A ceramic fiber product and its internal temperature testing method
By combining a two-stage microwave drying process with infrared heating, and dynamically adjusting microwave parameters and monitoring the internal temperature in real time, the structural damage caused by moisture vaporization and temperature runaway in ceramic fiber products during microwave drying is solved, resulting in a significant improvement in high-temperature anti-aging performance.
Patent Information
- Application Number
- CN202611389018.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ceramic fiber products are prone to structural damage during microwave drying due to excessively rapid moisture vaporization or temperature runaway, affecting their anti-aging performance. Furthermore, the internal moisture content cannot accurately reflect thickness differences, leading to insufficient product strength or cracking.
It adopts a two-stage microwave drying process, combined with infrared heating, dynamically adjusts microwave parameters and monitors internal temperature, and monitors internal temperature in real time through a fluorescent fiber optic sensor to avoid local overheating and control the moisture content to within 0.8wt%, ensuring high-temperature anti-aging performance.
It significantly improves the high-temperature anti-aging performance of ceramic fiber products, ensuring that the open gap pressure reaches more than 60 kPa after 5000 hot compression cycles at 900℃, thereby improving product consistency and anti-aging performance.
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic fiber technology, and more specifically to a ceramic fiber product and a method for testing its internal temperature. Background Technology
[0002] Ceramic fiber products are industrial products made from ceramic fibers as raw materials. They are lightweight, high temperature resistant, have good thermal stability, low thermal conductivity, low specific heat, good thermal insulation performance, good high temperature insulation performance, non-toxicity, and resistance to mechanical vibration. They are specially used in various high temperature, high pressure, and easily worn environments and are an excellent refractory material.
[0003] Existing technologies reduce the overall moisture content of ceramic fiber products through high-temperature drying, but fiber breakage, damage to the physical overlap between fibers or the bonding agent still occurs, leading to macroscopic cracks under repeated thermal shocks and a decline in the product's anti-aging performance.
[0004] In the microwave drying process of thick ceramic fiber products, improper control of microwave drying power or setting of the drying curve can easily lead to product scrap. If the internal moisture vaporizes too quickly and the pressure rises sharply during microwave drying, and the channels for moisture migration to the outside are blocked, the material structure may be ruptured, leading to cracking. Although microwave heating tends to self-balance, local energy concentration can still occur, causing the binder to scorch, resulting in yellowing, blackening, or even carbonization of the product, severely damaging its mechanical strength. Microwave heating causes rapid vaporization of moisture, but if the temperature gets out of control in the later stages of drying, excessively high temperatures can directly decompose the binder. This weakens the bonds between fibers, resulting in insufficient strength after drying, or even brittleness or powdering.
[0005] To improve efficiency, traditional processes often employ rapid heating. However, if the heating rate exceeds a certain temperature per minute, it can damage the ceramic fiber structure. Conversely, if the heating rate is too slow, insufficient internal pressure prevents water vapor from effectively escaping. Continuous high-power heating damages the structure, leading to decreased anti-aging properties at the same moisture content and causing fiber expansion, thus affecting product thickness. To address this issue, current technological solutions primarily focus on adjusting the adhesive system and formulation, and adding new functional additives. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention has discovered through research that there are significant differences in the internal moisture content of ceramic fiber products of different thicknesses, and that internal moisture content is an important factor affecting anti-aging performance. This invention proposes a method for testing the internal temperature of ceramic fiber products, which significantly reduces internal moisture content and exhibits excellent high-temperature anti-aging performance.
[0007] To address the shortcomings of existing technologies, this invention has discovered significant differences in the internal moisture content of ceramic fiber products of varying thicknesses. Furthermore, internal moisture content is a crucial factor influencing the decline in anti-aging performance. For ceramic fiber products with a thickness ≥ 5 mm, internal moisture content has a significant impact on anti-aging performance, and this impact intensifies with increasing thickness; the thicker the material, the more difficult it is to reduce the internal moisture content. The overall moisture content of thick ceramic fiber products cannot accurately reflect the content of free water trapped within the micropores and fiber overlaps. This trapped moisture vaporizes and expands rapidly at high temperatures, generating enormous vapor pressure and forming a vapor pressure gradient, leading to fiber breakage, interfacial debonding, and microcrack propagation. Excessive internal moisture content causes a large amount of water vapor to accumulate in a confined microenvironment shortly after heating, damaging the product's microstructure and macroscopic mechanical properties, significantly reducing its anti-aging properties and high-temperature stability. Especially in applications where ceramic fiber products undergo repeated heating, the internal moisture continuously impacts and damages the fiber structure during heating.
[0008] In a first aspect, the present invention provides a ceramic fiber product, wherein the thickness of the ceramic fiber product is greater than 5 mm and the internal moisture content is less than 0.8 wt%, and the high-temperature anti-aging performance of the ceramic fiber product meets the following requirement: after 5000 hot compression cycles at 900°C, the pressure at the open gap point is greater than 60 kPa.
[0009] In some embodiments, the thickness of the ceramic fiber product is 5mm-100mm, preferably 8-25mm, for example 8mm, 9mm, 10mm, 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm, 23mm, 24mm, 25mm.
[0010] In some embodiments, the internal moisture content of the ceramic fiber product is 0.1-0.8 wt%, preferably 0.3-0.7 wt%, such as 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, and 0.7 wt%.
[0011] In some embodiments, the high-temperature anti-aging properties of the ceramic fiber product meet the following requirements: after 5000 hot compression cycles at 900°C, the pressure at the open gap point is 60-70 kPa, preferably 65-70 kPa.
[0012] Secondly, the present invention provides a method for preparing ceramic fiber products, comprising: S1: Ceramic fiber pulping; S2: The material obtained in S1 is dehydrated and molded, and then surface-adhesive is applied to it using an adhesive. S3: Microwave drying, wherein the heating temperature of the microwave drying is 50-100℃ and the microwave power is 600-1200kW. The microwave drying is provided with a microwave heating zone and a microwave heat preservation zone. In the microwave heating zone, the material obtained in step S2 is rapidly heated under the heating temperature and microwave power conditions. When the internal temperature of the material reaches 100℃, it is sent to the microwave heat preservation zone. In the microwave heat preservation zone, a stable microwave energy lower than that in the heating zone is continuously supplied so that the material is dried under heat preservation conditions. S4: Infrared heating, natural gas heating, or hot air heating.
[0013] In some implementations, the ceramic fiber in step S1 is polycrystalline mullite fiber.
[0014] In some embodiments, the ceramic fibers described in step S1 have a fiber purity of 94-99.5%, a fiber diameter of 3-5 μm, and a length of 3-6 mm.
[0015] In some implementations, the adhesive is selected from epoxy resin emulsions.
[0016] In some embodiments, the infrared heating temperature is 80-120°C, preferably 100-120°C.
[0017] In some implementations, the infrared power is 65-85 kW, preferably, the infrared power in the first infrared zone of infrared heating is 83 kW, and the infrared power in the second infrared zone is 69 kW.
[0018] In some implementations, the natural gas heating is a double-layer heating system, with a heating temperature of 180-200℃, a heating time of 5-10 minutes, and an energy consumption of 50-80 m³ / h. 3 Natural gas, for example, heating to 190°C for 6 minutes, consumes 60m³ of energy per hour. 3 natural gas.
[0019] Thirdly, the present invention provides a ceramic fiber product prepared by the above method.
[0020] Fourthly, the present invention provides a high-temperature liner for a pollution control device, the liner comprising the aforementioned ceramic fiber articles.
[0021] Fifthly, the present invention provides a pollution control device, including a housing and a high-temperature liner, wherein the high-temperature liner is disposed inside the housing.
[0022] Sixthly, the present invention provides the application of the aforementioned ceramic fiber products in motor vehicle pollution control devices.
[0023] In some implementations, the application is the use of the aforementioned ceramic fiber products in high-temperature gaskets.
[0024] In a seventh aspect, the present invention provides a method for testing the internal temperature of ceramic fiber products, comprising: SS1, Sensor Preparation and Calibration A fluorescent fiber temperature sensor with a diameter ≤250μm was selected. The total length of the fiber was greater than the sum of the wet blank thickness and the lead-out path length. The fluorescent fiber temperature sensor and the standard temperature measuring device were placed in a high-temperature furnace simultaneously and calibrated at multiple temperature points. The temperature-optical signal standard function relationship was fitted to ensure measurement accuracy. SS2, Probe Pre-embedding and Wet Blank Forming The ceramic fiber raw material is stirred, pulped, and dehydrated and formed. Before the ceramic fiber wet blank is formed, the tip of the optical fiber probe is fixed in a set position inside the blank, and an outlet groove is set at the edge of the blank. Then, vacuum filtration is performed to complete the dehydration and forming. After dehydration and forming, the fiber naturally wraps around the optical fiber probe to form an in-situ pre-embedded structure. SS3, microwave drying and online control of internal temperature (1) Connect the pre-embedded sensor to the external signal demodulator through the fiber optic adapter to achieve interference-free transmission of signals inside and outside the microwave cavity; (2) In the heating zone and constant speed drying zone of the microwave device, microwave drying is carried out in the heating zone under the conditions of microwave power of 650W and microwave heating temperature of 60°C, and the internal temperature data is collected in real time. When the internal temperature reaches 100°C, the material is sent to the constant speed drying zone to stabilize the internal temperature of the material and remove free water. SS4. Remove the probe after drying.
[0025] In some implementations, in step SS2, the tip of the fiber optic probe is fixed to the central layer or central region of the blank.
[0026] In some implementations, in step SS2, a smooth arc-shaped guide groove is designed at the edge of the blank, with the fiber bending radius being greater than 40 mm.
[0027] In some implementations, in step SS3, the material is moved using a vibration or rotation device, and the surface temperature field is monitored using an infrared thermal imager. In some implementations, in step S3, an internal temperature-time curve is generated based on the internal temperature data.
[0028] In some implementations, step SS4, removing the probe after drying, includes both non-destructive and destructive removal.
[0029] In some implementations, in step SS4, after drying is complete, the probe is removed by physical removal.
[0030] In some implementations, in step SS4, the embedded connector and quick plug are connected by a detachable miniature fiber optic connector. After drying, the fiber can be pulled out by unscrewing the locking nut on the quick plug.
[0031] In some implementations, in step SS4, after drying is complete, the external optical fiber is cut off, leaving the probe inside the product.
[0032] Terminology Definition In this invention, unless otherwise defined, the internal moisture content refers to the value measured by sampling the central layer or central region of the ceramic fiber product according to the moisture content determination method specified in GB / T 3007-2017. The central layer or central region is a thin layer area with a thickness between 1 mm and 2 mm, defined with the centerline of the ceramic fiber product's thickness direction as a reference. The thickness of the central layer is determined by the thickness of the ceramic fiber product; a larger thickness results in a larger central layer thickness. For example, the central layer thickness of a 9 mm product is 1 mm, and the central layer thickness of a 17 mm product is 2 mm.
[0033] In this invention, unless otherwise defined, rapid heating refers to a heating process in which the system is heated from the initial temperature to the target temperature within 5 minutes at a heating rate of 15°C / min.
[0034] Beneficial effects This invention monitors the internal temperature and dynamically adjusts microwave parameters. It adopts a two-stage partitioned design with a microwave heating zone and a microwave heat preservation zone. When the internal temperature of the product approaches 100°C, it enters the microwave heat preservation zone to meet the drying characteristics of thick ceramic fiber products, which are initially fast and then slow.
[0035] This invention uses an internal temperature measuring device to monitor the internal temperature of fiber products in real time and dynamically adjust the microwave heating process to avoid localized overheating during microwave heating. The internal temperature control method enables a two-stage partitioned design of the microwave heating zone and the constant-speed drying zone. The product enters the constant-speed drying zone when its internal temperature approaches 100°C, satisfying the drying characteristics of thick ceramic fiber products, which are initially fast and then slow down, thus improving product consistency and anti-aging properties.
[0036] Using optical signal temperature measurement, it is completely unaffected by microwave electromagnetic fields, ensuring stable temperature measurement and reliable data; the temperature measurement accuracy can reach ±0.1℃, and it can capture internal temperature changes in real time; moreover, the probe diameter is small, and pre-embedding in the wet blank stage can avoid damaging the fiber structure and molding uniformity; at the same time, it can realize multi-point temperature measurement, fully reflecting the temperature field distribution in the thickness direction. Detailed Implementation
[0037] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0038] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0039] Example 1 Pulping: 22.8 kg of polycrystalline mullite fiber (fiber purity 94%, fiber diameter 3~5μm, length 3-6mm) was used as raw material. 3 tons of clean water were added, and the mixture was placed in a pulping tank for stirring and pulping. The stirring frequency and time were set (pulping frequency 35Hz, time 8 minutes). After uniform stirring, the mixture was removed and set aside. The main components of the polycrystalline mullite are sodium oxide, aluminum oxide, and silicon dioxide, with percentage contents of 0.17%, 44.06%, and 55.27%, respectively. Dehydration and surface reinforcement: The prepared material obtained in the previous step is dehydrated by sedimentation to form a wet paper web or preform. The forming thickness is controlled to be 9mm. The adhesive (epoxy resin emulsion) is sprayed onto the surface of the paper using an atomization spraying method.
[0040] Two-stage microwave drying: The material obtained from the dehydration, molding, and surface strengthening steps is microwave dried. The microwave power is 650W, and the microwave heating temperature is 60°C. The microwave drying equipment includes a microwave heating zone and a microwave insulation zone. The microwave heating zone consists of six microwave heating chambers, each with an array of 18 magnetrons. Upon entering the heating zone, the material rapidly absorbs high-intensity microwave energy, quickly rising from room temperature. When the internal temperature sensor detects that the internal temperature reaches 100°C, the material enters the microwave insulation zone. This zone consists of nine microwave insulation chambers, each with an array of 12 magnetrons. The radiation density is approximately two-thirds that of the heating zone, and the material spends a longer time within the nine chambers. The insulation zone provides a continuous supply of energy at a lower and more stable intensity, preventing fiber damage due to overheating. The total heating time for both the microwave heating and microwave insulation zones is 20 minutes.
[0041] Infrared drying: The semi-finished product after microwave drying is directly sent to the infrared heating box for final drying. The power of infrared zone 1 is 82kW, the power of infrared zone 2 is 69kW, the infrared heating temperature is 100°C, and the heating time is 30 minutes.
[0042] Cutting: Cut the product obtained in the previous step to the required size.
[0043] In the process of preparing ceramic fiber products, the internal moisture content is measured using the following steps.
[0044] S1. Sensor Preparation and Calibration A fluorescent fiber temperature sensor with a diameter ≤250μm was selected, and the total length of the fiber was greater than the sum of the wet blank thickness and the lead-out path length. The fluorescent fiber sensor and the standard temperature measuring device were placed in a high-temperature furnace simultaneously and calibrated at multiple temperature points. The temperature-optical signal standard function relationship was obtained by fitting.
[0045] S2, Probe pre-embedding and wet blank forming Before forming the wet blank, the tip of the fiber optic probe is fixed at the center layer in the thickness direction of the blank; a smooth arc-shaped guide groove is set at the edge of the blank to control the bending radius of the fiber optic cable > 40mm. The fiber slurry is precipitated and dehydrated to form a wet blank with a thickness controlled at 9mm; an epoxy resin emulsion is sprayed onto the surface of the wet blank using an atomizing spraying method for surface reinforcement, and the fiber naturally wraps around the fiber optic probe to form an in-situ pre-embedded structure.
[0046] S3, microwave drying and online temperature control By connecting the pre-embedded sensor to the external signal demodulator through an optical fiber adapter, interference-free transmission of signals inside and outside the microwave cavity can be achieved.
[0047] The wet blanks are fed into a two-stage microwave drying equipment with a total microwave power of 650W and a set heating temperature of 60℃. The microwave drying equipment includes a microwave heating zone and a constant-speed drying zone. The heating zone is equipped with 6 heating chambers, each with an array of 18 magnetrons. The constant-speed drying zone is equipped with 9 heat preservation chambers, each with an array of 12 magnetrons, and the radiation density is two-thirds that of the heating zone.
[0048] The product is rapidly heated in the heating zone, with the temperature monitored in real time by an internal temperature measuring device. When the internal temperature reaches 100℃, the product is placed in the microwave constant-speed drying zone for constant-speed drying to stabilize the internal temperature and remove free water. An internal temperature reading is generated based on the internal temperature data. Time curve. The total drying time for the microwave heating zone and the constant-speed drying zone is 20 minutes.
[0049] S4. Complete drying and remove the probe. After drying, the fiber optic probe is removed without damage using a physical removal method.
[0050] The product prepared in this embodiment has a thickness of 9 mm, an internal moisture content of 0.6%, and a high-temperature anti-aging performance of 61 kPa.
[0051] Example 2: A 17mm thick ceramic fiber product was prepared according to Example 1, and its internal moisture content was tested. The forming thickness was controlled to be 17mm during the dehydration and forming step. The conditions for the microwave drying and infrared drying steps were as follows: Two-stage microwave drying: The material obtained from the dehydration, molding, and surface strengthening steps is microwave dried. The microwave power is 950W, and the microwave heating temperature is 60°C. The microwave drying equipment includes a microwave heating zone and a microwave insulation zone. The microwave heating zone consists of six microwave heating chambers, each with an array of 18 magnetrons. Upon entering the heating zone, the material rapidly absorbs high-intensity microwave energy, quickly rising from room temperature. When the internal temperature sensor detects that the internal temperature reaches 100°C, the material enters the microwave insulation zone. This zone consists of nine microwave insulation chambers, each with an array of 12 magnetrons. The radiation density is approximately two-thirds that of the heating zone, and the material spends a longer time within the nine chambers. The insulation zone provides a continuous supply of energy at a lower and more stable intensity, preventing fiber damage due to overheating. The total heating time for both the microwave heating and microwave insulation zones is 40 minutes.
[0052] Infrared drying: The semi-finished product after microwave drying is directly sent to the infrared heating box for final drying. The power of infrared zone 1 is 82kW, the power of infrared zone 2 is 69kW, the infrared heating temperature is 120°C, and the heating time is 40 minutes.
[0053] The product prepared in this embodiment has a thickness of 17 mm, an internal moisture content of 0.7%, and a high-temperature anti-aging performance of 60.5 kPa.
[0054] The embodiments of the present invention have been described above. However, the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A ceramic fiber product, characterized in that, The ceramic fiber product has a thickness greater than 5 mm and an internal moisture content of less than 1.0 wt%. The high-temperature anti-aging performance of the ceramic fiber product meets the following requirement: after 5000 hot compression cycles at 900℃, the pressure at the open gap point is greater than 60 kPa.
2. The ceramic fiber product according to claim 1, characterized in that, The thickness of the ceramic fiber product is 5mm-25mm.
3. A method for preparing a ceramic fiber product according to any one of claims 1-2, characterized in that, include: S1: Ceramic fiber pulping; S2: The material obtained in S1 is dehydrated and molded, and then surface-adhesive is applied to it using an adhesive. S3: Microwave drying, wherein the heating temperature of microwave drying is 50-100℃ and the microwave power is 600-1200kW. The microwave drying is provided with a microwave heating zone and a microwave heat preservation zone. In the microwave heating zone, the material obtained in step S2 is rapidly heated under the heating temperature and microwave power conditions. When the internal temperature of the material reaches 100℃, it is sent to the microwave heat preservation zone. In the microwave heat preservation zone, a stable microwave energy lower than that in the heating zone is continuously supplied, so that the material can be dried in the heat preservation state. S4: Infrared heating, natural gas heating, or hot air heating.
4. A method for preparing a ceramic fiber product according to claim 3, characterized in that, The infrared heating temperature is 80-120℃, and the infrared power is 65-85 kW.
5. A method for preparing a ceramic fiber product according to claim 3, characterized in that, The natural gas heating is a double-layer heating system, with a heating temperature of 180-200℃, a heating time of 5-10 minutes, and an energy consumption of 50-80 m³ / h. 3 natural gas.
6. A ceramic fiber product prepared by the method according to any one of claims 3-5.
7. A high-temperature gasket for a pollution control device, characterized in that, The liner comprises the ceramic fiber article as described in any one of claims 1, 2, and 6.
8. A pollution control device, characterized in that, The pollution control device includes a housing and a high-temperature liner as described in claim 7, wherein the high-temperature liner is disposed inside the housing.
9. The application of the ceramic fiber product according to any one of claims 1, 2, and 6 in a motor vehicle pollution control device.
10. A method for testing the internal temperature of a ceramic fiber product according to claim 1, comprising: SS1, Sensor Preparation and Calibration A fluorescent fiber temperature sensor with a diameter ≤250μm was selected. The total length of the fiber was greater than the sum of the wet blank thickness and the lead-out path length. The fluorescent fiber temperature sensor and the standard temperature measuring device were placed in a high-temperature furnace simultaneously and calibrated at multiple temperature points. The temperature-optical signal standard function relationship was fitted to ensure measurement accuracy. SS2, Probe Pre-embedding and Wet Blank Forming The ceramic fiber raw material is stirred, pulped, and dehydrated and formed. Before the ceramic fiber wet blank is formed, the tip of the optical fiber probe is fixed in a set position inside the blank, and an outlet groove is set at the edge of the blank. Then, vacuum filtration is performed to complete the dehydration and forming. After dehydration and forming, the fiber naturally wraps around the optical fiber probe to form an in-situ pre-embedded structure. SS3, microwave drying and online control of internal temperature (1) Connect the pre-embedded sensor to the external signal demodulator through the fiber optic adapter to achieve interference-free transmission of signals inside and outside the microwave cavity; (2) In the heating zone and constant speed drying zone of the microwave device, microwave drying is carried out in the heating zone at a heating temperature of 50-100℃ and a microwave power of 600-1200kW, and the internal temperature data is collected in real time. When the internal temperature reaches 100℃, the material is sent to the constant speed drying zone to stabilize the internal temperature of the material and remove free water. SS4. Remove the probe after drying.