Alkali-activated lightweight high-strength thermal insulation material modified by oxidation-mineralization synergy and preparation method thereof
By employing a synergistic modification process involving ferrous activation persulfate oxidation, carbide slag mineralization, and slag co-grinding, the problems of organic matter inhibition and heavy metal stabilization in sludge-based foam lightweight materials were solved, resulting in improved lightweight, high-strength, and thermal insulation properties.
Patent Information
- Application Number
- CN202611468612.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively utilize dredged sludge from rivers and lakes, particularly in simultaneously weakening the inhibitory effect of organic matter on hydration reactions, pre-stabilizing heavy metals, and continuously constructing gelation reactions, resulting in poor performance of sludge-based foam lightweight materials.
Lightweight and high-strength thermal insulation materials are prepared through synergistic modification treatment of ferrous activated persulfate oxidation, carbide slag alkaline mineralization and slag co-grinding. This includes oxidative degradation of sludge, alkaline mineralization and mechanical co-grinding to form a C-(A)-SH type cementitious network.
It achieves the regulation of organic matter, the pre-stabilization of heavy metals and the activation of particle surface, improves the interfacial bonding between sludge particles and cementitious matrix, forms a continuous cementitious structure, and enhances the material's lightweight, high strength and thermal insulation properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_6
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization and polluted sludge stabilization treatment technology, and in particular to an alkali-activated lightweight high-strength thermal insulation material for sludge synergistic modification by oxidation-mineralization and its preparation method. Background Technology
[0002] Foamed lightweight soil is characterized by its low weight, good fluidity, convenient construction, and good thermal insulation properties, making it suitable for roadbed backfilling and underground cavity filling. Existing products mostly use ordinary silicate cement as the main cementing material, resulting in a high cement content. Silt generated from river and lake dredging, waterway dredging, and urban water environment management typically has high water content, high compressibility, fine particles, and high organic matter content; some silt also contains heavy metal pollutants. Current resource recovery methods often involve removing impurities, drying, and mechanically grinding the silt before directly incorporating it into the cementing system. This treatment primarily improves particle size and water content, but it is difficult to simultaneously weaken the inhibitory effect of organic matter on hydration reactions, and it is also difficult to construct a continuous process for heavy metal pre-stabilization, silt particle activation, and subsequent cementing reactions. Existing alkali-activated solid waste cementing materials typically use single slag or single calcareous solid waste as the main raw material. Although slag is rich in active Si and Al components, its reaction rate is slow under conditions of interference from organic matter in sludge and insufficient alkalinity. While carbide slag can provide Ca(OH)2 and an alkaline environment, it lacks the active silica and alumina components required to form a continuous cementitious network. Furthermore, using sodium carbonate alone for activation typically results in slow early reaction and strength development, while using water glass alone may lead to increased slurry viscosity, excessively rapid coagulation, or decreased foam stability. Therefore, how to utilize the complementary compositions of slag and carbide slag, and how to regulate the reaction rate, cementitious product formation, and cell stability through composite alkali activators, are problems that need further investigation in sludge-based lightweight foam materials. Summary of the Invention
[0003] To address the technical problems of existing technologies, such as conventional drying and grinding of sludge only serving as a low-activity filler, the adverse effects of sludge organic matter on alkali-activated reactions and interfacial bonding, heavy metal stabilization mainly relying on physical encapsulation after molding, and the lack of functional integration between various processing stages, this invention provides a method for preparing lightweight, high-strength thermal insulation materials by first subjecting the sludge to ferrous activation and persulfate oxidation, then using carbide slag for alkaline mineralization and co-grinding with slag, and finally through alkali activation, foaming, fiber toughening, and aerogel insulation. This invention provides a continuous and synergistic sludge modification technology route involving oxidative degradation, alkaline mineralization, mechanical co-grinding, and alkali-activated solidification, and applies it to slag-carbide slag lightweight, high-strength thermal insulation materials.
[0004] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of this invention is an alkali-activated lightweight high-strength thermal insulation material for sludge synergistic modification by oxidation and mineralization, wherein the raw materials, by mass parts, include: The composition includes 53-64 parts of slag, 9.5-16 parts of calcium carbide slag, 20-38 parts of modified sludge precursor, 0.20-0.60 parts of polyethylene fiber, 1.0-3.0 parts of SiO2 aerogel, 0.80-0.98 parts of water-reducing agent, composite alkali activator and composite foaming agent; The composite alkali activator is composed of water glass and sodium carbonate. The total alkali equivalent of the composite alkali activator is 4.0% to 6.0% of the total mass of slag and carbide slag based on Na2O. The sodium carbonate content is 2% of the total mass of slag and carbide slag, and the remainder is supplemented by liquid sodium silicate water glass.
[0005] In a preferred embodiment of the present invention, the method for preparing the modified sludge precursor includes the following steps: S1. Remove impurities from the original sludge, determine the moisture content and calculate the dry basis mass, adjust the dry solids mass fraction to 25% to 35% with deionized water, and adjust the initial pH to 6.0 to 7.5; S2. Add ferrous salt aqueous solution and mix for 5-10 min, then add persulfate solution in batches or dropwise over 10-20 min, controlling the persulfate dosage to be 0.5%-2.0% of the dry sludge mass. Fe 2+ With S2O8 2- The molar ratio is 0.3–0.9, and the reaction is carried out at 20–35°C with stirring for 30–120 min. S3. Detect residual persulfate. When the residual amount is not higher than 5% of the initial amount, add carbide slag slurry, adjust the pH of the system to 10.0-11.5 and stir for 20-40 min, then add slag, continue mixing for 10-20 min and age for 2-6 h. S4. Centrifuge the aged product obtained in step S3 to remove water, and dry it at 60-80℃ to constant weight; S5. Grind the dried and conditioned material obtained in step S4 for 20–60 min and pass it through a 200-mesh sieve to obtain a D50 of 10–30 μm and a specific surface area of 400–650 m². 2 / kg of modified sludge precursor.
[0006] The silt is generated during river and lake dredging projects. After impurities are removed through a 5 mm sieve, the undisturbed silt is not immediately dried at high temperature. Instead, the dry solids content is adjusted to 25%–35%, and the initial pH is adjusted to 6.0–7.5. The silt contains SiO2, Al2O3, Fe2O3, CaO, and clay minerals, as well as organic matter and various heavy metals such as Pb, Zn, Cu, Cr, Ni, and Cd.
[0007] In a preferred embodiment of the present invention, the ferrous salt is one or more of ferrous sulfate, ferrous chloride and their hydrates; the persulfate is one or more of sodium persulfate, potassium persulfate and ammonium persulfate.
[0008] In a preferred embodiment of the present invention, the mass fraction of calcium carbide slag in the calcium carbide slag slurry is 10% to 30%; the amount of calcium carbide slag used is 5% to 15% of the dry weight of the sludge; and the amount of slag used is 2% to 10% of the dry weight of the sludge.
[0009] In this invention, the dry basis of silt refers to the mass of solid matter contained in undisturbed silt after deducting evaporable moisture. Specifically, a representative undisturbed silt sample is taken, dried at 105±5℃ to constant weight, and the moisture content is determined based on the mass difference before and after drying. The dry basis mass of the silt is then calculated by multiplying the undisturbed silt mass by its solid mass fraction.
[0010] The modified sludge precursor of this invention undergoes sequential treatments including ferrous activated persulfate oxidation, carbide slag alkaline mineralization, low-temperature drying, and slag co-grinding. If the oxidation step is omitted, the organic matter in the sludge will continue to coat the particle surface and inhibit subsequent gelation reactions. If carbide slag is added before the persulfate is fully consumed, the rapid increase in system pH will lead to ferrous ion hydrolysis and precipitation, consuming active species and reducing the oxidation effect. If the carbide slag mineralization step is omitted, it is difficult to simultaneously neutralize the acidic substances produced by oxidation and pre-stabilize heavy metals. If the slag co-grinding step is omitted, calcium- and iron-containing mineralization products and active silica-alumina components are difficult to distribute evenly on the surface of the sludge particles, which is detrimental to the formation of a modified sludge precursor with high reactivity.
[0011] Process parameters are mainly determined based on a comprehensive consideration of reaction uniformity, modification effect, and particle activity. The dry solids content of the sludge is controlled at 25%–35% to ensure sufficient contact between the admixture and the sludge particles while avoiding excessive dilution or insufficient fluidity of the slurry; the dosage of persulfate and Fe... 2+ With S2O8 2- By controlling the molar ratio within the aforementioned limits, both the oxidation efficiency of organic matter and the utilization rate of active species can be balanced. During the mineralization stage, the pH is controlled at 10.0–11.5, and the amount of carbide slag and mineral slag is limited. This can achieve the neutralization of acidic substances and the stabilization of heavy metals while reducing localized rapid precipitation and particle agglomeration.
[0012] In a preferred embodiment of the present invention, the composite foaming agent is prepared by mixing plant protein hydrolysate, sodium α-alkenyl sulfonate, cocamidopropyl betaine, hydroxypropyl methylcellulose and water in a mass ratio of 10-15:2-4:1-2:0.2-0.6:80-86. When used, it is diluted with water 20-40 times and formed into pre-made foam by a physical foaming mechanism.
[0013] In a preferred embodiment of the present invention, the polyethylene fiber is a high-strength polyethylene short-cut fiber with a length of 6-12 mm, an equivalent diameter of 10-30 μm, a preferred aspect ratio of 200-1000, a density of 0.95-0.98 g / cm³, a preferred tensile strength of not less than 1500 MPa, and a preferred elastic modulus of not less than 40 GPa; the SiO₂ aerogel is a hydrophobic silica aerogel particle with an average particle size of 0.1-2.0 mm and a thermal conductivity at room temperature not higher than 0.025 W / (m·K), and the SiO₂ aerogel bulk density is 50-150 kg / m³. 3 The porosity is not less than 90%, and the specific surface area is preferably 500–1000 m². 2 / g, with a hydrophobic contact angle preferably not less than 120°.
[0014] Furthermore, the slag is S95 grade granulated blast furnace slag powder, with a preferred specific surface area of 400–500 m². 2 / kg, with a moisture content of no more than 1.0%, and its main active components include CaO, SiO2, Al2O3 and MgO.
[0015] Furthermore, the sodium carbonate is anhydrous sodium carbonate, with a Na2CO3 purity of not less than 98%, and preferably a particle size of not more than 300 μm.
[0016] Furthermore, the water glass is liquid sodium silicate water glass with a modulus of 1.8 and a solid content of 38% to 42%, preferably 40%; the mass fraction of Na2O in the water glass is preferably 14% to 15%, and the mass fraction of SiO2 is preferably 24% to 27%.
[0017] Furthermore, the water-reducing agent is a polycarboxylate-based high-performance water-reducing agent, preferably an ether-based polycarboxylate water-reducing agent with good compatibility with the alkali-activated system, with a solid content preferably of 35% to 45%, and the dosage of the water-reducing agent is 1.0% to 1.4% of the total mass of slag and carbide slag.
[0018] Furthermore, in a preferred embodiment of the present invention, the water-cement ratio of the alkali-activated lightweight high-strength thermal insulation material of the oxidized-mineralized synergistic modified sludge is 0.25–0.30, and the designed wet density is 570 ± 20 kg / m³. 3 ~620±20 kg / m 3 .
[0019] The second technical solution of the present invention is a method for preparing an alkali-activated lightweight high-strength thermal insulation material of the above-mentioned oxidation-mineralization synergistic modification of sludge, comprising the following steps: Subtract the slag and carbide slag used to prepare the modified sludge precursor from the total amount of the formula to obtain the remaining slag and remaining carbide slag; separate the slag used for pre-dispersing SiO2 aerogel and polyethylene fiber from the remaining slag to obtain the remaining slag; dry mix the modified sludge precursor, the remaining slag and the remaining carbide slag, then add the premix of SiO2 aerogel and slag and the premix of polyethylene fiber and slag in sequence, and continue stirring to obtain the dry mixture; Sodium carbonate was dissolved in part of the mixing water. After the solution temperature returned to room temperature, water glass was added, stirred and allowed to stand to obtain a composite alkali activator. Add the composite alkali activator, water-reducing agent and remaining mixing water to the dry mix, stir at 120 r / min for 2 min, then increase to 200 r / min and stir for 2 min to obtain the basic slurry; The composite foaming agent was diluted with water at a mass ratio of 1:30, and pre-made foam was prepared using a compressed air physical foaming machine, with the density of the pre-made foam controlled at 65±5 kg / m³. 3 ; The pre-made foam was added to the base slurry in three parts. After each addition, the mixture was stirred at a low speed of 40-50 r / min for 30-40 seconds. After all the pre-made foam was added, the mixture was stirred at a low speed for another 60 seconds. The slurry is poured into the mold without mechanical vibration. The surface is lightly scraped and then covered with a polyethylene film and left to stand for 24 hours. After demolding, it is placed in an environment with a temperature of 20±2℃ and a relative humidity of not less than 95% to cure for the specified age.
[0020] In a preferred embodiment of the present invention, the SiO2 aerogel is premixed with slag at a mass ratio of 1:3 before use to obtain a premix of SiO2 aerogel and slag; the polyethylene fiber is pre-dispersed in a dry state at a mass ratio of 1:5 before use to obtain a premix of polyethylene fiber and slag.
[0021] The third technical solution of this invention is the application of the above-mentioned alkali-activated lightweight high-strength thermal insulation material of oxidized-mineralized synergistic modified sludge in building thermal insulation filling, roadbed backfilling, or underground cavity filling.
[0022] This invention utilizes a sequence of oxidation, mineralization, co-grinding, and final alkali activation to ensure that organic matter regulation, heavy metal pre-stabilization, particle surface activation, and gel network formation occur in suitable chemical environments. The ferrous activation of persulfate stage weakens the shielding effect of some organic macromolecules on the gelation reaction and particle interfaces; the calcium carbide slag mineralization stage utilizes Ca... 2+ OH -The process involves the adsorption of pollutants by iron hydrolysis products; the slag co-grinding stage improves the distribution of calcium, iron, and silicon-aluminum components on the surface of sludge particles; and the subsequent water glass and sodium carbonate composite alkali activation system promotes the formation of C-(A)-SH type cementitious products. This continuous process can improve the surface condition of sludge particles and their interfacial bonding with the cementitious matrix, and enhance the stability of heavy metals and the continuity of the cementitious structure.
[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) Ferrous activation persulfate oxidation and calcium carbide slag mineralization are carried out in stages. Oxidation is first carried out under near-neutral conditions to avoid premature addition of calcium carbide slag and rapid quenching of free radicals; after the residual persulfate is reduced, the pH is increased so that the iron species are hydrolyzed and together with the calcium-containing precipitate phase, they undertake the pre-stabilization function of pollutant elements.
[0024] (2) The mineralized conditioner and the reserved slag are co-ground to form a composite modified sludge precursor. The mechanical action exposes the edges and defect sites of clay minerals, while promoting the uniform loading of calcium- and iron-containing mineralized products and active silica-alumina components on the surface of sludge particles. After the modified sludge precursor enters the composite alkali-activated system, it can shorten the mass transfer distance between sludge particles and cementation products and improve the interfacial bonding.
[0025] (3) Synergistic effect of slag-carbide slag composite cementing system and water glass-sodium carbonate composite activating system. Slag provides the active Si and Al components required to form the cementing network, while carbide slag provides Ca. 2+ and OH - The coupling reaction of sodium carbonate with Ca(OH)₂ can gradually increase the alkalinity of the liquid phase and promote the nucleation and pore filling of carbonates, while water glass replenishes the soluble silica source and promotes gel condensation. This can regulate the early reaction rate, avoid excessively slow slurry coagulation or excessively rapid local reactions, and promote the continuous formation of C-(A)-SH gels in the later stage while maintaining the stability of the pores.
[0026] (4) The macroscopic properties are jointly regulated by the lightweighting of foam, the toughening of polyethylene fiber and the thermal insulation of aerogel. The pre-fabricated foam reduces the bulk density, the hydrophobic silica aerogel and macroscopic pores form a multi-scale thermal insulation structure, and the polyethylene fiber inhibits the propagation of microcracks in the pore walls and matrix through bridging. Detailed Implementation
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0029] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0030] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0031] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0032] This invention sequentially links ferrous activation persulfate oxidation, alkaline mineralization with carbide slag, slag co-grinding activation, and subsequent alkaline activation reactions. In the oxidation stage, sulfate free radicals and their transformed active species are used to break down some humic substances and fulvic acid and other organic macromolecules, improving sludge dewatering and particle surface accessibility. Subsequently, carbide slag is added, transitioning the system from the oxidation stage to the alkaline mineralization stage, where the carbide slag provides Ca2+. 2+ and OH - The Fe(III) hydrolysis products and calcium-containing precipitates formed after oxidation adsorb various heavy metal pollutants such as Pb, Cu, Zn, Cr, Ni, and Cd. Further co-milling with a small amount of slag allows the calcium- and iron-containing mineralization products and active silica-alumina components to be uniformly loaded onto the surface of the sludge particles. The resulting modified sludge precursor, after activation by a composite alkali activation system of water glass and sodium carbonate, forms a continuous solidified network with the remaining slag and carbide slag, primarily composed of C-(A)-SH gels. This network, along with foam, polyethylene fiber, and aerogel, contributes to lightweight, crack-resistant, and thermally insulating properties.
[0033] This invention provides a method for preparing an alkali-activated lightweight and high-strength thermal insulation material of sludge synergistically modified by oxidation and mineralization, comprising the following steps: S1, the original silt was passed through a 5 mm sieve to remove stones, plant residues, shells and other impurities, the moisture content was measured and the dry basis mass was calculated, the dry solids mass fraction was adjusted to 25% to 35% with deionized water, and the initial pH was adjusted to 6.0 to 7.5 with dilute sulfuric acid and sodium hydroxide solution. S2, prepare a 5%–10% (w / w) solution of ferrous salt and add it to the sludge obtained in step S1, mixing for 5–10 minutes; separately, prepare a 5%–10% (w / w) solution of persulfate and add it in batches or dropwise over 10–20 minutes, controlling the amount of persulfate to be 0.5%–2.0% of the dry weight of the sludge, Fe 2+ With S2O8 2- The molar ratio is 0.3–0.9, and the reaction is carried out at 20–35°C with stirring for 30–120 min. S3. Residual persulfate is detected using iodometric titration or other equivalent methods. When the residual amount is not higher than 5% of the initial dosage, the carbide slag reserved from the total formula is used to prepare a slurry with a solid mass fraction of 10% to 30%. The oxidative conditioning sludge is slowly added, the pH is adjusted to 10.0 to 11.5 and stirred for 20 to 40 minutes. Then, the slag reserved from the total formula is added, and the mixture is continued to be mixed for 10 to 20 minutes and aged for 2 to 6 hours. S4. The oxidized-mineralized conditioning material obtained in step S3 is centrifuged and dehydrated, and dried at 60-80°C to constant weight to obtain the dried conditioning material. The drying temperature should be below 105°C to reduce the risk of rapid volatilization of organic residues and hard agglomeration of particles after oxidized conditioning. S5. The dried and prepared material is co-milled for 20–60 min and passed through a 200-mesh sieve to obtain a D50 of 10–30 μm and a specific surface area of 400–650 m². 2 / kg of modified sludge precursors ensures that calcium- and iron-containing mineral products and active silica-alumina components are evenly distributed on the surface of sludge particles. S6. Weigh out the modified sludge precursor, residual slag, residual carbide slag, water-reducing agent (0.80-0.98 parts), polyethylene fiber (0.20-0.60 parts), and SiO2 aerogel (1-3 parts) by weight. Separate the slag from the residual slag for pre-dispersing SiO2 aerogel and polyethylene fiber. Premix the SiO2 aerogel and slag at a mass ratio of 1:3, and dry-disperse the polyethylene fiber and slag at a mass ratio of 1:5. Dry-mix the modified sludge precursor, the remaining slag, and the residual carbide slag at 40-60 r / min for 2-4 min, then add the two premixes in sequence and continue stirring for 1-3 min. S7. Sodium carbonate is added to part of the mixing water and dissolved completely. Then water glass with a modulus of 1.8 and a solid content of 38% to 42% is added. The mixture is stirred evenly and allowed to stand for 10 to 20 minutes to obtain a composite alkali activator. S8. Slowly add the composite alkali activator, water-reducing agent and remaining mixing water to the mixture obtained in step S6, stir at 80-120 r / min for 2-4 min, and then stir at 150-250 r / min for 1-3 min to obtain a uniform base slurry. S9, dilute the composite foaming agent 20 to 40 times and make it into pre-made foam through a physical foaming mechanism, add it to the base slurry in 3 parts, and stir at a low speed of 30 to 60 r / min for 1 to 3 min; S10: Pour the obtained slurry into the mold and cover it with a film. After standing for 24 to 48 hours, remove it from the mold and cure it at 20±2℃ and relative humidity not less than 95% until the specified age.
[0034] Unless otherwise specified, the technical solutions described in this invention are all conventional solutions in the field, and the reagents or raw materials used are all purchased from commercial channels or are publicly available unless otherwise specified.
[0035] The present invention is illustrated below using paired experiments: Examples 1 to 6 all use modified sludge precursors that have undergone a complete process of ferrous activation persulfate oxidation, carbide slag mineralization, and slag co-grinding activation; Comparative Examples 1 to 6 use the same batch of sludge, the same mix ratio, and the same curing regime as Examples 1 to 6, the only difference being that the comparative examples use ordinary dried ball-milled sludge powder.
[0036] The slag used in this embodiment of the invention is S95 grade granulated blast furnace slag powder, which is grayish-white powder with an apparent density of 2.89 g / cm³. 3 Specific surface area is 445 m² 2 / kg, with a moisture content of less than 1.0%. XRD analysis results show that the slag is mainly composed of an amorphous glassy phase and has high potential cementitious activity. The slag mainly contains components such as CaO, SiO2, Al2O3 and MgO, and can undergo glassy phase depolymerization and subsequent condensation reactions under alkaline conditions.
[0037] The calcium carbide slag used is a solid waste generated during the industrial hydrolysis of calcium carbide to produce acetylene. The undisturbed calcium carbide slag was dried to constant weight in an 80℃ forced-air drying oven, then preliminarily crushed by a crusher, and finally ball-milled for 30 minutes. After passing through a 200-mesh sieve, calcium carbide slag powder was obtained. The median particle size D50 of the obtained calcium carbide slag powder was approximately 44.7 μm, and the specific surface area was approximately 510 m². 2 / kg, with a Ca(OH)2 content of approximately 82%. The high Ca(OH)2 content in the carbide slag can provide Ca to the system. 2+ and a certain amount of OH -It forms a synergistic activating effect with slag and composite alkali activator.
[0038] The silt was taken from the bottom sediment generated by river and lake dredging projects. The initial organic matter content of the undisturbed silt after impurity removal through a 5 mm sieve was approximately 20.4%, and the pH was 7.3. The silt used in Examples 1-6 was successively subjected to ferrous activated persulfate oxidation, carbide slag mineralization, low-temperature drying, and slag co-milling to obtain modified silt precursors; in Comparative Examples 1-6, the same batch of silt was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve, resulting in ordinary silt powder with a D50 of approximately 23.6 μm.
[0039] The ferrous salts used in Examples 1-6 were all ferrous sulfate heptahydrate (FeSO4·7H2O), and the persulfates used were all sodium persulfate (Na2S2O8). The preparation method of the modified sludge precursor is as follows: S1. The undisturbed silt was passed through a 5 mm sieve to remove stones, plant debris, shells and other impurities. The moisture content was measured and the dry weight of the silt was calculated. Based on the dry solids mass fraction of the undisturbed silt, the dry solids mass fraction was adjusted to 30% by centrifugation or by adding deionized water. The initial pH was then adjusted to 6.5 using a dilute sulfuric acid solution.
[0040] S2, prepare an 8% (w / w) aqueous solution of ferrous sulfate heptahydrate, add it to the sludge obtained in step S1, and mix for 8 min; separately, prepare an 8% (w / w) aqueous solution of sodium persulfate, add it dropwise to the sludge over 15 min, and stir the reaction at 25±2℃. In Examples 1-6, the amount of sodium persulfate used is 0.5%–2.0% of the dry weight of the sludge. 2+ With S2O8 2- The molar ratio is 0.30 to 0.90, and the oxidation time is 30 to 120 min. For specific values, please refer to the corresponding examples.
[0041] S3. Residual sodium persulfate was detected using iodometric titration. When the residual amount was no more than 5% of the initial addition, oxidized and conditioned sludge was obtained. A slurry with a solid mass fraction of 20% was prepared from the carbide slag reserved in the total amount of the corresponding embodiment formula. This slurry was slowly added to the oxidized and conditioned sludge, and the pH of the system was controlled at 11.0 ± 0.2. Stirring was continued for 30 min. Subsequently, slag reserved in the total amount of the corresponding embodiment formula was added, and mixing was continued for 15 min followed by aging. In Examples 1-6, the amount of reserved carbide slag was 5%–15% of the dry sludge mass, the amount of reserved slag was 2%–10% of the dry sludge mass, and the aging time was 2–6 h. Specific values are given in the corresponding embodiments.
[0042] S4. The aged product obtained in step S3 is centrifuged and dehydrated, and then dried at 70°C to constant weight to obtain the dried conditioner.
[0043] S5, the dried conditioning material is co-milled and passed through a 200-mesh sieve to obtain the modified sludge precursor. The co-milling time in Examples 1-6 is 30-60 min, and the specific values are given in the corresponding examples.
[0044] The main chemical compositions of slag, carbide slag, ordinary sludge powder, and modified sludge precursor were determined using X-ray fluorescence spectrometry. Ordinary sludge powder was obtained by drying the impurity-removed undisturbed sludge to constant weight at 80℃, ball milling for 45 min, and passing it through a 200-mesh sieve; this powder was used for comparative examples 1–6. The modified sludge precursor was represented by the sample prepared in Example 3. The determination results are shown in Table 1.
[0045] Table 1. Main chemical composition (%) of slag, carbide slag, and sludge before and after modification
[0046] Table 1 shows that the slag contains high levels of CaO, SiO2, and Al2O3, which can provide the main active Ca, Si, and Al components for the alkali-activated reaction. The carbide slag is mainly composed of calcium-containing components, which can provide a calcium source for the depolymerization of the glassy phase of the slag and the formation of C-(A)-SH type cementitious products. Ordinary sludge powder mainly contains SiO2, Al2O3, Fe2O3, and CaO, indicating that the original sludge contains quartz, clay minerals, and iron-containing minerals. In Example 3, the modified sludge precursor, after ferrous activation persulfate oxidation, carbide slag mineralization, and slag co-grinding, exhibits a higher CaO content compared to ordinary sludge powder, and also contains abundant SiO2, Al2O3, and Fe2O3, which can provide calcium-containing components and active silicon-aluminum components for the subsequent alkali-activated reaction.
[0047] Ordinary sludge powder was acid digested, and the content of typical heavy metal elements was determined by inductively coupled plasma atomic emission spectrometry. Cr, Cu, Zn, Pb, Ni and Cd were selected as representative evaluation indicators, and their initial contents are shown in Table 2.
[0048] Table 2. Content of typical heavy metal elements in silt
[0049] The water glass is liquid sodium silicate water glass with a modulus of 1.8 and a solid content of 40%, of which the mass fraction of Na2O is approximately 14.6%; the sodium carbonate is industrial-grade anhydrous Na2CO3 with a purity of not less than 98%. The water glass and sodium carbonate together constitute a composite alkali activator, and the total alkali equivalent of the composite alkali activator is calculated based on the percentage of Na2O in the total mass of the slag and carbide slag.
[0050] In each embodiment, the sodium carbonate content was controlled at 2% of the total mass of slag and carbide slag, with the remaining Na2O equivalent supplemented by liquid water glass with a modulus of 1.8 and a solid content of 40%. This method allows sodium carbonate to primarily play a role in regulating alkalinity and early reaction rates, while the water glass, in addition to providing an alkaline environment, also supplements the soluble silicon source.
[0051] The water-reducing agent used was a polycarboxylate-based high-performance water-reducing agent, purchased from Jiangsu Subote New Material Co., Ltd., with a solid content of 40%. The polyethylene fiber used was high-strength polyethylene short-cut fiber, with a length of 9 mm, an average diameter of approximately 20 μm, and a density of approximately 0.97 g / cm³. 3 The tensile strength is not less than 2500 MPa. Before use, the polyethylene fiber is pre-dispersed with a small amount of slag powder in a dry state to reduce the agglomeration phenomenon that occurs when the fiber is directly added to the slurry.
[0052] The aerogel used was hydrophobic SiO2 aerogel particles, purchased from Sinopharm Chemical Reagent Co., Ltd., with a particle size mainly distributed between 0.2 and 1.0 mm and a bulk density of approximately 80 kg / m³. 3 The porosity is approximately 95%, and the thermal conductivity at room temperature is approximately 0.018 W / (m·K). Before use, the aerogel is premixed with slag at a mass ratio of 1:3 to ensure that the aerogel particles are uniformly attached to and dispersed in the slag powder, thereby reducing the floating and agglomeration that may occur after direct addition to the liquid phase.
[0053] The plant protein hydrolysate is enzymatically hydrolyzed soybean protein, purchased from Beijing Hongrun Baoshun Technology Co., Ltd., product number HRBS-Y005A, reagent grade. The soybean protein peptone is a light yellow to brown powder with a total nitrogen content of not less than 8.0% on a dry basis, an amino nitrogen content of not less than 2.0% on a dry basis, a moisture content of not more than 7.0%, and an ash content of not more than 17.0% on a dry basis. Its 2% aqueous solution has a pH of 6.8–7.2. The composite foaming agent is prepared by mixing the above-mentioned plant protein hydrolysate, sodium α-alkenyl sulfonate, cocamidopropyl betaine, hydroxypropyl methylcellulose, and water in a mass ratio of 12:3:1.5:0.4:83.1. Before use, the composite foaming agent is diluted with water at a mass ratio of 1:30, and pre-made foam is prepared using a compressed air physical foaming machine, controlling the density of the freshly made foam to be 65±5 kg / m³. 3 .
[0054] The preparation method of alkali-activated lightweight high-strength thermal insulation material of sludge synergistically modified by oxidation-mineralization in this embodiment of the invention includes the following steps: The modified sludge precursor was prepared according to the aforementioned method, wherein the carbide slag and slag used for mineralization and co-grinding were both taken from the total feed amount of the formulation in the corresponding embodiment. According to the formulation of the corresponding embodiment, all the obtained modified sludge precursor and the remaining slag and carbide slag after deducting the amount of the modified sludge precursor for preparation were weighed. Slag for pre-dispersing SiO2 aerogel and polyethylene fiber were separated from the remaining slag. The SiO2 aerogel and slag were premixed at a mass ratio of 1:3, and the polyethylene fiber and slag were dry-dispersed at a mass ratio of 1:5. Subsequently, the modified sludge precursor, the remaining slag after deducting the above pre-dispersed amount, and the remaining carbide slag were added to a mixer and stirred at 60 r / min for 3 min; the premix of SiO2 aerogel and slag was added, and stirring continued for 2 min; then the premix of polyethylene fiber and slag was slowly and gradually added, and stirring continued at 60 r / min for 2 min to obtain a dry mixture.
[0055] Add the weighed sodium carbonate to part of the mixing water and stir thoroughly until completely dissolved. After the solution temperature returns to room temperature, add liquid water glass, stir for 3 minutes and let stand for 15 minutes to obtain the composite alkali activator.
[0056] Add the composite alkali activator, water-reducing agent and remaining mixing water to the dry mixture, stir at 120 r / min for 2 min, and then increase to 200 r / min for 2 min to form a uniform basic slurry from the modified sludge precursor, the remaining slag and the remaining carbide slag.
[0057] The amount of pre-made foam added was determined through trial mixing based on the target wet density set in each embodiment. The determined amount of pre-made foam was added to the base slurry in three portions, and after each addition, it was stirred at a low speed of 40-50 r / min for 30-40 s; after all the pre-made foam was added, it was stirred at a low speed for another 60 s to ensure that the foam was evenly distributed in the slurry, while avoiding a large number of foam breakages caused by high-speed shearing.
[0058] The obtained slurry is poured into a mold, and without mechanical vibration, the surface is only slightly scraped smooth. Then, it is covered with a polyethylene film and left to stand for 24 hours. After demolding, it is placed in an environment with a temperature of 20±2℃ and a relative humidity of not less than 95% for curing to the specified age.
[0059] The 7-day and 28-day compressive strengths were determined according to JG / T 266-2011 "Foamed Concrete". 100 mm × 100 mm × 100 mm cube specimens were used, with 3 parallel specimens set for each group. The average value of the 3 specimen test values was taken as the final result.
[0060] Thermal conductivity was determined according to GB / T 10294-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Thermal Insulation Materials - Protective Hot Plate Method", using a 300 mm × 300 mm × 30 mm plate specimen. The specimen was cured for 28 days and then dried. During testing, the cold plate temperature was set to 15℃ and the hot plate temperature to 35℃. The thermal conductivity was recorded after the heat flow reached a steady state.
[0061] The drying shrinkage performance was determined according to GB / T 11969-2020 "Test Methods for Performance of Autoclaved Aerated Concrete", using 40 mm × 40 mm × 160 mm prism specimens. After the specimens reached the specified initial age, the reference length was measured, and they were dried in an environment with a temperature of 20±2℃ and a relative humidity of 60±5%. The length changes at 1 day, 7 days, 14 days, 21 days, and 28 days were recorded. The drying shrinkage rate at 28 days was calculated according to formula (1): (1) In the formula L 0 As the reference length, L t For drying t The length of the specimen after the event.
[0062] The heavy metal leaching test was conducted according to HJ 557-2010 "Leaching Toxicity of Solid Waste - Horizontal Oscillation Method". 28-day cured samples were crushed and passed through a 3 mm sieve. 100 g of dry weight of the sample was weighed, and secondary water meeting the requirements of GB / T 6682 was added as the leaching agent at a liquid-to-solid ratio of 10:1 L / kg. The sample was horizontally oscillated at 110±10 times / min and an amplitude of 40 mm for 8 h at room temperature, followed by standing for 16 h. The solution was then filtered through a 0.45 μm filter membrane, and the concentrations of Cr, Cu, Zn, Pb, Ni, and Cd in the leachate were determined using ICP-OES. Another batch of cured samples was acid-digested to determine the total content of each heavy metal element in the cured material, which was used to calculate the heavy metal leaching rate. The heavy metal leaching rate was calculated according to formula (2): (2) In the formula, L i For the first i Leaching rate of several heavy metal elements; C i This refers to the concentration of the element in the leachate; V This represents the volume of the extract. m The dry mass of the solid sample used in the leaching test; W i This refers to the total content of the corresponding heavy metal elements in the same batch of cured materials.
[0063] The organic matter content of the sludge was determined according to HJ 761—2015 "Determination of Organic Matter in Solid Waste by Loss on Ignition Method": The sludge sample was cleaned, ground, and passed through a 0.25 mm sieve. It was dried at 105±5 ℃ to constant weight. About 0.5 g of the dried sample was weighed and placed in a pre-weighed porcelain crucible. The total mass of the crucible and sample was m1, and the mass of the empty crucible was m0. Then, it was ignited in a muffle furnace at 600±20 ℃ for 3 h, cooled in a desiccator, and weighed. The ignition was repeated until the difference between two adjacent weighings did not exceed 0.001 g. The total mass of the crucible and residue was recorded as m2. The organic matter content of the sludge was calculated according to formula (3): (3) Example 1 The following components were used: 64 parts slag, 16 parts calcium carbide slag, and 20 parts dry sludge. The total alkali equivalent was 4.0%, the water-cement ratio was 0.30, the water-reducing agent was 0.80 parts, the polyethylene fiber was 0.20 parts, and the SiO2 aerogel was 1.0 part. The designed wet density was 620±20 kg / m³. 3 Adjust the dry solids content of the cleaned wet sludge to 30% and the pH to 6.5; according to Fe... 2+ With S2O8 2- The amount of FeSO4·7H2O was calculated based on a molar ratio of 0.30, and prepared into an 8% (w / w) aqueous solution. This solution was added to the sludge and mixed for 8 min. Separately, 0.10 parts of Na2S2O8 (0.50% of the dry weight of the sludge) were prepared into an 8% (w / w) aqueous solution and added dropwise to the sludge over 15 min. The sludge was then oxidized at 25±2℃ for 30 min. After the residual persulfate was no more than 5% of the initial amount, 1.00 parts of reserved carbide slag were added, the pH was adjusted to 10.8–11.2, and the mixture was stirred for 30 min. Then, 0.40 parts of reserved slag were added, the mixture was aged for 2 h, dried at 70℃ to constant weight, co-milled for 30 min, and passed through a 200-mesh sieve. The resulting modified sludge precursor was mixed with the remaining 63.60 parts of slag and 15.00 parts of carbide slag. Subsequent pulping, foaming, and curing were carried out according to the aforementioned general methods.
[0064] Example 2 The sample consisted of 62.4 parts slag, 15.6 parts calcium carbide slag, and 22 parts dry sludge, with a total alkali equivalent of 4.5%, a water-cement ratio of 0.29, 0.858 parts water-reducing agent, 0.30 parts polyethylene fiber, and 1.50 parts SiO2 aerogel. The designed wet density was 610±20 kg / m³. 3 Adjust the dry solids content of the cleaned wet sludge to 30% and the pH to 6.5; according to Fe... 2+ With S2O8 2-The amount of FeSO4·7H2O was calculated based on a molar ratio of 0.45, and prepared into an 8% (w / w) aqueous solution. This solution was added to the sludge and mixed for 8 min. Separately, 0.176 parts of Na2S2O8 (0.80% of the dry weight of the sludge) were prepared into an 8% (w / w) aqueous solution and added dropwise to the sludge over 15 min. The sludge was then oxidized at 25±2℃ for 45 min. After the residual persulfate was no more than 5% of the initial amount, 1.76 parts of reserved carbide slag were added, the pH was adjusted to 10.8–11.2, and the mixture was stirred for 30 min. Then, 0.88 parts of reserved slag were added, the mixture was aged for 3 h, dried at 70℃ to constant weight, co-milled for 40 min, and passed through a 200-mesh sieve. The resulting modified sludge precursor was mixed with the remaining 61.52 parts of slag and 13.84 parts of carbide slag. Subsequent pulping, foaming, and curing were carried out according to the aforementioned general methods.
[0065] Example 3 The following components were used: 60 parts slag, 15 parts calcium carbide slag, and 25 parts dry sludge. The total alkali equivalent was 5.0%, the water-cement ratio was 0.28, the water-reducing agent was 0.90 parts, the polyethylene fiber was 0.40 parts, and the SiO2 aerogel was 2.0 parts. The designed wet density was 600±20 kg / m³. 3 Adjust the dry solids content of the cleaned wet sludge to 30% and the pH to 6.5; according to Fe... 2+ With S2O8 2- The amount of FeSO4·7H2O was calculated based on a molar ratio of 0.60, and it was prepared into an 8% (w / w) aqueous solution. This solution was added to the sludge and mixed for 8 min. Separately, 0.25 parts of Na2S2O8 (1.00% of the dry weight of the sludge) were prepared into an 8% (w / w) aqueous solution and added dropwise to the sludge over 15 min. The oxidative reaction was carried out at 25±2℃ for 60 min. After the residual persulfate was no more than 5% of the initial amount, 2.50 parts of reserved carbide slag were added, the pH was adjusted to 10.8–11.2, and the mixture was stirred for 30 min. Then, 1.25 parts of reserved slag were added, and the mixture was aged for 4 h. It was then dried at 70℃ to constant weight, co-milled for 45 min, and passed through a 200-mesh sieve. The resulting modified sludge precursor was mixed with the remaining 58.75 parts of slag and 12.50 parts of carbide slag and then molded and cured using general methods.
[0066] Example 4 The sludge modification parameters were the same as in Example 3; the dry basis of slag, carbide slag, and sludge remained 60 parts, 15 parts, and 25 parts, respectively; the total alkali equivalent was increased to 5.5%; the water-cement ratio was 0.27; the water-reducing agent was 0.975 parts; the polyethylene fiber was 0.50 parts; the SiO2 aerogel was 2.50 parts; and the designed wet density was 590±20 kg / m³. 3 The obtained modified sludge precursor was mixed with the remaining 58.75 parts of slag and 12.50 parts of carbide slag, and then molded and cured according to general methods.
[0067] Example 5 The sample consisted of 57.6 parts slag, 14.4 parts calcium carbide slag, and 28 parts dry sludge, with a total alkali equivalent of 6.0%, a water-cement ratio of 0.27, 0.864 parts water-reducing agent, 0.50 parts polyethylene fiber, and 2.0 parts SiO2 aerogel. The designed wet density was 600±20 kg / m³. 3 Adjust the dry solids content of the cleaned wet sludge to 30% and the pH to 6.5; according to Fe... 2+ With S2O8 2- The amount of FeSO4·7H2O was calculated based on a molar ratio of 0.75, and prepared into an 8% (w / w) aqueous solution. This solution was added to the sludge and mixed for 8 min. Separately, 0.42 parts of Na2S2O8 (1.50% of the dry weight of the sludge) were prepared into an 8% (w / w) aqueous solution and added dropwise to the sludge over 15 min. The oxidative reaction was carried out at 25±2℃ for 90 min. After the residual persulfate was no more than 5% of the initial amount, 3.36 parts of reserved carbide slag were added, the pH was adjusted to 10.8–11.2, and the mixture was stirred for 30 min. Then, 2.24 parts of reserved slag were added, the mixture was aged for 5 h, dried at 70℃ to constant weight, co-milled for 50 min, and passed through a 200-mesh sieve. The resulting modified sludge precursor was mixed with the remaining 55.36 parts of slag and 11.04 parts of carbide slag. Subsequent pulping, foaming, and curing were carried out according to the aforementioned general methods.
[0068] Example 6 The following components were used: 56 parts slag, 14 parts calcium carbide slag, and 30 parts dry sludge. The total alkali equivalent was 5.5%, the water-cement ratio was 0.30, the water-reducing agent was 0.98 parts, the polyethylene fiber was 0.60 parts, and the SiO2 aerogel was 3.0 parts. The designed wet density was 570±20 kg / m³. 3 Adjust the dry solids content of the cleaned wet sludge to 30% and the pH to 6.5; according to Fe... 2+ With S2O8 2- The amount of FeSO4·7H2O was calculated based on a molar ratio of 0.90, and prepared into an 8% (w / w) aqueous solution. This solution was added to the sludge and mixed for 8 min. Separately, 0.60 parts of Na2S2O8 (2.00% of the dry weight of the sludge) were prepared into an 8% (w / w) aqueous solution and added dropwise to the sludge over 15 min. The oxidative reaction was carried out at 25±2℃ for 120 min. After the residual persulfate was no more than 5% of the initial amount, 4.50 parts of reserved carbide slag were added, the pH was adjusted to 10.8–11.2, and the mixture was stirred for 30 min. Then, 3.00 parts of reserved slag were added, the mixture was aged for 6 h, dried at 70℃ to constant weight, co-milled for 60 min, and passed through a 200-mesh sieve. The resulting modified sludge precursor was mixed with the remaining 53.00 parts of slag and 9.50 parts of carbide slag. Subsequent pulping, foaming, and curing were carried out according to the aforementioned general methods.
[0069] Comparative Example 1 The same batch of purified sludge as in Example 1 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 1.
[0070] Comparative Example 2 The same batch of purified sludge as in Example 2 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 2.
[0071] Comparative Example 3 The same batch of purified sludge as in Example 3 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 3.
[0072] Comparative Example 4 The same batch of purified sludge as in Example 4 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 4.
[0073] Comparative Example 5 The same batch of purified sludge as in Example 5 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 5.
[0074] Comparative Example 6 The same batch of purified sludge as in Example 6 was used, without the addition of ferrous salts and persulfates, and without carbide slag mineralization or slag co-grinding. The sludge was dried to constant weight at 80°C, ball-milled for 45 min, and passed through a 200-mesh sieve. Except for replacing the modified sludge precursor with ordinary sludge powder of the same dry basis weight, the remaining final raw material proportions, total alkali equivalent, water-cement ratio, water-reducing agent, fiber, aerogel, target wet density, mixing regime, and curing conditions were the same as in Example 6.
[0075] The experimental data for the examples and comparative examples are shown in Tables 3, 4 and 5.
[0076] Table 3 Organic matter content of sludge before and after modification
[0077] Table 4 Heavy metal leaching rates (%) of the examples and paired comparative examples
[0078] Table 5 Mechanical, thermal insulation, and drying shrinkage properties of the examples and paired comparative examples
[0079] The main difference between silt and inorganic solid raw materials such as slag and carbide slag lies in its higher organic matter content. The original silt used in this invention has an organic matter content of 20.40%, in which organic components such as humic acid and fulvic acid consume the OH groups in the system. - Organic matter adsorbs onto the surface of slag and sludge particles, hindering the dissolution of active silicon and aluminum components and the deposition of cementitious products on the particle surface, thus reducing the continuity of the cementitious structure. Simultaneously, organic matter increases the water demand of the sludge, reduces slurry fluidity and foam stability, thereby adversely affecting material strength and pore structure. This invention uses ferrous activated persulfate to oxidize and modify the sludge. 2+ Activation of persulfate ions generates sulfate radicals and hydroxyl radicals, which are highly oxidizing, causing chain scission, ring opening, and oxidative decomposition of large organic molecules such as humic substances; the Fe produced in the reaction... 3+ Further hydrolysis forms an iron hydroxyl precipitate, which adsorbs and co-precipitates residual organic matter and heavy metal ions. Subsequently, carbide slag is added, utilizing its provided Ca(OH)₂ to neutralize the acidic substances produced during oxidation and to allow Ca to... 2+ It reacts with carbonate, sulfate, and other ions in the system to form calcium-containing mineralization products. After the above treatment, the organic matter content of the sludge in each example decreased from 20.40% to 3.96%–5.86%, which is significantly lower than the 18.72%–19.25% of the comparative example, indicating that ferrous activated persulfate oxidation and calcium carbide slag mineralization have a good synergistic modification effect.
[0080] Co-milling modified sludge with a portion of slag can disrupt particle agglomeration through mechanical shearing and collision, increasing particle specific surface area and surface defects, thus fully exposing the active silica-alumina components in the slag. In the alkaline environment formed by water glass and sodium carbonate, the glassy phase of the slag undergoes depolymerization and condensation, reacting with the Ca provided by the calcium carbide slag. 2+ The reaction generates C-(A)-SH gel; the generated gel and calcium-containing mineralization products fill the gaps between particles and coat the silt particles, limiting the migration of heavy metals through adsorption, ion exchange, precipitation, and physical encapsulation, thus controlling the heavy metal leaching rate in all embodiments to within 3%. Simultaneously, pre-fabricated foam and aerogel construct multi-scale insulating pores, and polyethylene fibers inhibit crack propagation in the foam walls and gel matrix through bridging, thereby balancing the material's lightweight, thermal insulation, strength, and volume stability.
[0081] The wet density of the oxidative-mineralization synergistic modified sludge lightweight high-strength thermal insulation material prepared in the embodiments of the present invention is 570-620 kg / m³. 3 The 7-day compressive strength is 2.58–3.49 MPa, the 28-day compressive strength is 3.38–4.56 MPa, the 28-day thermal conductivity is 0.092–0.142 W / (m·K), and the 28-day drying shrinkage rate is 0.168%–0.211%. This invention effectively reduces the adverse effects of silt organic matter on alkali-activated gelation reactions, improves the activity of silt particles and the stability of heavy metals, and the resulting material can be used for building insulation filling, roadbed backfilling, and underground cavity filling.
[0082] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. An alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification by oxidation and mineralization, characterized in that, By weight, the raw materials include: The composition includes 53-64 parts of slag, 9.5-16 parts of calcium carbide slag, 20-38 parts of modified sludge precursor, 0.20-0.60 parts of polyethylene fiber, 1.0-3.0 parts of SiO2 aerogel, 0.80-0.98 parts of water-reducing agent, composite alkali activator and composite foaming agent; The composite alkali activator is composed of water glass and sodium carbonate. The total alkali equivalent of the composite alkali activator is 4.0% to 6.0% of the total mass of slag and carbide slag based on Na2O. The sodium carbonate content is 2% of the total mass of slag and carbide slag, and the remainder is supplemented by liquid sodium silicate water glass.
2. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 1, characterized in that, The method for preparing the modified sludge precursor includes the following steps: S1. Remove impurities from the original sludge, determine the moisture content and calculate the dry basis mass, adjust the dry solids mass fraction to 25% to 35% with deionized water, and adjust the initial pH to 6.0 to 7.5; S2. Add ferrous salt aqueous solution and mix for 5-10 min, then add persulfate solution in batches or dropwise over 10-20 min, controlling the persulfate dosage to be 0.5%-2.0% of the dry sludge mass. Fe 2+ With S2O8 2- The molar ratio is 0.3–0.9, and the reaction is carried out at 20–35°C with stirring for 30–120 min. S3. Detect residual persulfate. When the residual amount is not higher than 5% of the initial amount, add carbide slag slurry, adjust the pH of the system to 10.0-11.5 and stir for 20-40 min, then add slag, continue mixing for 10-20 min and age for 2-6 h. S4. Centrifuge the aged product obtained in step S3 to remove water, and dry it at 60-80℃ to constant weight; S5. Grind the dried and conditioned material obtained in step S4 for 20–60 min and pass it through a 200-mesh sieve to obtain a D50 of 10–30 μm and a specific surface area of 400–650 m². 2 / kg of modified sludge precursor.
3. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 2, characterized in that, The ferrous salt is one or more of ferrous sulfate, ferrous chloride and their hydrates; the persulfate is one or more of sodium persulfate, potassium persulfate and ammonium persulfate.
4. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 2, characterized in that, The mass fraction of calcium carbide slag in the calcium carbide slag slurry is 10% to 30%; the amount of calcium carbide slag used is 5% to 15% of the dry weight of the sludge; and the amount of slag used is 2% to 10% of the dry weight of the sludge.
5. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 1, characterized in that, The composite foaming agent is prepared by mixing plant protein hydrolysate, sodium α-alkenyl sulfonate, cocamidopropyl betaine, hydroxypropyl methylcellulose and water in a mass ratio of 10-15:2-4:1-2:0.2-0.6:80-86. When used, it is diluted with water 20-40 times and then processed into pre-made foam by a physical foaming mechanism.
6. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 1, characterized in that, The polyethylene fiber is a high-strength polyethylene short-cut fiber with a length of 6 to 12 mm; the SiO2 aerogel is a hydrophobic silica aerogel particle with an average particle size of 0.1 to 2.0 mm and a thermal conductivity at room temperature of no more than 0.025 W / (m·K).
7. The alkali-activated lightweight high-strength thermal insulation material for alkali-activated sludge synergistic modification according to claim 1, characterized in that, The water-cement ratio of the alkali-activated lightweight high-strength thermal insulation material of the oxidized-mineralized sludge synergistic modification is 0.25–0.30, and the designed wet density is 570 ± 20 kg / m³. 3 ~620±20 kg / m 3 .
8. A method for preparing an alkali-activated lightweight high-strength thermal insulation material of sludge synergistically modified by oxidation-mineralization as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Subtract the slag and carbide slag used to prepare the modified sludge precursor from the total amount of the formula to obtain the remaining slag and remaining carbide slag; separate the slag used for pre-dispersing SiO2 aerogel and polyethylene fiber from the remaining slag to obtain the remaining slag. The modified sludge precursor, the remaining slag and the remaining carbide slag were dry-mixed, and then the premix of SiO2 aerogel and slag and the premix of polyethylene fiber and slag were added in sequence. The mixture was stirred to obtain the dry mixture. Sodium carbonate was dissolved in part of the mixing water. After the solution temperature returned to room temperature, water glass was added, stirred and allowed to stand to obtain a composite alkali activator. Add the composite alkali activator, water-reducing agent and remaining mixing water to the dry mix, stir at 120 r / min for 2 min, then increase to 200 r / min and stir for 2 min to obtain the basic slurry; The composite foaming agent was diluted with water at a mass ratio of 1:30, and pre-made foam was prepared using a compressed air physical foaming machine, with the density of the pre-made foam controlled at 65±5 kg / m³. 3 ; The pre-made foam was added to the base slurry in three parts. After each addition, the mixture was stirred at a low speed of 40-50 r / min for 30-40 s. After all the pre-made foam was added, the mixture was stirred at a low speed for another 60 s. The slurry is poured into the mold without mechanical vibration. The surface is lightly scraped and then covered with a polyethylene film and left to stand for 24 hours. After demolding, it is placed in an environment with a temperature of 20±2℃ and a relative humidity of not less than 95% to cure for the specified age.
9. The preparation method according to claim 8, characterized in that, Before use, the SiO2 aerogel is premixed with slag at a mass ratio of 1:3; before use, the polyethylene fiber is pre-dispersed in a dry state at a mass ratio of 1:
5.
10. The application of the alkali-activated lightweight high-strength thermal insulation material of oxidative-mineralization synergistic modification of sludge as described in any one of claims 1 to 7 in building thermal insulation filling, roadbed backfilling, or underground cavity filling.