A green and environmentally friendly aerogel thermal insulation coating and its preparation method
By replacing virgin fillers with various industrial solid wastes and combining the synergistic effect of silica sol and hydrophobically modified aerogel, the problems of high cost and insufficient crack resistance of aerogel insulation coatings are solved, achieving efficient and environmentally friendly improvement in insulation performance and resource utilization of solid waste, which is suitable for building insulation materials.
Patent Information
- Application Number
- CN202611527681.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aerogel insulation coatings have high costs for virgin fillers, insufficient crack resistance, low environmental friendliness, and limited forms of solid waste resource utilization, making it difficult to achieve the dual benefits of 'cost reduction + efficiency improvement'.
Various industrial solid wastes, such as fly ash cenospheres, microsilica powder, waste alumina slag, calcined waste diatomaceous earth, and recycled rock wool short fibers, are used to replace the original fillers. Through the multi-dimensional physicochemical synergistic effect of silica sol and hydrophobically modified silica aerogel, a multi-level porous structure and silicon-oxygen network are constructed to enhance the bonding strength and crack resistance, while maintaining the Class A non-combustible properties.
It achieves reduced thermal conductivity of the coating, improved bonding strength and crack resistance, reduced raw material costs, reduced carbon emissions, and is suitable for high-performance thermal insulation needs in various scenarios such as building interior and exterior walls, roofs, and cold storage.
Abstract
Description
Technical Field
[0001] This invention relates to the field of building insulation coating technology, specifically to the cross-disciplinary field of solid waste resource utilization and inorganic insulation materials, and in particular to a green and environmentally friendly aerogel insulation coating and its preparation method. Background Technology
[0002] With the continuous advancement of building energy conservation and the "dual-carbon" strategy, high-efficiency thermal insulation materials have become the core carrier for reducing energy consumption in the building sector. Aerogel, due to its ultra-low thermal conductivity resulting from its nanoporous structure, has become a new generation of high-performance thermal insulation materials. Among them, inorganic silica sol tape aerogel thermal insulation coatings, due to their Class A non-combustible, environmentally friendly, and non-toxic characteristics, have broad application prospects in building interior and exterior wall and roof insulation scenarios.
[0003] However, existing aerogel insulation coatings generally have the following shortcomings: First, auxiliary heat insulation fillers and bulk fillers mostly rely on virgin materials such as hollow ceramic microspheres, high-purity aluminum hydroxide, and virgin diatomaceous earth, resulting in high raw material costs and large carbon emissions; Second, single silica sol film-forming systems suffer from problems such as large drying shrinkage, easy cracking, and insufficient bonding strength, with a prominent risk of cracking during thick coating construction; Third, the forms of solid waste resource utilization are limited, mostly involving single-component replacement of fillers, failing to explore the physicochemical synergistic effects between solid waste, the matrix, and the aerogel, making it difficult to achieve the dual benefits of "cost reduction + efficiency improvement".
[0004] At the same time, the annual output of bulk industrial solid wastes such as fly ash cenospheres from the thermal power industry, microsilica powder from the ferroalloy industry, construction waste rock wool, alumina slag from the aluminum processing industry, and food and chemical waste diatomaceous earth is enormous. Traditional stockpiling and landfilling not only occupy land but also pose environmental hazards, and there is an urgent need for high-value-added and large-scale resource utilization pathways.
[0005] Therefore, developing an inorganic Class A non-flammable gel insulation coating that can synergistically replace multiple solid wastes and has both excellent thermal insulation and mechanical crack resistance properties is of great significance for promoting the green and low-carbon transformation of building insulation materials and turning industrial solid waste into valuable resources. Summary of the Invention
[0006] To address the shortcomings of existing inorganic aerogel thermal insulation coatings, such as high cost of virgin fillers, insufficient crack resistance, and low level of green environmental protection, the technical problem to be solved by this invention is to provide a green and environmentally friendly aerogel thermal insulation coating and its preparation method. This method uses a variety of industrial solid wastes to synergistically replace virgin fillers, and through physicochemical synergy, it simultaneously improves core properties such as thermal insulation, strength, and crack resistance, while maintaining Class A non-combustible properties throughout the process, thus achieving a balance between high-value utilization of solid waste and material performance upgrades.
[0007] One technical solution provided by this invention is a green and environmentally friendly aerogel thermal insulation coating, comprising, by mass percentage: 15.0%~18.0% deionized water, 23.0%~25.0% inorganic silica sol binder, 14.0%~15.0% hydrophobically modified silica aerogel, 9.0%~12.0% fly ash cenospheres, 5.0%~7.0% waste alumina slag, 3.0%~5.0% aluminum hydroxide flame retardant powder, and microsilica. The composition includes: 2.0%~4.0% powder, 5.0%~7.0% calcined waste diatomaceous earth, 2.0%~4.0% talc, 3.5%~4.5% rutile titanium dioxide, 0.8%~1.5% recycled rock wool short fiber, 1.6%~2.0% dispersant and wetting agent, 0.8%~1.2% silane coupling agent, 0.4%~0.6% defoamer, 2.0%~2.5% propylene glycol, and 1.0%~1.5% inorganic thickener, with the total of all components being 100%.
[0008] Detailed descriptions of the above core components:
[0009] (1) Fly ash cenospheres: Closed-cell hollow spherical particles separated from fly ash in thermal power plants. They are aluminosilicate solid waste naturally formed by high-temperature combustion of coal powder. The particle size is 30~100 μm, the porosity is ≥80%, and the thermal conductivity is 0.035~0.045 W / (m·K). They are used to replace virgin hollow ceramic microspheres and some bulk fillers.
[0010] (2) Microsilica powder (silica fume): It is an ultrafine dust collected from the flue gas of ferrosilicon and industrial silicon smelting. The amorphous SiO2 content is ≥85%, and the average particle size is 0.1~0.5 μm. It is a by-product solid waste of the ferroalloy industry. It is used to replace some inert fillers and strengthen the film-forming matrix.
[0011] (3) Calcinated waste diatomaceous earth: It is obtained from waste filter aid diatomaceous earth used in the beer, beverage and chemical industries. It is calcined at 500~600℃ to remove organic matter and purify and desalinate. The soluble salt content is ≤0.5% and the porosity is ≥80%. It is used to replace virgin diatomaceous earth and some talc powder.
[0012] (4) Waste alumina slag: It is obtained from the waste slag generated by the aluminum profile anodizing process, and is purified by water washing and ultra-fine grinding. The main components are aluminum hydroxide and activated alumina, with a particle size of 10~30 μm. It is a solid waste from non-ferrous metal processing and is used to partially replace the original aluminum hydroxide flame retardant filler.
[0013] (5) Recycled rock wool short fibers: taken from waste rock wool insulation cotton from building demolition and industrial pipeline elimination, and processed by opening, impurity removal and shearing processes. The fiber length is controlled at 1~3 mm and the thermal conductivity is 0.038~0.045 W / (m·K). It is used to replace virgin glass fiber powder to construct a crack-resistant skeleton.
[0014] (6) Hydrophobic modified silica aerogel: the core thermal insulation component, which adopts silane surface hydrophobic modification to avoid water absorption and pore collapse failure; the original aerogel has a porosity of 85%~95%, a particle size of 20~80 μm, and a thermal conductivity of 0.018~0.024 W / (m·K).
[0015] The preparation method of hydrophobically modified silica aerogel includes the following steps:
[0016] Step S1: Using hexamethyldisilazane or methyltrimethoxysilane as the modifier and anhydrous ethanol as the dispersion solvent, prepare a silane modification solution with a mass concentration of 5% to 10%, and the mass ratio of the modification solution to the aerogel powder is 3:1 to 5:1.
[0017] Step S2: Add the virgin silica aerogel powder into the modification solution and impregnate it at low speed under normal temperature and pressure for 6-12 h, or react it in a water bath at 50-60℃ for 3-6 h with a stirring speed of 80-120 r / min.
[0018] Step S3: After impregnation, filter and separate the aerogel, rinse 2-3 times with anhydrous ethanol, and age in an environment of 40-50℃ for 8-12 hours;
[0019] Step S4: Transfer to a vacuum drying oven at 60℃ and dry for 6~10 h to obtain hydrophobic modified silica aerogel, and store in a sealed container; the original silica aerogel has a porosity of 85%~95%, a particle size of 20~80 μm, and a thermal conductivity of 0.018~0.024 W / (m·K).
[0020] (7) Inorganic silica sol binder: alkaline silica sol, SiO2 content 30%~35%, particle size 10~20 nm, pH value 9.0~10.0; no organic emulsion is added to the whole system, and the combustion performance meets the Class A non-combustible requirements in GB 8624-2012.
[0021] (8) The dispersing and wetting agent is a sodium polyacrylate dispersant; the silane coupling agent is KH550 or KH560; the defoamer is an organosilicon defoamer; and the inorganic thickener is lithium-based bentonite or attapulgite.
[0022] The green and environmentally friendly aerogel thermal insulation coating of this invention achieves simultaneous improvement in thermal insulation, strength, and crack resistance through the multi-dimensional physicochemical synergistic effect of five solid wastes, silica sol, and aerogel. The core mechanism is as follows:
[0023] Synergistic multi-level porous insulation: Constructing a gradient pore structure of "aerogel nanopores + cenosphere micron closed pores + diatomaceous earth mesopores + micro silica powder micro-filling" blocks air convection heat transfer paths at different scales, significantly reducing the overall thermal conductivity of the coating; compared with a single aerogel insulation system, the proportion of convection heat transfer is reduced by more than 20%, and the thermal conductivity of the dry film can be as low as 0.024~0.025W / (m·K).
[0024] Synergistic enhancement of silicon-oxygen network: The highly active amorphous SiO2 in the microsilica powder undergoes a sol-gel condensation reaction with the silica sol during the curing process, forming a continuous and dense three-dimensional Si-O-Si network; the active Al2O3 in the waste alumina slag participates in interfacial bonding, improving the bonding force between the filler and the matrix, and ultimately increasing the coating adhesion strength by more than 25%, while significantly improving water resistance and density.
[0025] Triple crack resistance and toughening synergy: Recycled rock wool short fibers form a three-dimensional interwoven network inside the coating, which prevents crack propagation through bridging; the spherical ball effect of fly ash cenospheres reduces frictional resistance within the system and reduces internal stress from curing shrinkage; the dense silicon-oxygen network matrix enhances the cohesive strength of the material; under the synergistic effect of the three, the coating drying shrinkage rate is reduced by more than 30%, and the impact resistance is greatly improved.
[0026] Synergistic flame retardant performance: Waste alumina slag and aluminum hydroxide decompose simultaneously at high temperatures, absorbing heat and releasing water vapor. Combined with the all-inorganic aluminosilicate matrix, they jointly achieve Class A non-combustibility. Furthermore, the decomposition products can form a dense ceramic phase protective layer, improving the coating stability at high temperatures.
[0027] Another technical solution provided by this invention is a method for preparing a green and environmentally friendly aerogel thermal insulation coating, comprising the following steps:
[0028] Step S1, Premixing and Dispersion: Add the prescribed amounts of deionized water, dispersing and wetting agent, silane coupling agent, defoamer, and propylene glycol to a mixing tank and stir at low speed until uniform; then add microsilica powder, calcined waste diatomaceous earth, waste alumina slag, aluminum hydroxide flame retardant powder, talc powder, and rutile titanium dioxide in sequence, and stir at a speed of 300~500 r / min for 10~15 min until there are no obvious agglomerated particles, thus obtaining the base material slurry.
[0029] Step S2, mixing of lightweight fillers: reduce the stirring speed to 150~250 r / min, add fly ash cenospheres and recycled rock wool short fibers in sequence, stir at low speed for 5~8 min to ensure uniform dispersion and avoid cenosphere breakage and fiber entanglement caused by high speed.
[0030] Step S3, aerogel mixing: Maintain a low stirring speed of 150~250 r / min, slowly and evenly add hydrophobic modified silica aerogel, and continue stirring for 8~12 min after the addition is complete to ensure that the aerogel is evenly dispersed and the nanoporous structure is intact.
[0031] Step S4, film formation and viscosity adjustment: Add the prescribed amount of inorganic silica sol binder and maintain low-speed stirring for 5-10 minutes to mix evenly; finally, add inorganic thickener in batches to adjust the viscosity of the system to 80-120 s (25℃) of Fore-4 cup, stir evenly, and then filter through a 100-mesh sieve to obtain the finished coating.
[0032] Furthermore, high-speed shear dispersion, sand milling, ball milling and other strong shear processes are prohibited throughout the entire preparation process. The maximum stirring speed shall not exceed 600 r / min to avoid the breakage of the aerogel nanoporous structure and the rupture of the bead walls, which would lead to a decrease in thermal insulation performance.
[0033] Compared with existing technologies, the green and environmentally friendly aerogel thermal insulation coating and its preparation method of this invention have the following advantages:
[0034] (1) Comprehensive performance upgrade: Through the synergistic effect of multiple solid wastes, the thermal conductivity of the coating is as low as 0.024 W / (m·K), and the bonding strength, crack resistance and water resistance are significantly better than ordinary inorganic aerogel coatings. At the same time, it maintains the Class A non-combustible rating in GB 8624-2012, and is suitable for the insulation needs of multiple scenarios such as building interior and exterior walls, roofs, and cold storage.
[0035] (2) High-value utilization of solid waste: It can dispose of bulk solid waste from multiple industries such as thermal power, metallurgy, construction, aluminum processing and chemical industry. The solid waste replacement rate accounts for 40% to 55% of the total filler, which greatly reduces the cost of raw materials, reduces the consumption of primary minerals and carbon emissions, and is in line with the circular economy and dual carbon strategy.
[0036] (3) Simple and controllable process: It can be prepared by conventional low-speed stirring process, without the need for special equipment, and is compatible with existing coating production lines; the construction is compatible with multiple processes such as spraying, scraping and troweling, and the project is highly feasible.
[0037] (4) The system is stable and reliable: the inorganic components have good chemical compatibility, no risk of alkali return, no gas generation, no hydrophobic damage to aerogel, and long storage and service life. Detailed Implementation
[0038] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the invention.
[0039] The technical parameters of some materials involved in the following embodiments include:
[0040] Inorganic silica sol binder: alkaline silica sol, with a SiO2 content of 32%, a particle size of 15 nm, and a pH value of 9.5;
[0041] Hydrophobic modified silica aerogel: self-made, prepared according to the above method, with a particle size of 40~60 μm, a porosity of 92%, and a thermal conductivity of 0.020 W / (m·K);
[0042] Fly ash cenospheres: power plant sorting, particle size 40~80 μm, porosity 85%, thermal conductivity 0.040 W / (m·K);
[0043] Microsilica powder: a byproduct of ferrosilicon smelting, with a SiO2 content of 92% and an average particle size of 0.3 μm;
[0044] Calcination of waste diatomaceous earth: Calcination of waste diatomaceous earth at 550℃ for 3 hours yields 0.3% soluble salts;
[0045] Waste alumina slag: Alumina profile alumina slag, washed and ground, with a particle size of 15~25 μm and an Al(OH)3 content of 75%;
[0046] Recycled rock wool short fibers: waste building rock wool cut to a length of 1~2 mm;
[0047] All other additives are industrial-grade conventional products.
[0048] Example 1
[0049] Raw materials are formulated by weight percentage as follows: deionized water 16.5%, inorganic silica sol binder 24.0%, hydrophobically modified silica aerogel 15.0%, fly ash cenospheres 11.0%, waste alumina slag 6.0%, aluminum hydroxide flame retardant powder 4.0%, microsilica powder 3.0%, calcined waste diatomaceous earth 6.0%, talc powder 3.0%, rutile titanium dioxide 4.0%, recycled rock wool short fiber 1.0%, dispersing and wetting agent 1.8%, silane coupling agent 1.0%, defoamer 0.5%, propylene glycol 2.2%, and inorganic thickener 1.0%.
[0050] Preparation steps:
[0051] Add deionized water, dispersant and wetting agent, silane coupling agent, defoamer, and propylene glycol to a mixing tank and stir at 200 r / min for 3 min to mix evenly; add microsilica powder, calcined waste diatomaceous earth, waste alumina slag, aluminum hydroxide flame retardant powder, talc powder, and titanium dioxide, and stir at 400 r / min for 12 min to obtain a uniform slurry.
[0052] Reduce the speed to 200 r / min, add fly ash cenospheres and rock wool short fibers, and stir for 6 min.
[0053] Slowly add the hydrophobically modified silica aerogel and stir at 200 r / min for 10 min.
[0054] Add inorganic silica sol binder and stir for 7 minutes to mix thoroughly; add inorganic thickener to adjust the viscosity to 100 seconds for a Forte 4 cup, then filter and discharge.
[0055] Example 2
[0056] The raw materials were prepared according to the following percentages by weight: deionized water 17.0%, inorganic silica sol binder 23.5%, hydrophobically modified silica aerogel 14.5%, fly ash cenospheres 12.0%, waste alumina slag 5.5%, aluminum hydroxide flame retardant powder 4.5%, microsilica powder 3.5%, calcined waste diatomaceous earth 5.5%, talc powder 2.5%, rutile titanium dioxide 3.8%, recycled rock wool short fiber 0.9%, dispersing and wetting agent 1.9%, silane coupling agent 0.9%, defoamer 0.5%, propylene glycol 2.3%, and inorganic thickener 1.2%. The preparation method was the same as in Example 1.
[0057] Example 3
[0058] The raw materials were prepared according to the following percentages by weight: deionized water 17.5%, inorganic silica sol binder 23.0%, hydrophobically modified silica aerogel 14.5%, fly ash cenospheres 9.0%, waste alumina slag 6.5%, aluminum hydroxide flame retardant powder 4.5%, microsilica powder 3.5%, calcined waste diatomaceous earth 6.5%, talc powder 3.2%, rutile titanium dioxide 3.9%, recycled rock wool short fiber 1.5%, dispersing and wetting agent 1.7%, silane coupling agent 1.1%, defoamer 0.5%, propylene glycol 2.1%, and inorganic thickener 1.0%. The preparation method was the same as in Example 1.
[0059] Comparative Example 1
[0060] This comparative example uses an all-virgin filler formulation with no solid waste substitutes. Specifically, it includes: 16.0% deionized water, 24.0% inorganic silica sol binder, 15.0% hydrophobically modified silica aerogel, 10.0% hollow ceramic microspheres, 10.0% aluminum hydroxide flame retardant powder, 7.0% talc, 7.0% diatomaceous earth, 4.0% rutile titanium dioxide, 0.3% glass fiber powder, 1.8% dispersant and wetting agent, 0.9% silane coupling agent, 0.5% defoamer, 2.3% propylene glycol, and 1.2% inorganic thickener. The preparation method is the same as in Example 1.
[0061] Comparative Example 2
[0062] This comparative example uses fly ash cenospheres as the sole additive, with no other solid waste. Specifically, it comprises: 16.2% deionized water, 24.0% inorganic silica sol binder, 15.0% hydrophobically modified silica aerogel, 10.0% fly ash cenospheres, 10.0% aluminum hydroxide flame retardant powder, 7.0% talc, 7.0% diatomaceous earth, 4.0% rutile titanium dioxide, 0.3% glass fiber powder, 1.8% dispersing and wetting agent, 0.9% silane coupling agent, 0.5% defoamer, 2.3% propylene glycol, and 1.0% inorganic thickener. The preparation method is the same as in Example 1.
[0063] Comparative Example 3
[0064] This comparative example differs from Example 1 in that it does not contain recycled rock wool short fibers. The remaining components are the same as in Example 1, except that the recycled rock wool short fibers are removed, and the amount of talc powder is increased accordingly to make up for the deficiency. The preparation method is the same as in Example 1.
[0065] Comparative Example 4
[0066] The difference between this comparative example and Example 1 is that it uses an unmodified hydrophilic aerogel; the other components are the same as in Example 1. The preparation method is the same as in Example 1.
[0067] Comparative Example 5
[0068] The difference between this comparative example and Example 1 is that a high-speed shearing process was used in the preparation process. The raw materials were the same as in Example 1. After the aerogel was added, the mixture was stirred at 800 r / min for 15 min.
[0069] Performance tests were conducted in accordance with JGJ / T 253-2019 "Technical Standard for Inorganic Lightweight Aggregate Mortar Insulation System", GB / T25261-2010 "Reflective Thermal Insulation Coatings for Buildings", and GB 8624-2012 "Classification of Combustion Performance of Building Materials and Products". The results are shown in the table below:
[0070] Test Project unit Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 dry film thermal conductivity W / (m·K) 0.024 0.023 0.025 0.028 0.026 0.025 0.038 0.031 Tensile bond strength (standard condition) MPa 0.62 0.58 0.65 0.48 0.51 0.49 0.45 0.55 Drying shrinkage rate % 0.22 0.24 0.20 0.32 0.29 0.30 0.35 0.26 Combustion performance rating - Grade A Grade A Grade A Grade A Grade A Grade A Grade A Grade A Water resistance (96h) - No bubbling, no peeling No bubbling, no peeling No bubbling, no peeling Slight bubbling Slight bubbling Slight bubbling Severe blistering and peeling No foaming Impact resistance Second-rate No cracks after 10 tests 9 times without cracks No cracks after 12 tests Cracks appeared 5 times Cracks appeared 6 times Cracks appeared 4 times Cracks appeared 3 times Cracks appeared 7 times
[0071] Comparison of Examples 1-3 with Comparative Example 1: The thermal conductivity, bonding strength, drying shrinkage rate and impact resistance of the multi-solid waste synergistic formulation of the present invention are significantly better than those of the all-virgin filler formulation, proving that solid waste substitution not only does not reduce performance, but also achieves performance upgrade through synergistic effect.
[0072] Comparison of Comparative Example 2 and Comparative Example 1: The addition of fly ash cenospheres can only slightly reduce the thermal conductivity, and the improvement in strength and crack resistance is limited, which verifies the necessity of multi-solid waste synergy.
[0073] Comparison Example 3 with Example 1: The crack resistance decreased significantly after the rock wool fiber was removed, proving the key role of the three-dimensional fiber skeleton in improving impact resistance and reducing shrinkage.
[0074] Comparison of Example 4 and Example 1: After absorbing water, the unmodified aerogel collapsed, the thermal conductivity increased significantly, and the water resistance decreased severely, which verified the necessity of hydrophobic modification.
[0075] Comparison of Example 5 and Example 1: High-speed shearing destroys the aerogel structure, leading to a decrease in thermal insulation performance, which verifies the importance of low-speed stirring process.
[0076] In summary, this invention uses inorganic silica sol as the bonding substrate and introduces five major industrial solid wastes: fly ash cenospheres, microsilica powder, recycled rock wool short fibers, calcined waste diatomaceous earth, and waste alumina slag. These materials synergistically replace virgin hollow ceramic microspheres, extender fillers, flame-retardant fillers, and reinforcing fibers. Combined with hydrophobically modified silica aerogel as the core thermal insulation component, an inorganic Class A non-combustible gel thermal insulation coating is prepared through a low-speed dispersion process.
[0077] This invention simultaneously improves the thermal insulation performance, bonding strength, crack resistance, and water resistance of coatings through the synergistic effect of multi-level pores (nanopores, micropores, and mesopores), the enhancement of silicon-oxygen network interfaces, and the multiple effects of a three-dimensional fiber crack-resistant skeleton. The combustion performance reaches GB8624 Class A. At the same time, it realizes the high-value utilization of various types of industrial solid waste, reduces raw material costs and carbon emissions, and has a simple process that is compatible with both spraying and scraping applications. It can be widely used in thermal insulation projects for building interior and exterior walls, roofs, cold storage, etc.
[0078] Although the present invention has been described in detail above with general descriptions and specific embodiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.
Claims
1. A green and environmentally friendly aerogel thermal insulation coating, characterized in that: By mass percentage, the raw material composition is as follows: deionized water 15.0%~18.0%, inorganic silica sol binder 23.0%~25.0%, hydrophobically modified silica aerogel 14.0%~15.0%, fly ash cenospheres 9.0%~12.0%, waste alumina slag 5.0%~7.0%, aluminum hydroxide flame retardant powder 3.0%~5.0%, microsilica powder 2.0%~4.0%, calcined waste diatomaceous earth 5.0%~7.0%, talc powder 2.0%~4.0%, rutile titanium dioxide 3.5%~4.5%, recycled rock wool short fiber 0.8%~1.5%, dispersing and wetting agent 1.6%~2.0%, silane coupling agent 0.8%~1.2%, defoamer 0.4%~0.6%, propylene glycol 2.0%~2.5%, and inorganic thickener 1.0%~1.5%, with the total of all components being 100%.
2. The green and environmentally friendly aerogel thermal insulation coating according to claim 1, characterized in that: The fly ash cenospheres are closed-cell hollow spherical particles obtained from the fly ash sorting of thermal power plants, and their composition is aluminosilicate. The microsilica powder is ultrafine dust collected from ferrosilicon / industrial silicon smelting; The calcined waste diatomaceous earth is obtained by calcining and removing impurities from waste diatomaceous earth filter aids in the food / chemical industry. The waste alumina slag is obtained by washing, purifying and ultra-fine grinding the waste slag of aluminum profile anodizing. Its components include aluminum hydroxide and activated alumina. The recycled rock wool short fibers are obtained from waste construction / industrial rock wool through opening, impurity removal, and shearing.
3. The green and environmentally friendly aerogel thermal insulation coating according to claim 1, characterized in that: The fly ash cenospheres have a particle size of 30~100 μm, a porosity of ≥80%, and a thermal conductivity of 0.035~0.045 W / (m·K). The microsilica powder contains ≥85% amorphous SiO2 and has an average particle size of 0.1~0.5 μm; The calcination temperature of the calcined waste diatomaceous earth is 500~600℃, and the soluble salt content is ≤0.5%, and the porosity is ≥80%. The particle size of the waste alumina slag is 10~30 μm; The recycled rock wool short fibers have a fiber length of 1~3 mm and a thermal conductivity of 0.038~0.045 W / (m·K).
4. The green and environmentally friendly aerogel thermal insulation coating according to claim 1, characterized in that: The preparation method of the hydrophobically modified silica aerogel includes the following steps: Step S1: Using hexamethyldisilazane or methyltrimethoxysilane as the modifier and anhydrous ethanol as the dispersion solvent, prepare a silane modification solution with a mass concentration of 5% to 10%, and the mass ratio of the modification solution to the aerogel powder is 3:1 to 5:
1. Step S2: Add the virgin silica aerogel powder into the modification solution and impregnate it at low speed under normal temperature and pressure for 6-12 hours, or react it in a water bath at 50-60℃ for 3-6 hours with a stirring speed of 80-120 r / min. Step S3: After impregnation, filter and separate the aerogel, rinse 2-3 times with anhydrous ethanol, and age in an environment of 40-50℃ for 8-12 hours; Step S4: Transfer to a vacuum drying oven at 60℃ and dry for 6~10 h to obtain hydrophobic modified silica aerogel, and store in a sealed container; the virgin silica aerogel has a porosity of 85%~95%, a particle size of 20~80 μm, and a thermal conductivity of 0.018~0.024 W / (m·K).
5. The green and environmentally friendly aerogel thermal insulation coating according to claim 1, characterized in that: The inorganic silica sol binder is an alkaline silica sol with a SiO2 content of 30%~35%, a particle size of 10~20 nm, and a pH value of 9.0~10.
0.
6. The green and environmentally friendly aerogel thermal insulation coating according to claim 1, characterized in that: The dispersing and wetting agent is a sodium polyacrylate dispersant. The silane coupling agent is KH550 or KH560; The defoamer is an organosilicon defoamer; The inorganic thickener is lithium-based bentonite or attapulgite.
7. A method for preparing a green and environmentally friendly aerogel thermal insulation coating as described in any one of claims 1-6, characterized in that: Includes the following steps: Step S1: Premixing and Dispersion: Add deionized water, dispersing and wetting agent, silane coupling agent, defoamer, and propylene glycol to a mixing tank and stir at low speed until homogeneous; then add microsilica powder, calcined waste diatomaceous earth, waste alumina slag, aluminum hydroxide flame retardant powder, talc powder, and rutile titanium dioxide in sequence, and stir at 300~500 r / min for 10~15 min until there are no obvious agglomerated particles; Step S2: Lightweight filler mixing: Reduce the stirring speed to 150~250 r / min, add fly ash cenospheres and recycled rock wool short fibers in sequence, and stir at low speed for 5~8 min to avoid cenosphere breakage and fiber entanglement; Step S3: Aerogel mixing: While maintaining a low stirring speed, slowly add the hydrophobic modified silica aerogel and continue stirring for 8~12 min to ensure that the aerogel is uniformly dispersed and structurally intact. Step S4: Film formation and viscosity adjustment: Add inorganic silica sol binder and stir for 5-10 minutes to mix evenly; finally, add inorganic thickener to adjust the viscosity of the system to 80-120 s (Ford Cup 4), stir evenly, filter and discharge to obtain the finished coating.
8. The preparation method according to claim 6, characterized in that: The maximum speed of the stirring is no more than 600 r / min.