specifically, the second pressure can be any value among 1.4 MPa, 1.45 MPa, 1.5 MPa, 1.55 MPa, and 1.6 MPa.

[0089] The pressurization time is 1-3 minutes to ensure sufficient time for plastic deformation and particle rearrangement in each pressure stage. Specifically, the pressurization time can be any value among 1 minute, 1.5 minutes, 2 minutes, 2.5 minutes, and 3 minutes.

[0090] The pressure gradient is 0.2-0.5 MPa; the pressure gradient refers to the difference between two adjacent pressure stages. A smaller gradient helps to ensure smooth pressure transmission and prevents local stress concentration that could cause internal cracks in the material. Specifically, the pressure gradient can be any value among 0.2 MPa, 0.3 MPa, 0.4 MPa, and 0.5 MPa.

[0091] For example, in the specific implementation process, the aerogel foam mixture can be pressurized with a first pressure of 0.5 MPa and held for 1 minute to allow the aerogel powder to initially adhere to the polymer matrix in the foam; then, the pressure can be continued to be increased with 1 MPa and held for 1 minute; finally, the pressure can be continued to be increased with a second pressure of 1.5 MPa for 1 minute to improve the uniformity of material density and surface smoothness.

[0092] By gradually increasing the pressure, the pressure transmission is made stable, avoiding the impact and breakage of aerogel particles by instantaneous high pressure, thus preserving more intact nanopores, which is beneficial to reducing the thermal conductivity.

[0093] Step S42: Dry the aerogel foam mixture under normal pressure.

[0094] Specifically, in this embodiment, the aerogel foam mixture is dried under normal pressure. The combination of cold pressing and normal pressure drying processes is beneficial for forming a multi-level porous structure containing micron-sized air bubbles and nano-sized aerogel pores. This structure further improves the thermal insulation efficiency of the aerogel insulation material, resulting in a final product with excellent thermal insulation performance and good flexibility.

[0095] The drying temperature is 55-65℃ to ensure sufficient evaporation of moisture while avoiding thermal damage to the polymer matrix and the internal structure of the aerogel powder. This allows the aerogel insulation material to maintain a high aerogel content while possessing good mechanical strength and thermal insulation performance. Specifically, the drying temperature can be any value among 55℃, 58℃, 60℃, 62℃, and 65℃.

[0096] The drying time is 5-7 hours to ensure complete removal of moisture. Specifically, the drying time can be any value among 5 hours, 5.5 hours, 6 hours, 6.5 hours, and 7 hours.

[0097] This application provides a method for preparing an aerogel thermal insulation material. The method involves first mixing 6%-8% binder, 1%-2% foam stabilizer, 0.5%-2% reinforcing fiber, and 85%-95% water by weight to obtain a slurry. Then, the slurry is physically stirred and foamed to form a foam body. Next, 17-21 parts by weight of aerogel powder are added to 33-37 parts by weight of the foam body and mixed evenly to form an aerogel foam mixture. Finally, the aerogel foam mixture is cold-pressed and dried. By using a physical stirring foaming process instead of chemical foaming, the adverse effects of residual chemical foaming agents on the aerogel thermal insulation material are eliminated, effectively improving the thermal stability and service life of the aerogel thermal insulation material, and making it more environmentally friendly. It also facilitates the formation of a multi-level porous structure containing micron-sized air bubbles and nano-sized aerogel pores, further improving the thermal insulation efficiency and resulting in a final product with excellent thermal insulation performance. Furthermore, the process sequence of first forming the foam skeleton and then introducing the aerogel powder reduces damage to the nanoporous structure of the aerogel powder, effectively improving thermal insulation performance. The synergistic effect of the binder and foam stabilizer improves the stability of the bubbles, allowing the foam to disperse more aerogel powder; combined with reinforcing fibers that provide skeletal support, the aerogel insulation material possesses excellent mechanical properties and formability, overcoming the shortcomings of pure aerogel, such as high brittleness and difficulty in molding.

[0098] See Figure 2 , Figure 2This is a schematic flowchart illustrating the preparation method of the aerogel thermal insulation material provided in the second embodiment of this application. The second embodiment of this application provides a method for preparing an aerogel thermal insulation material, specifically including: Step S10: Provide a mixed slurry; the mixed slurry includes a solvent, binder, foam stabilizer and reinforcing material, but does not contain a foaming agent.

[0099] Step S20: Stir and foam the mixed slurry to form a foam body.

[0100] Step S30: Add aerogel powder to the foam and mix to form an aerogel foam mixture.

[0101] Step S40: Cold press the aerogel foam mixture and dry it.

[0102] The specific implementation process of the above steps is the same as or similar to the preparation method of the aerogel thermal insulation material provided in the first embodiment of this application. No foaming agent is added in the whole process, and the foaming is achieved only by physical stirring. For details, please refer to the first embodiment of this application, which will not be repeated here.

[0103] See Figure 3 , Figure 3 This is a schematic diagram of the structure of an aerogel insulation material provided in one embodiment of this application; this application also provides an aerogel insulation material, which is prepared by the preparation method of the aerogel insulation material involved in any of the above embodiments.

[0104] Specifically, this aerogel insulation material is free of foaming agents, eliminating the adverse effects of residual chemical foaming agents on aerogel insulation materials. This effectively improves the thermal stability and service life of the aerogel insulation material and is more environmentally friendly. By weight percentage, the aerogel insulation material comprises the following components: 8%-14% binder, 1%-3% foam stabilizer, 0.5%-1.5% reinforcing fibers, and 80%-90% aerogel powder. This aerogel insulation material possesses excellent mechanical properties and moldability, overcoming the shortcomings of pure aerogel, such as high brittleness and difficulty in molding.

[0105] Among them, common component analysis methods such as high performance liquid chromatography and headspace gas chromatography can be used to analyze the composition of aerogel insulation materials; these methods can detect the various components and approximate proportions of aerogel insulation materials, and can detect whether aerogel insulation materials contain foaming agents.

[0106] In a specific embodiment, the reinforcing fiber may include long fibers and short fibers in a mass ratio of 6:4 to 8:2; specifically, the mass ratio of long fibers to short fibers may be any one of 6:4, 7:3, or 8:2.

[0107] The long fibers have a length of 4-8mm, and the short fibers have a length of 2-4mm. Specifically, the length of the long fibers can be any value among 4mm, 5mm, 6mm, 7mm, and 8mm; the length of the short fibers can be any value among 2mm, 2.5mm, 3mm, 3.5mm, and 4mm.

[0108] In a specific embodiment, the aerogel powder may include aerogel particles with a particle size of 5-50 μm and aerogel particles with a particle size of 50-100 μm. The mass fraction of aerogel particles with a particle size of 5-50 μm is 60%-80%, and the mass fraction of aerogel particles with a particle size of 50-100 μm is 20%-40%. Specifically, the particle size of the small particles exhibits a normal distribution within the 5-50 μm range; and the particle size of the large particles exhibits a normal distribution within the 50-100 μm range.

[0109] In a specific embodiment, the aerogel insulation material may further include a light-blocking agent; the aerogel powder may be silica aerogel. The mass ratio of silica to the light-blocking agent is 6:4-8:2; specifically, the mass ratio of silica to the light-blocking agent may be any one of 6:4, 7:3, or 8:2.

[0110] Specifically, the light-blocking agent can be incorporated into silica aerogel to form a light-blocking agent-doped silica composite aerogel, or it can be dispersed independently in the aerogel insulation material. Specifically, the light-blocking agent can be silicon carbide or carbon black; preferably, the light-blocking agent is silicon carbide.

[0111] In specific embodiments, the aerogel insulation material may also include a silane coupling agent.

[0112] The present invention will be described in more detail below with reference to the embodiments and comparative examples. However, the embodiments and comparative examples provided below are merely illustrative of the present application, and the scope of the present application is not limited thereto.

[0113] Example 1A Step S1: Preparation of the mixed slurry: First, mix 7% polyvinyl alcohol, 1.5% sodium carboxymethyl cellulose, and 91% water by mass percentage to obtain a mixed solution; then add 0.5% glass fiber by mass percentage to the mixed solution and stir evenly to obtain the mixed slurry. The glass fiber is a single-length fiber; specifically, it can be a long fiber with a length of 4-8 mm.

[0114] Step S2: Physically stir and foam the mixed slurry until the foam is dense to form a foam body; wherein, the stirring speed is fixed at 1000 r / min and the stirring time is 9 min.

[0115] Step S3: Add 16 parts by weight of silica aerogel to 35 parts by weight of foam and mix evenly by stirring and extrusion to form an aerogel-foam mixture; wherein the silica aerogel is mainly composed of large-diameter particles, specifically including silica aerogel particles with a diameter of 50-100 μm. Specifically, the particle size of the silica aerogel particles exhibits a normal distribution within the range of 50-100 μm.

[0116] Among them, silica aerogel is a hydrophobic aerogel. Specifically, hydrophobic aerogels are produced by surface modification of silica aerogels using hydrophobic agents, aiming to endow silica aerogels with excellent hydrophobic properties through chemical modification. This type of hydrophobic treatment can effectively reduce the surface energy of aerogel particles, thereby enabling them to repel moisture and prevent water absorption, ensuring the structural stability and thermal insulation performance of aerogel insulation materials during preparation and application.

[0117] Hydrophobic agents can specifically include various organosilicon compounds such as trimethylchlorosilane, methyltrimethoxysilane, hexamethyldisilazane, and hexamethyldisiloxane. These hydrophobic agents can chemically react with the silanol groups (-SiOH) on the surface of the aerogel, such as through silanization, thereby forming a stable hydrophobic organic layer on the particle surface, achieving a fundamental transformation from hydrophilic to hydrophobic.

[0118] Step S4: The aerogel foam mixture is cold-pressed and dried; wherein the cold-pressing pressure is fixed at 2.7 MPa; the drying temperature is 60℃ and the drying time is 6h.

[0119] Example 1B The preparation method of the aerogel in Example 1B is basically the same as that of the aerogel in Example 1A, except that in step S3, the weight of the silica aerogel is 17 parts.

[0120] Example 1C The preparation method of the aerogel in Example 1C is basically the same as that of the aerogel in Example 1A, except that in step S3, the weight of the silica aerogel is 19 parts.

[0121] Example 1D The preparation method of the aerogel in Example 1D is basically the same as that of the aerogel in Example 1A, except that in step S3, the weight of the silica aerogel is 21 parts.

[0122] Example 1E The preparation method of the aerogel in Example 1E is basically the same as that of the aerogel in Example 1A, except that in step S3, the weight of the silica aerogel is 22 parts.

[0123] Example 2A The preparation method of the aerogel in Example 2A is basically the same as that of the aerogel in Example 1C, except that the mass percentage of glass fiber is 1% in step S1.

[0124] Example 2B The preparation method of the aerogel in Example 2B is basically the same as that of the aerogel in Example 1C, except that the mass percentage of glass fiber is 2% in step S1.

[0125] Example 3 The preparation method of the aerogel in Example 3 is basically the same as that of the preparation method of the aerogel in Example 1C. The difference is that in step S1, the glass fiber may include long fibers and short fibers with a mass ratio of 7:3; wherein the length of the long fiber is 4-8 mm and the length of the short fiber is 2-4 mm.

[0126] Example 4 The preparation method of the aerogel in Example 4 is basically the same as that of the preparation method of the aerogel in Example 1C. The difference is that in step S2, the mixed slurry is foamed by gradually increasing the stirring speed: first, the mixed slurry is initially stirred at a first stirring speed of 600 r / min for 3 min; then, the mixed slurry containing bubble nuclei is further stirred at a stirring speed of 1000 r / min for 3 min; finally, the mixed slurry containing bubble nuclei is stirred at a second stirring speed of 1200 r / min for 3 min.

[0127] Example 5 The preparation method of the aerogel in Example 5 is basically the same as that of the preparation method of the aerogel in Example 1C. The difference is that in step S2, when the mixed slurry is physically stirred and foamed, the foam density of the foam body is controlled at 0.1 g / cm³, and the average diameter of the foam body is controlled at 200 μm.

[0128] Example 6A The preparation method of the aerogel in Example 6A is basically the same as that in Example 1C, except that in step S3, the silica aerogel is mainly composed of small-diameter particles, specifically silica aerogel particles with a diameter of 5-50 μm. Specifically, the particle size of the silica aerogel particles exhibits a normal distribution within the 5-50 μm range.

[0129] Example 6B The preparation method of the aerogel in Example 6B is basically the same as that in Example 1C, except that in step S3, the silica aerogel includes silica aerogel particles with a particle size of 5-50 μm and silica aerogel particles with a particle size of 50-100 μm. The mass fraction of aerogel particles with a particle size of 5-50 μm is 70%, and the mass fraction of aerogel particles with a particle size of 50-100 μm is 30%.

[0130] Specifically, the particle size of silica aerogel particles exhibits a normal distribution within the 50-100μm range; and the particle size of silica aerogel particles also exhibits a normal distribution within the 5-50μm range.

[0131] Example 7 The preparation method of the aerogel in Example 7 is basically the same as that of the aerogel in Example 1C. The difference is that, before step S3, the surface of the aerogel powder is modified and pretreated with 0.5% silane coupling agent.

[0132] Specifically, silane coupling agents containing amino or epoxy groups can be used to further modify the surface of hydrophobic aerogels to optimize their interfacial compatibility and bonding with the polymer matrix or other components. There are many types of such coupling agents, such as γ-glycidoxypropyltrimethoxysilane and 3-aminopropyltrihexyloxysilane. They can effectively improve the performance of the composite material by chemically reacting with the aerogel surface and surrounding materials or by physical adsorption through their functional groups. Among these, γ-aminopropyltriethoxysilane is preferred because its amino groups readily interact with various functional groups, resulting in a more balanced modification effect.

[0133] Example 8A The preparation method of the aerogel in Example 8A is basically the same as that of the preparation method of the aerogel in Example 1C, except that the silica aerogel includes silicon carbide-doped silica composite aerogel; specifically, in step S3, silicon carbide-doped silica composite aerogel can be formed by in-situ doping of silicon carbide; wherein, the mass ratio of silica to silicon carbide is 7:3.

[0134] Example 8B The preparation method of the aerogel in Example 8B is basically the same as that of the aerogel in Example 1C, except that silicon carbide is added to the aerogel foam mixture after step S3; wherein the mass ratio of silicon dioxide to silicon carbide is 7:3.

[0135] Example 9 The preparation method of the aerogel in Example 9 is basically the same as that of the preparation method of the aerogel in Example 1C. The difference is that in step S3, silica aerogel is added to the foam in small amounts and multiple times. After each addition of silica aerogel, the foam is stirred at a low speed of 400 r / min for 1 min, and then the foam is extruded by roller pressing for 30 s. The same stirring and extrusion method is repeated multiple times.

[0136] Example 10 The preparation method of the aerogel in Example 10 is basically the same as that of the preparation method of the aerogel in Example 1C. The difference is that in step S4, the aerogel foam mixture is pressurized by gradually increasing the pressure: first, the aerogel foam mixture is pressurized with a first pressure of 0.5 MPa and held for 1 min; then, the pressure is increased by 1 MPa and held for 1 min; finally, the pressure is increased by a second pressure of 1.5 MPa and held for 1 min.

[0137] Example 11 The preparation method of the aerogel in Example 10 is basically the same as that of the aerogel in Example 1C, except that in step S3, the silica aerogel is a non-hydrophobic aerogel.

[0138] Comparative Example 1 The preparation method of the aerogel in Comparative Example 1 is basically the same as that of the aerogel in Example 1C, except that in step S1, a certain amount of foaming agent is added and stirred evenly; and step S2 is omitted.

[0139] Comparative Example 2 According to the existing method for preparing silica aerogel felt, silica aerogel is combined with fiber felt in sequence by sol-gel method, impregnation composite method and supercritical drying method to prepare flexible silica aerogel felt; wherein, the fiber felt can be glass fiber felt or ceramic fiber felt.

[0140] The following performance tests were performed on the above embodiments and comparative examples: the thermal conductivity of the aerogel insulation material was tested using the heat flow method (ASTM C518); the density of the aerogel insulation material was tested using the volumetric weighing method; the compressibility of the aerogel insulation material was tested using a universal testing machine (GB / T 8813); the stiffness of the aerogel insulation material was tested using a bending test combined with visual inspection and tactile examination, wherein the bending phenotype was: soft and bendable (no powder shedding or cracking) < soft < relatively soft < relatively stiff (powder shedding when bending); the thermal insulation performance of the aerogel insulation material was tested using a thermal insulation tester.

[0141] The specific test results are shown in Table 1, which presents the performance test results of different aerogel insulation materials.

[0142] According to the test results in Table 1, compared with the aerogel insulation material containing foaming agent in Comparative Example 1 and the fiber-reinforced aerogel felt in Comparative Example 2, the performance of the aerogel insulation materials provided in Examples 1A-10 is significantly improved. They have lower thermal conductivity, better insulation performance, compressibility and stiffness.

[0143] Specifically, according to the test results of Examples 1A-1E, compared with Examples 1B-1D, Example 1A is softer and stronger, but its thermal insulation performance is significantly reduced; while Example 1E, although meeting the thermal insulation requirements, suffers from being too hard, prone to powdering, and having poor molding properties. Therefore, it can be concluded that an aerogel powder weight of 17-21 parts provides a more balanced performance across all aspects.

[0144] According to the test results of Example 1C and Examples 2A-2B, it can be seen that appropriately increasing the content of reinforcing fibers can improve the mechanical properties of aerogel insulation materials and reduce cracking caused by drying.

[0145] According to the test results of Examples 1C and 3, using a combination of long and short fibers in the reinforcing fibers can further improve the skeleton strength and crack resistance of aerogel insulation materials, and also help to further reduce the shrinkage and deformation of aerogel insulation materials during the drying process.

[0146] According to the test results of Examples 1C and 4, it can be seen that foaming the mixed slurry by gradually increasing the stirring speed is beneficial to reducing the thermal conductivity of the aerogel insulation material and improving its insulation uniformity.

[0147] According to the test results of Examples 1C and 5, by precisely controlling the foam density and average diameter of the foam body, the foam skeleton is made more stable and the silica aerogel is dispersed more evenly, thereby effectively improving the thermal insulation performance of the aerogel insulation material.

[0148] According to the test results of Example 1C and Examples 6A-6B, it can be seen that using silica aerogel with a bimodal particle size distribution can significantly improve the thermal insulation performance of aerogel insulation materials.

[0149] Based on the test results of Examples 1C and 7, it can be seen that the stiffness of Example 7 is better than that of Example 1C. Therefore, it can be seen that the surface modification pretreatment of aerogel powder with silane coupling agent can effectively improve the interfacial bonding strength and structural stability, thereby significantly enhancing the mechanical strength of the final prepared aerogel thermal insulation material, greatly improving the powder shedding resistance, and also significantly improving the dimensional stability and performance retention rate of the material during the heat treatment process.

[0150] According to the test results of Examples 1C and 8A-8B, it can be seen that adding a light-shielding agent such as silicon carbide by in-situ doping and physical mixing can significantly improve the thermal insulation performance of aerogel insulation materials.

[0151] According to the test results of Examples 1C and 9, adding silica aerogel to the foam in small amounts multiple times can significantly improve the thermal insulation performance of aerogel insulation materials.

[0152] According to the test results of Examples 1C and 10, pressurizing the aerogel foam mixture by gradually increasing the pressure effectively reduces the thermal conductivity of the aerogel insulation material.

[0153] According to the test results of Examples 1C and 11, it can be seen that using non-hydrophobic silica aerogel can improve the mechanical properties and strength of aerogel insulation materials.

[0154] The above description is merely an embodiment of this application and does not limit the patent scope of this application. Any equivalent structural or procedural transformations made using the content of this application's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this application.

Claims

1. A method for preparing an aerogel thermal insulation material, characterized in that, include: Mix 6%-8% binder, 1%-2% foam stabilizer, 0.5%-2% reinforcing fiber, and 85%-95% water by weight to obtain a mixed slurry; The mixed slurry is physically stirred and foamed to form a foam body; Add 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mix evenly to form an aerogel foam mixture; The aerogel foam mixture is cold-pressed and dried.

2. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture includes: The aerogel powder is added to the foam in small amounts multiple times; and after each addition, the foam is stirred and extruded for a certain period of time.

3. The method for preparing the aerogel thermal insulation material according to claim 2, characterized in that, The steps of stirring and pressing the foam for a certain period of time after each addition include: The foam body is stirred at low speed and then extruded by roller pressing and repeated multiple times; wherein the stirring speed of the low speed stirring is 300-500 r / min, the stirring time is 1-2 min, and the roller pressing time is 30 s-1 min.

4. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture includes: The aerogel powder is formed by in-situ doping with a light-blocking agent; the aerogel powder includes a light-blocking agent-doped silica composite aerogel; and / or... After the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture, the method further includes: A light-blocking agent is added to the aerogel foam mixture; the aerogel powder comprises silica aerogel. The mass ratio of silicon dioxide to the light-blocking agent is 6:4-8:

2.

5. The method for preparing the aerogel thermal insulation material according to any one of claims 1-4, characterized in that, The aerogel powder includes aerogel particles with a particle size of 5-50 μm and aerogel particles with a particle size of 50-100 μm; and the mass fraction of aerogel particles with a particle size of 5-50 μm is 60%-80%.

6. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The step of physically stirring and foaming the mixed slurry includes: The mixed slurry is foamed by gradually increasing the stirring speed; wherein the stirring speed increases gradually between a first stirring speed and a second stirring speed; the first stirring speed is 500-700 r / min, the second stirring speed is 1100-1300 r / min; the gradient of stirring speed is 200-400 r / min, and the stirring time of each gradient is 2-3 min.

7. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The foam density of the foam body is 0.08–0.12 g / cm³; the average diameter of the foam body is less than or equal to 200 μm.

8. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The step of cold-pressing and drying the aerogel foam mixture includes: The aerogel foam mixture is pressurized by gradually increasing the pressure, and after depressurization, the mold is kept closed for 3-5 minutes before demolding; wherein the pressurization pressure is gradually increased between a first pressure and a second pressure; the first pressure is 0.4-0.6 MPa, and the second pressure is 1.4-1.6 MPa; the pressurization time is 1-3 minutes; and the pressure gradient is 0.2-0.5 MPa. The aerogel foam mixture is dried under normal pressure; wherein the drying temperature is 55-65℃ and the drying time is 5-7h.

9. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, Prior to the step of adding 17-21 parts by weight of aerogel powder to 33-37 parts by weight of the foam and mixing them evenly to form an aerogel foam mixture, the method further includes: The surface of the aerogel powder was modified and pretreated using 0.2%-1% silane coupling agent.

10. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The reinforcing fiber comprises long fibers and short fibers in a mass ratio of 6:4 to 8:2; the long fibers have a length of 4-8 mm, and the short fibers have a length of 2-4 mm.

11. The method for preparing the aerogel thermal insulation material according to claim 1, characterized in that, The step of uniformly mixing 6%-8% binder, 1%-2% foam stabilizer, 0.5%-2% reinforcing fiber, and 85%-95% water by weight to obtain a mixed slurry specifically includes: A mixed solution is obtained by mixing 6%-8% of the adhesive, 1%-2% of the foam stabilizer, and 85%-95% of the water by weight. The reinforcing fiber, at a mass percentage of 0.5%-2%, is added to the mixed solution and stirred until homogeneous to obtain the mixed slurry.

12. A method for preparing an aerogel thermal insulation material, characterized in that, include: A mixed slurry is provided; the mixed slurry includes a solvent, a binder, a foam stabilizer, and a reinforcing material, but does not contain a foaming agent; The mixed slurry is stirred and foamed to form a foam body; Aerogel powder is added to the foam and mixed to form an aerogel foam mixture; The aerogel foam mixture is cold-pressed and dried.

13. An aerogel thermal insulation material, characterized in that, The aerogel insulation material is prepared using the preparation method of aerogel insulation material as described in any one of claims 1-11.

14. An aerogel thermal insulation material, characterized in that, The aerogel insulation material does not contain a foaming agent; by weight percentage, the aerogel insulation material comprises the following components: 8%-14% binder, 1%-3% foam stabilizer, 0.5%-1.5% reinforcing fiber and 80%-90% aerogel powder.