An elastic self-healing cement grout, its preparation method and application
By compounding components such as hollow glass microspheres, microsilica, silane-modified rubber powder, and silane-modified carbon fiber, an elastic self-healing cement slurry was prepared, which solved the problems of elasticity and sealing of cement slurry in supercritical carbon dioxide geothermal wells and achieved long-term sealing integrity under high temperature and high pressure environment.
Patent Information
- Application Number
- CN202611602357.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cement slurry has insufficient elasticity, poor sealing and plugging capabilities in supercritical carbon dioxide geothermal wells, and cannot meet the long-term sealing integrity requirements under high temperature and high pressure environments.
The cement grout is made by compounding components such as hollow glass microspheres, microsilica, silane-modified rubber powder, silane-modified carbon fiber, water loss reducing agent, drag reducing agent and defoamer, etc., to form an elastic self-healing cement grout. Through synergistic effect, the elasticity, sealing and plugging ability of the cement grout are improved.
It achieves low density, low permeability, and crack resistance of cement stone under high temperature and high pressure environment, which can buffer the expansion and contraction of the casing, reduce interface debonding and micro-annular gaps, and improve the sealing ability and plugging effect of the annulus.
Smart Images

Figure CN123106094A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of geothermal well cementing materials, annular sealing and wellbore integrity control, specifically relating to an elastic self-healing cement slurry and its preparation method and application. Background Technology
[0002] Supercritical carbon dioxide coaxial closed-loop geothermal wells utilize the casing and coaxial inner tube to form a closed circulation channel, absorbing formation heat through the circulation of carbon dioxide working fluid within the wellbore. These wells endure high pressure and repeated heating, cooling, and start-stop cycles during operation. Differences in thermal expansion coefficients and elastic deformation exist between the casing, cement stone, and formation. If the cement stone cracks or micro-annular gaps form at the casing-cement stone interface, carbon dioxide may leak along the annulus. Therefore, the cement stone used for cementing must not only meet early-stage construction performance requirements but also possess long-term elasticity, interface sealing, and fracture plugging capabilities.
[0003] Conventional G-grade oil well cement stone has high rigidity. When wellbore temperature and pressure change, the radial expansion and contraction of the casing can easily generate tensile and shear stresses in the cement stone, potentially leading to brittle fractures, interfacial debonding, and annular air channeling. Supercritical carbon dioxide, upon contact with residual moisture in the well, can also form an acidic medium, continuously affecting the pore structure of the cement stone and the outer wall of the casing. This means that even wellbores with initially acceptable cementing quality may still face the risk of decreased sealing integrity after long-term operation.
[0004] Existing low-density cement slurry, latex cement slurry, anti-gas-channeling cement slurry, and fiber-reinforced cement slurry are typically designed to address a single issue, such as reducing leakage, minimizing water loss, inhibiting gas intrusion, or improving toughness. Adding only lightweight materials may reduce the compressive strength of the cement paste; adding only elastic materials may affect thickening time, rheology, and early strength.
[0005] In summary, existing cement slurries cannot meet the requirements of supercritical carbon dioxide geothermal wells due to insufficient elasticity, poor sealing and plugging capabilities. Summary of the Invention
[0006] To address the technical problems of insufficient elasticity, poor sealing and plugging capabilities of existing cement slurries, this invention provides an elastic self-healing cement slurry, its preparation method, and its applications. The elastic self-healing cement slurry provided by this invention possesses excellent elastic properties, sealing capabilities, and plugging capabilities, meeting the application requirements in supercritical carbon dioxide coaxial closed-loop geothermal wells.
[0007] To achieve the above objectives, the present invention employs the following technical solution: An elastic self-healing cement grout, comprising Grade G oil well cement, additives, and water for grout preparation.
[0008] Based on the weight of Grade G oil well cement, the percentage of each component in the auxiliary materials is as follows: hollow glass microspheres 10%–20%, microsilica 8%–12%, water loss reducer 0.67%–1.33%, drag reducer 0.3%–0.67%, anti-gas channeling agent 3%–7%, defoamer 0.05%–0.2%, silane-modified rubber powder 1%–4%, latex 10%–18%, and silane-modified carbon fiber 0.2%–0.8%.
[0009] In a preferred embodiment of the present invention, the percentage of each component in the auxiliary materials by weight of G-grade oil well cement is as follows: 12%–18% hollow glass microspheres, 10%–12% microsilica, 1%–1.17% water loss reducer, 0.5%–0.67% drag reducer, 5%–6% anti-gas channeling agent, 0.1%–0.15% defoamer, 1.5%–3% silane-modified rubber powder, 12%–16% latex, and 0.3%–0.6% silane-modified carbon fiber.
[0010] In a preferred embodiment of the present invention, the hollow glass microspheres are sodium-calcium borosilicate hollow glass beads, and the D of the hollow glass microspheres is... 10 The size ranges from 15μm to 25μm.
[0011] In a preferred embodiment of the present invention, the D of G-grade oil well cement 50 The diameter of primary particles in microsilicon ranges from 15μm to 25μm; the average diameter of primary particles in microsilicon ranges from 0.15μm to 0.20μm.
[0012] In a preferred embodiment of the present invention, the silane-modified rubber powder is obtained by vulcanizing rubber powder and then modifying it with a methacryloyloxy silane coupling agent.
[0013] In a preferred embodiment of the present invention, the methacryloyloxy silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane, and the D of the rubber powder is... 50 The size ranges from 90μm to 120μm.
[0014] In a preferred embodiment of the present invention, silane-modified carbon fiber is obtained by oxidizing carbon fiber and then impregnating it with an amino-based silane coupling agent as a modifier.
[0015] In a preferred embodiment of the present invention, the amino-based silane coupling agent is γ-aminopropyltriethoxysilane, and the length of the carbon fiber is 2.5 mm to 3.5 mm.
[0016] If the various additives lack particle size compatibility and synergistic design, problems such as sedimentation, agglomeration, increased pumping resistance, or unstable high-temperature performance can easily occur. The D grade G oil well cement used in this invention... 50 The D of hollow glass microspheres is controlled within the range of 15μm to 25μm.10 The main particle skeleton consists of G-grade oil well cement and hollow glass microspheres, with a particle size of 15μm to 25μm. The primary particles of microsilica have an average diameter of 0.15μm to 0.20μm, and secondary aggregates D are formed after wet dispersion. 90 No larger than 10μm, used to fill the secondary pores between G-grade oil well cement particles and hollow glass microspheres; D of silane-modified rubber powder 50 The particles are controlled to be 90μm–120μm in size, serving as dispersed, flexible third-scale particles to avoid competition between a large amount of fine rubber powder and microsilica for adsorbing admixtures. Silane-modified carbon fibers with a length of 2.5mm–3.5mm and a diameter of 7μm achieve cross-scale bridging. This results in a composite structure that combines a three-dimensional particle size framework of microsilica, G-grade oil well cement / hollow glass microspheres, and silane-modified rubber powder with silane-modified carbon fiber bridging, taking into account suspension stability, pumpability, low permeability, and crack resistance.
[0017] This invention also provides a method for preparing the above-mentioned elastic self-healing cement grout, comprising the following steps: Weigh each component according to the mass fraction; disperse the water loss reducing agent in the external water to obtain an aqueous solution of the water loss reducing agent, and disperse the drag reducing agent in the external water to obtain an aqueous solution of the drag reducing agent; it should be noted that the external water refers to water that is measured separately from the water used for slurry preparation.
[0018] Divide the water used for slurry preparation into two portions; disperse the microsilica in one portion of the water and disperse evenly to obtain the microsilica slurry.
[0019] G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber are mixed in the first stage to obtain a solid premix.
[0020] The other portion of the slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer are mixed a second time to form a liquid phase material.
[0021] The solid premix and liquid material are first stirred at 3800 r / min to 4200 r / min. After the first stirring is completed, the speed is increased to 11500 r / min to 12500 r / min for the second stirring. After the second stirring is completed, the speed is reduced to 550 r / min to 650 r / min, hollow glass microspheres are added, and a third stirring is carried out to obtain elastic self-healing cement slurry.
[0022] In this invention, the elastic self-healing cement slurry is prepared in the following order: solid phase pre-dispersion, liquid phase material homogenization, high-shear compounding, and low-shear addition of hollow glass microspheres. The preparation method of this invention helps to reduce the agglomeration of silane-modified carbon fiber and silane-modified rubber powder, and reduces the risk of hollow glass microspheres breaking under high shear, thereby taking into account the uniformity of slurry dispersion, density stability and pumpability.
[0023] It should be noted that when adding water, this invention determines the amount of water to be added based on the target slurry density and pumpability of the elastic self-healing cement slurry. Using G-grade oil well cement, hollow glass microspheres, microsilica, silane-modified rubber powder, and silane-modified carbon fiber as the solid phase, aqueous solutions of water loss reducing agent, drag reducing agent, and anti-gas channeling agent as the solutions, and latex as the emulsion, the amount of water to be added is calculated based on volume balance. The calculation formula is as follows: ; In the formula, m w For the quality of water used in slurry preparation, m i and ρ i These represent the mass and measured density of the i-th raw material, excluding the water used for pulp preparation, ρ. d ρ is the target slurry density. w Let m be the density of water. p To reduce the water content in aqueous solutions of dehydrating agents, drag-reducing agents, anti-gas channeling agents, and latex.
[0024] After calculating using the above formula, the slurry density, rheological properties, free liquid content, and density difference between the upper / middle / lower parts were verified through pre-mixing tests. The water content for slurry preparation in Examples 1 to 5 was 44 parts by mass; the measured density of the cement slurry obtained in Examples 1 to 3 was 1.42 ± 0.02 g / cm³, respectively. 3 1.49±0.02g / cm 3 and 1.36±0.02g / cm 3 The theoretical slurry densities calculated based on the nominal density of the raw materials in Examples 4 and 5 are approximately 1.49 g / cm³. 3 and 1.35g / cm 3 The actual value shall be based on the results of the pre-mixing test.
[0025] It should be noted that the water used for wet pre-dispersion of microsilica in each embodiment was measured from the 44 parts by mass of slurry-mixing water specified in that embodiment, and the remaining slurry-mixing water was added when preparing the liquid phase material; the pre-mixing water for the water loss reducing agent aqueous solution and the drag reducing agent aqueous solution was measured separately. Density and rheology were continuously monitored during the mixing process, and the slurry-mixing water was measured once according to the amount specified in the formula, and no temporary adjustments were allowed without recording; the maximum density difference between the upper / middle / lower parts of the resulting slurry was not greater than 0.03 g / cm³. 3 The free liquid content is 0, and the volume fraction of entrained air is no more than 1.0%.
[0026] This invention also provides an application of elastic self-healing cement slurry in supercritical carbon dioxide geothermal wells. The application method is as follows: pre-fluid, elastic self-healing cement slurry and displacement fluid are sequentially pumped into the annulus channel of a coaxial double-tube well. The displacement fluid is used to press the pre-fluid and elastic self-healing cement slurry into the annulus area between the outer wall of the coaxial double-tube well and the formation. The elastic self-healing cement slurry returns to the desired position along the annulus area. After solidification, it forms elastic self-healing cement stone.
[0027] The coaxial double column includes a casing and an inner tube. The inner tube is coaxially sleeved inside the casing, and an annular channel is formed between the outer wall of the inner tube and the inner wall of the casing. A vortex stabilizer is located on the outer wall of the casing to keep the coaxial double column in the center position.
[0028] Compared with the prior art, the present invention has the following beneficial effects: This invention utilizes hollow glass microspheres to reduce the density of elastic self-healing cement slurry and alleviate annular fluid column pressure in easily leaky formations. After the elastic self-healing cement slurry solidifies to form elastic self-healing cement stone, microsilica fills the capillary pores of the cement stone, and silane-modified carbon fibers form a dispersed bridging skeleton within the elastic self-healing cement stone, resulting in a synergistic effect of lightweighting, densification, and enhanced crack resistance. Silane-modified rubber powder and latex form a flexible phase within the elastic self-healing cement stone, reducing its brittleness and improving its radial deformation adaptability. This allows the elastic self-healing cement stone to buffer the expansion and contraction of the casing during injection, heat extraction, and well shutdown, reducing interfacial debonding and microannular formation. A fluid loss reducer, an anti-gas channeling agent, and latex work together to control cement slurry fluid loss, static gel strength transition, and early gas intrusion, reducing the risk of annular gas channeling during the setting stage and improving the low-permeability sealing capability of the elastic self-healing cement stone after solidification. In addition, through the continuous reaction and filling of crack channels by microsilica and incompletely hydrated micro-gel particles, combined with the elastic bonding of silane-modified rubber powder and latex to the crack surface and the bridging and crack-limiting effect of silane-modified carbon fiber, a self-healing mechanism is formed, which includes filling of reaction products, bonding of flexible phases and inhibition of secondary opening of fibers. This seals the micro-cracks formed by temperature and pressure cycling and restores the local sealing ability.
[0029] This invention combines elastic self-healing cement slurry with casing straightening and vortex displacement, which keeps the casing centered in the wellbore and improves the fluid replacement efficiency in the narrow annulus, reducing residual drilling fluid, mud cake and non-cemented areas, forming a continuous elastic self-healing cement stone with a relatively uniform thickness.
[0030] This invention also specifies the steps for formula design, mixing sequence, pumping displacement, curing during the curing period, and evaluation of the integrity of temperature and pressure cycles, so that the material properties can be matched with the on-site construction process. It can be used for supercritical carbon dioxide coaxial closed geothermal wells and wellbore annulus seals with similar high temperature and high pressure circulation conditions. Attached Figure Description
[0031] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0032] Figure 1 This is a schematic diagram of the overall layout of elastic self-healing cement stone in a supercritical carbon dioxide geothermal well.
[0033] Figure 2 This is a flowchart of the preparation of elastic self-healing cement slurry and cementing method.
[0034] Figure 3 This is a schematic diagram of the elastic buffering and crack sealing mechanism at the casing-elastic self-healing cement stone-formation interface, where (a) represents the initial cementation state and (b) represents the synergistic sealing state after temperature and pressure cycling.
[0035] Figure 4 The diagram shows the annular displacement structure of cement slurry under vortex normalization conditions, where (a) is a cross-sectional view and (b) is a cross-sectional view.
[0036] Reference numerals: 1-Corrosion-resistant sealing wellhead, 2-Casing, 3-Inner tube, 4-Elastic self-healing cement stone, 5-Formation, 6-Swirl stabilizer, 7-Airtight threaded connection component, 8-Sealed bottomhole assembly. Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0038] Supercritical carbon dioxide coaxial closed-loop geothermal wells use supercritical CO2 as the circulating working fluid to achieve closed-loop heat exchange that extracts heat without extracting water. The system can reach pressures of up to 35 MPa, with frequent temperature and pressure fluctuations during operation. Simultaneously, CO2 can form an acidic medium under aqueous conditions, causing carbonization corrosion of the cement slurry. Therefore, the cement slurry used in this type of well must not only possess excellent resistance to CO2 corrosion but also good elasticity, toughness, and interfacial bonding strength to resist micro-annular gaps and micro-cracks induced by thermal cycling. This ensures that the well maintains its sealing integrity for a long period under high temperature, high pressure, and alternating stress, thereby guaranteeing the safe circulation of the CO2 working fluid and the efficient development of geothermal resources.
[0039] In existing technologies, researchers have employed various methods to address supercritical carbon dioxide environments. These include using hollow components to contain carbonization products within cement compositions to achieve CO2 corrosion resistance; employing self-healing latex cement slurry systems that utilize active mineral surface coatings to achieve self-repair after cement stone damage; using low-density anti-channeling cement slurry systems composed of hollow glass microspheres, microsilica, and styrene-butadiene latex to achieve both low density and anti-channeling properties; and treating hollow glass microspheres with surface glazing technology and combining them with silica powder and styrene-butadiene rubber powder to form a high-temperature, low-density cement slurry system to improve the stability of hollow glass microspheres in high-temperature alkaline environments. However, these existing methods focus on single or partial performance dimensions such as CO2 resistance sealing, self-healing, low-density anti-channeling, or high-temperature stability, failing to simultaneously meet the comprehensive performance requirements of low density, elasticity and toughness, self-healing, and CO2 resistance sealing.
[0040] Based on this, the present invention combines hollow glass microspheres, microsilica, silane-modified rubber powder, latex, silane-modified carbon fiber, water loss reducing agent, drag reducing agent, anti-gas channeling agent and defoamer, and the synergistic effects between the components are as follows: 1. Synergistic effect of lightweight, dense and crack-resistant: This invention uses hollow glass microspheres as raw material to reduce the density of cement slurry. Microsilica fills the pores between the glass microspheres and cement particles and strengthens the interface transition zone between the elastic self-healing cement stone and the wellbore formation, and between the elastic self-healing cement stone and the casing. Silane-modified carbon fibers cross potential cracks and limit crack propagation. These three elements work together to offset the decrease in pressure-bearing capacity and sealing performance caused by using lightweight materials alone, enabling the cement slurry to simultaneously achieve low density, low permeability, and crack resistance. Omitting microsilica, silane-modified carbon fibers, or using conventional lightweight materials for equal-density replacement is problematic because omitting microsilica would make it difficult to fully fill the secondary pores between particles, leading to a decrease in the density and impermeability of the elastic self-healing cement stone; omitting silane-modified carbon fibers would result in a lack of cross-crack bridging and propagation constraints for cracks; and using conventional lightweight materials with different densities, strengths, and particle size distributions for equal-density replacement would alter the particle gradation and load-bearing skeleton, making it difficult to simultaneously achieve low density, pressure-bearing capacity, impermeability, and crack resistance, thus failing to form the aforementioned complete synergistic structure.
[0041] 2. Flexible-bridging collaboration: Silane-modified rubber powder, acting as dispersed flexible particles, reduces localized stress concentration. Latex forms a continuous or semi-continuous flexible phase at the interface between the elastic self-healing cement paste and the casing. Silane-modified carbon fiber provides bridging constraints across the joint. The combination of silane-modified rubber powder, latex, and silane-modified carbon fiber enables the elastic self-healing cement paste to possess low elastic modulus, high ultimate strain, stable interfacial bonding, and low leakage characteristics after thermo-pressure cycling; all three are indispensable. The absence of any one component prevents the simultaneous achievement of these effects.
[0042] 3. Synergistic effect of water loss prevention, gas leakage prevention, and interface sealing: The water loss reducer decreases filtrate precipitation, the gas channeling inhibitor shortens the transition time to static gelation and inhibits gas intrusion, and the latex also improves early film formation and low permeability after curing. These three components block gas channeling during the waiting period and maintain a low-permeability interface seal after curing, thereby simultaneously reducing water loss, shortening the static gelation strength transition time, and inhibiting high-pressure carbon dioxide migration along the annulus.
[0043] 4. Crack Self-Healing and Sealing Restoration: After microcracks are formed by temperature and pressure cycling, incompletely hydrated cementitious particles continue to react. Incompletely hydrated cement particles continue to hydrate with water to form hydration products. Microsilica reacts with calcium hydroxide released from cement hydration to form pozzolanic reaction products. These hydration products and pozzolanic reaction products deposit and fill the crack channels. Silane-modified rubber powder and latex maintain the elastic adhesion of the crack surface, while silane-modified carbon fibers limit further crack opening. These combined effects narrow the crack channels, reduce permeability and leakage, and restore sealing capacity, forming the elastic self-healing mechanism of this invention.
[0044] The G-grade oil well cement used in this invention is HSR G-grade oil well cement produced by Shandong Chongzheng Special Cement Co., Ltd., which conforms to GB / T 10238-2015 and API Spec 10A; its typical specific gravity is 3.15, and the laser particle size is controlled to D during use. 10 =3μm~8μm, D 50 =15μm~25μm, D 90 ≤70μm.
[0045] The hollow glass microspheres are high-strength hollow glass microspheres, specifically HL46 type sodium-calcium borosilicate hollow glass microspheres from Zhengzhou Shenglete Hollow Microsphere New Material Co., Ltd., with a true density of 0.44 g / cm³. 3 ~0.48g / cm 3 The compressive strength is 6000 psi, approximately 41.4 MPa. 50 Typical values are 40 μm and D 90 ≤70μm, moisture content ≤0.3%; D when using 10 The microspheres were controlled to be between 15μm and 25μm. Unless otherwise specified, the hollow glass microspheres used in the following examples and comparative examples were all from this manufacturer.
[0046] The microsilicon used is 940U type dry amorphous microsilicon powder from Shanghai Tiankai Building Materials Technology Co., Ltd., with a typical SiO2 content of 94.8%, an average primary particle diameter of 0.15μm to 0.20μm, and a BET specific surface area of approximately 19m². 2 / g, 45μm sieve residue ≤3.0%, moisture content ≤0.5%, secondary agglomerates D after wet dispersion before slurry preparation 90 ≤10μm.
[0047] The fluid loss reducing agent used is the BS108 type AMPS multi-component copolymer high-temperature fluid loss reducing agent from Sichuan Hongsheng Petroleum Engineering Technology Service Co., Ltd., with a 0.315mm sieve residue of ≤12%. It is suitable for downhole environments with a bottom-hole circulation temperature of 110℃~200℃, and the fluid loss of high-temperature cement slurry is ≤50mL. In this invention, the fluid loss reducing agent is used as a 33.3% (w / w) aqueous solution. When the mass of the fluid loss reducing agent, i.e., the AMPS multi-component copolymer, is 1 part, the amount of the aqueous solution added is 3 parts.
[0048] The drag-reducing agent used is the USZ type ketone-aldehyde condensate oil well cement drag-reducing agent from Weihui Chemical Co., Ltd., with a 0.315mm sieve residue <15%, initial consistency ≤15Bc, and rheological index n≥0.55 and consistency coefficient K≤0.50 Pa·s at 52℃. n Before use, a compatibility test is conducted under the target operating condition of 180℃. This invention uses a drag-reducing agent in an aqueous solution with a mass concentration of 33.3%.
[0049] The anti-gas channeling agent uses branched polyethyleneimine aqueous solution P434396 from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No. 9002-98-6, with a number average molecular weight Mn of approximately 60,000, a weight average molecular weight Mw of approximately 750,000, and a solid content of 50%±2%. Its cationic polymer is adsorbed onto cement particles and early hydration structures, reducing the connectivity channels in the critical gelation stage.
[0050] The defoamer used is XP-1 type polyether oil well cement defoamer from Weihui Chemical Co., Ltd. Using this defoamer, the cement slurry density recovery rate is ≥90%.
[0051] This invention uses silane-modified rubber powder to improve its wetting and dispersion in cement slurry. The silane coupling agent used in this invention is γ-(methacryloyloxy)propyltrimethoxysilane, denoted as KH570. The preparation steps of the silane-modified rubber powder are as follows: Step 1: Based on 100 parts by weight of rubber powder, add 5 parts by weight of zinc oxide, 1 part by weight of stearic acid, 15 parts by weight of N550 carbon black and 2.5 parts by weight of dicumyl peroxide, and mix at 70℃ and 60r / min for 8 minutes to obtain the compound.
[0052] Step 2: Vulcanize the compound at 170℃ and 10MPa for 15 minutes to achieve a Shore A hardness of 90-95, thus obtaining vulcanized rubber.
[0053] The vulcanized rubber was cut into 5mm-10mm particles, frozen in liquid nitrogen at -80℃ for 20 minutes, then cryogenically pulverized and sieved to control D. 10 45μm~65μm, D50 90μm~120μm, D 90 Its diameter is 160μm to 200μm, and its true density is 1.10g / cm³. 3 ~1.20g / cm 3 The resulting vulcanized rubber powder is obtained.
[0054] Step 3: Prepare the mixture by mixing the vulcanized rubber powder, deionized water and KH-570 in a mass ratio of 1:2:0.005. After mixing the deionized water and KH570 evenly, adjust the pH to 4.5 with acetic acid and stir at 40°C for 40 minutes to obtain the silane coupling agent solution.
[0055] After adding vulcanized rubber powder to the silane coupling agent solution, the mixture was stirred at 500 r / min at 40°C for 60 min. The mixture was then filtered and washed with deionized water until the filtrate was neutral. Finally, the mixture was vacuum dried at 60°C for 12 h and then sealed for storage.
[0056] The rubber powder used in this invention is J-4045 type EPDM rubber from Jilin Petrochemical Company of China National Petroleum Corporation, with an ethylene content of 49% to 55%, Mooney viscosity ML(1+4) at 100°C of 40 to 50, tensile strength ≥15MPa, and elongation at break ≥320%.
[0057] The latex used is GR-L type styrene-butadiene latex for oil well cement from Weihui Chemical Co., Ltd., with a solid content controlled at 48%–50% and a pH of 7.0–9.0. In this invention, it is measured based on a solid content of 49% and the wet basis of the commercial emulsion. The latex used in this invention has a water loss of ≤100mL under the conditions of 80℃, 6.9MPa, and 30min, and a compressive strength of ≥14MPa under the conditions of 102℃, 21MPa, and 24h.
[0058] Compared to raw carbon fibers, the silane-modified carbon fibers used in this invention have increased polar groups on the carbon fiber surface through modification treatment, and improved the interfacial bonding between the carbon fibers and cement hydration products, as well as the slurry dispersion performance. The silane coupling agent used in this invention is γ-aminopropyltriethoxysilane, denoted as KH550. The preparation steps of the silane-modified carbon fibers are as follows: Step 1: Oxidize the carbon fiber in nitric acid at 60℃ and 8mol / L for 1 hour. Wash it with deionized water until the filtrate is neutral, and then dry it under vacuum at 100℃ for 2 hours to obtain oxidized carbon fiber.
[0059] Step 2: Mix anhydrous ethanol and deionized water at a volume ratio of 90:10 to obtain a mixed solution. Add KH-550 to the mixed solution to prepare a 3% (w / w) solution. Adjust the pH to 5.0 with acetic acid and stir at 25°C for 30 minutes to obtain the hydrolysate.
[0060] Step 3: Measure out the hydrolysate at a mass ratio of 10:1 to carbon dioxide, immerse the carbon dioxide in the hydrolysate, sonicate for 2 hours, and let it stand for 30 minutes. Filter and wash three times with anhydrous ethanol, then vacuum dry at 75°C for 12 hours to obtain KH-550 modified carbon fiber, i.e., silane modified carbon fiber, and seal for later use.
[0061] The carbon fiber used is SYT49S-12K type PAN-based carbon fiber from Zhongfu Shenying Carbon Fiber Co., Ltd., with a length of 3.0±0.5mm, a single filament diameter of 7μm, a tensile strength of 4900MPa, a tensile modulus of 230GPa, an elongation at break of 2.1%, and a density of 1.79g / cm³. 3 The linear density is 800 g / km.
[0062] The water used for preparing the slurry is laboratory deionized water, Na + and Cl The concentrations of each component should not exceed 10 mg / L, the pH should be 6.5–7.5, and the total dissolved solids should not exceed 100 mg / L.
[0063] It should be noted that the raw materials used in this invention are not limited to those from the aforementioned manufacturers. Those skilled in the art can select commercially available similar products based on performance indicators. In this invention, the "parts" in the examples and comparative examples refer to parts by mass, which is the mass of commercially available dosage forms and does not include solvents added during experimental preparation. For example, water loss reducers and drag reducers are calculated based on the effective dry matter content, while anti-gas channeling agents and latex are calculated based on the wet basis of commercially available specifications. For instance, the percentage of anti-gas channeling agent in the weight of G-grade oil well cement is 3% to 7%, which means that the P434396 type branched polyethyleneimine aqueous solution accounts for 3% to 7% of the weight of G-grade oil well cement. Those skilled in the art can convert the aforementioned parts by mass to kg, g, or ton, etc., according to the actual production scale. In the following examples and comparative examples, parts by mass refer to g.
[0064] In the following embodiments, the mass fraction of each component is measured based on 100 parts of Grade G oil well cement. When the amount of Grade G oil well cement is changed due to project requirements, the amount of each admixture is converted proportionally.
[0065] It should be noted that the water added to prepare the aqueous solutions of the water loss reducing agent and the drag reducing agent is external water, which is separately measured from the 44 parts by mass of the water used for slurry preparation mentioned above.
[0066] Example 1 This embodiment provides an elastic self-healing cement grout, which is composed of the following components in parts by weight: The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 44 parts by weight of water, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0067] This embodiment also provides a method for preparing elastic self-healing cement grout, which is prepared according to the following steps: Step 1, Raw material pretreatment: One part of the water loss reducing agent was dispersed in external water to prepare an aqueous solution of the water loss reducing agent with a mass concentration of 33.3%.
[0068] 0.5 parts of drag-reducing agent were dispersed in external water to prepare an aqueous solution of drag-reducing agent with a mass concentration of 33.3%.
[0069] 20 parts by weight of water were measured from the 44 parts by weight of water used for slurry preparation in this embodiment, and 10 parts by weight of microsilica were added to it. The mixture was dispersed using a high-speed disperser at 2000 r / min for 10 min to obtain secondary agglomerates D. 90 Microsilica slurry with a particle size not exceeding 10 μm and wet dispersion.
[0070] Step 2: Preparation of solid-phase premix and liquid-phase materials A horizontal ribbon mixer was used to dry mix G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber. The dry mixing speed was 60 r / min and the dry mixing time was 10 min. This ensured that the silane-modified carbon fiber was evenly dispersed without forming fiber clumps, thus obtaining a solid premix.
[0071] Add the remaining 24 parts by weight of slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer to the liquid phase tank, and circulate and stir at 1000 r / min for 5 min to form a uniform liquid phase material.
[0072] Step 3: Mix in sequence to form an elastic self-healing cement slurry. Under continuous stirring conditions at a speed of 4000 r / min, the solid premix was added to the liquid material and stirred for 15 s. Then the speed was increased to 12000 r / min and high shear was applied for 35 s. After the high shear was completed, the speed was reduced to 600 r / min and hollow glass microspheres were added in 3 batches. The time was started from the addition of the first batch of hollow glass microspheres. The total time for the 3 batches of material addition and low-speed stirring was 3 min, resulting in elastic self-healing cement slurry.
[0073] Example 2 The following ingredients were used: 100 parts by weight of Grade G oil well cement, 12 parts by weight of hollow glass microspheres, 12 parts by weight of microsilica, 1 part by weight of water loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 1.5 parts by weight of silane-modified rubber powder, 12 parts by weight of latex, 0.3 parts by weight of silane-modified carbon fiber, and 44 parts by weight of water for slurry preparation. The resulting cement slurry had a density of 1.49 ± 0.02 g / cm³. 3 .
[0074] This embodiment also provides a method for preparing elastic self-healing cement grout, which is prepared according to the following steps: Step 1, Raw material pretreatment: One part of the water loss reducing agent was dispersed in external water to prepare an aqueous solution of the water loss reducing agent with a mass concentration of 33.3%.
[0075] 0.5 parts of drag-reducing agent were dispersed in external water to prepare an aqueous solution of drag-reducing agent with a mass concentration of 33.3%.
[0076] 24 parts by weight of water were measured from the 44 parts by weight of water used for slurry preparation in this embodiment, and 12 parts by weight of microsilica were added to it. The mixture was dispersed using a high-speed disperser at 2000 r / min for 10 min to obtain secondary agglomerates D. 90 Microsilica slurry with a particle size not exceeding 10 μm and wet dispersion.
[0077] Step 2: Preparation of solid-phase premix and liquid-phase materials A horizontal ribbon mixer was used to dry mix G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber. The dry mixing speed was 60 r / min and the dry mixing time was 10 min. This ensured that the silane-modified carbon fiber was evenly dispersed without forming fiber clumps, thus obtaining a solid premix.
[0078] Add the remaining 20 parts by weight of slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer to the liquid phase tank, and circulate and stir at 1000 r / min for 5 min to form a uniform liquid phase material.
[0079] Step 3: Mix in sequence to form an elastic self-healing cement slurry. Under continuous stirring conditions at a speed of 4000 r / min, the solid premix was added to the liquid material and stirred for 15 s. Then the speed was increased to 12000 r / min and high shear was applied for 35 s. After the high shear was completed, the speed was reduced to 600 r / min and hollow glass microspheres were added in 3 batches. The time was started from the addition of the first batch of hollow glass microspheres. The total time for the 3 batches of material addition and low-speed stirring was 3 min, resulting in elastic self-healing cement slurry.
[0080] Example 3 The following ingredients were added: 100 parts by weight of Grade G oil well cement, 18 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1.17 parts by weight of water loss reducer, 0.67 parts by weight of drag reducer, 6 parts by weight of anti-gas channeling agent, 0.15 parts by weight of defoamer, 3 parts by weight of silane-modified rubber powder, 16 parts by weight of latex, 0.6 parts by weight of silane-modified carbon fiber, and 44 parts by weight of water for slurry preparation. The resulting cement slurry had a density of 1.36 ± 0.02 g / cm³. 3 .
[0081] This embodiment also provides a method for preparing elastic self-healing cement grout, which is prepared according to the following steps: Step 1, Raw material pretreatment: 1.17 parts of the water loss reducing agent were dispersed in external water to prepare an aqueous solution of the water loss reducing agent with a mass concentration of 33.3%.
[0082] 0.67 parts of drag-reducing agent were dispersed in external water to prepare an aqueous solution of drag-reducing agent with a mass concentration of 33.3%.
[0083] 20 parts by weight of water were measured from the 44 parts by weight of water used for slurry preparation in this embodiment, and 10 parts by weight of microsilica were added to it. The mixture was dispersed using a high-speed disperser at 2000 r / min for 10 min to obtain secondary agglomerates D. 90 Microsilica slurry with a particle size not exceeding 10 μm and wet dispersion.
[0084] Step 2: Preparation of solid-phase premix and liquid-phase materials A horizontal ribbon mixer was used to dry mix G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber. The dry mixing speed was 60 r / min and the dry mixing time was 10 min. This ensured that the silane-modified carbon fiber was evenly dispersed without forming fiber clumps, thus obtaining a solid premix.
[0085] Add the remaining 24 parts by weight of slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer to the liquid phase tank, and circulate and stir at 1000 r / min for 5 min to form a uniform liquid phase material.
[0086] Step 3: Mix in sequence to form an elastic self-healing cement slurry. Under continuous stirring conditions at a speed of 4000 r / min, the solid premix was added to the liquid material and stirred for 15 s. Then the speed was increased to 12000 r / min and high shear was applied for 35 s. After the high shear was completed, the speed was reduced to 600 r / min and hollow glass microspheres were added in 3 batches. The time was started from the addition of the first batch of hollow glass microspheres. The total time for the 3 batches of material addition and low-speed stirring was 3 min, resulting in elastic self-healing cement slurry.
[0087] Example 4 The mixture comprises 100 parts by weight of Grade G oil well cement, 10 parts by weight of hollow glass microspheres, 8 parts by weight of microsilica, 0.67 parts by weight of water loss reducer, 0.67 parts by weight of drag reducer, 3 parts by weight of anti-gas channeling agent, 0.05 parts by weight of defoamer, 1 part by weight of silane-modified rubber powder, 18 parts by weight of latex, 0.2 parts by weight of silane-modified carbon fiber, and 44 parts by weight of water for slurry preparation. The theoretical slurry density, calculated based on the nominal density of the raw materials, is approximately 1.49 g / cm³. 3 The actual value shall be based on the results of the pre-mixing test.
[0088] This embodiment also provides a method for preparing elastic self-healing cement grout, which is prepared according to the following steps: Step 1, Raw material pretreatment: 0.67 parts of the water loss reducing agent were dispersed in external water to prepare an aqueous solution of the water loss reducing agent with a mass concentration of 33.3%.
[0089] 0.67 parts of drag-reducing agent were dispersed in external water to prepare an aqueous solution of drag-reducing agent with a mass concentration of 33.3%.
[0090] 16 parts by weight of water were measured from the 44 parts by weight of water used for slurry preparation in this embodiment, and 8 parts by weight of microsilica were added to it. The mixture was dispersed using a high-speed disperser at 2000 r / min for 10 min to obtain secondary agglomerates D. 90 Microsilica slurry with a particle size not exceeding 10 μm and wet dispersion.
[0091] Step 2: Preparation of solid-phase premix and liquid-phase materials A horizontal ribbon mixer was used to dry mix G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber. The dry mixing speed was 65 r / min and the dry mixing time was 10 min. This ensured that the silane-modified carbon fiber was evenly dispersed without forming fiber clumps, thus obtaining a solid premix.
[0092] Add the remaining 28 parts by weight of slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer to the liquid phase tank, and circulate and stir at 1050 r / min for 5 min to form a uniform liquid phase material.
[0093] Step 3: Mix in sequence to form an elastic self-healing cement slurry. Under continuous stirring conditions at a speed of 4200 r / min, the solid premix was added to the liquid material and stirred for 15 s. Then the speed was increased to 12500 r / min and high shear was applied for 35 s. After the high shear was completed, the speed was reduced to 650 r / min and hollow glass microspheres were added in 3 batches. The time was started from the addition of the first batch of hollow glass microspheres. The total time for the 3 batches of material addition and low-speed stirring was 3 min, resulting in elastic self-healing cement slurry.
[0094] Example 5 The mixture comprises 100 parts by weight of Grade G oil well cement, 20 parts by weight of hollow glass microspheres, 12 parts by weight of microsilica, 1.33 parts by weight of water loss reducer, 0.3 parts by weight of drag reducer, 7 parts by weight of anti-gas channeling agent, 0.2 parts by weight of defoamer, 4 parts by weight of silane-modified rubber powder, 10 parts by weight of latex, 0.8 parts by weight of silane-modified carbon fiber, and 44 parts by weight of water for slurry preparation. The theoretical slurry density, calculated based on the nominal density of the raw materials, is approximately 1.35 g / cm³. 3 The actual value shall be based on the results of the pre-mixing test.
[0095] This embodiment also provides a method for preparing elastic self-healing cement grout, which is prepared according to the following steps: Step 1, Raw material pretreatment: 1.33 parts by mass of the water loss reducing agent were dispersed in external water to prepare an aqueous solution of the water loss reducing agent with a mass concentration of 33.3%.
[0096] 0.3 parts by mass of drag-reducing agent were dispersed in external water to prepare an aqueous solution of drag-reducing agent with a mass concentration of 33.3%.
[0097] 24 parts by weight of water were measured from the 44 parts by weight of water used for slurry preparation in this embodiment, and 12 parts by weight of microsilica were added to it. The mixture was dispersed using a high-speed disperser at 2000 r / min for 10 min to obtain secondary agglomerates D. 90 Microsilica slurry with a particle size not exceeding 10 μm and wet dispersion.
[0098] Step 2: Preparation of solid-phase premix and liquid-phase materials A horizontal ribbon mixer was used to dry mix G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber. The dry mixing speed was 55 r / min and the dry mixing time was 10 min. This ensured that the silane-modified carbon fiber was evenly dispersed without forming fiber clumps, thus obtaining a solid premix.
[0099] Add the remaining 20 parts by weight of slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer to the liquid phase tank, and circulate and stir at 950 r / min for 5 min to form a uniform liquid phase material.
[0100] Step 3: Mix in sequence to form an elastic self-healing cement slurry. Under continuous stirring conditions at a speed of 3800 r / min, the solid premix was added to the liquid material and stirred for 15 s. Then the speed was increased to 11500 r / min and high shear was applied for 35 s. After the high shear was completed, the speed was reduced to 550 r / min and hollow glass microspheres were added in 3 batches. The time was started from the addition of the first batch of hollow glass microspheres. The total time for the 3 batches of material addition and low-speed stirring was 3 min, resulting in elastic self-healing cement slurry.
[0101] Comparative Example 1 The density of the cement slurry obtained by using 100 parts by weight of Grade G oil well cement and 44 parts by weight of water for slurry preparation is 1.89 ± 0.02 g / cm³. 3 .
[0102] In this comparative example, G-grade oil well cement was added to the slurry preparation water and stirred for 15 seconds under continuous stirring conditions at a speed of 4000 r / min. Then, the speed was increased to 12000 r / min and high shear was applied for 35 seconds to obtain cement slurry.
[0103] Comparative Example 2 The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 35.5 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0104] The preparation method of this comparative example is the same as that of Example 1.
[0105] Comparative Example 3 The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 45.1 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0106] The preparation method of this comparative example is the same as that of Example 1.
[0107] Comparative Example 4 The cement slurry, consisting of 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 0.4 parts by weight of silane-modified carbon fiber, and 57.1 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0108] The preparation method of this comparative example is the same as that of Example 1.
[0109] Comparative Example 5 The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 0.4 parts by weight of silane-modified carbon fiber, and 58.2 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0110] The preparation method of this comparative example is the same as that of Example 1.
[0111] Comparative Example 6 The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, and 43.8 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0112] The preparation method of this comparative example is the same as that of Example 1.
[0113] Comparative Example 7 The following ingredients were added: 100 parts by weight of Grade G oil well cement, 15 parts by weight of oil well cement weight-reducing agent, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducing agent, 0.5 parts by weight of drag reducing agent, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 90.9 parts by weight of water for slurry preparation. The resulting cement slurry had a density of 1.42 ± 0.02 g / cm³. 3 .
[0114] The preparation method of this comparative example is the same as that of Example 1.
[0115] The oil well cement weight-reducing agent used in this comparative example is the CP-52 type oil well cement weight-reducing agent from Beijing Aokaili Technology Development Co., Ltd., which is a conventional hollow ceramic microsphere of the cenosphere type with a density ≤0.80g / cm³. 3 Bulk density ≤ 0.50 g / cm³ 3 The slurry density was ≤10% on a 0.315mm sieve and ≤0.2% on a moisture content sieve. The density of the slurry was adjusted to be the same as that of the cement slurry in Example 1, which was 1.42 ± 0.02 g / cm³, by adjusting the amount of conventional hollow ceramic microspheres and water used in the slurry preparation. 3 .
[0116] Comparative Example 8 The cement slurry, made from 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 4 parts by weight of microsilica, 1 part by weight of water loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 31.6 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0117] The preparation method of this comparative example is the same as that of Example 1.
[0118] Comparative Example 9 The following ingredients were added: 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 15 parts by weight of microsilica, 1 part by weight of water loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 40.9 parts by weight of water for slurry preparation. The density of the resulting cement slurry was 1.42 ± 0.02 g / cm³. 3 .
[0119] The preparation method of this comparative example is the same as that of Example 1.
[0120] Comparative Example 10 The cement slurry, consisting of 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 2 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 36.7 parts by weight of water for slurry preparation, has a density of 1.42 ± 0.02 g / cm³. 3 .
[0121] In this comparative example, the raw materials and amounts used are the same as in Example 1. The difference is that, during preparation, the microsilica is not dispersed using slurry water, but is directly dry-mixed with Grade G oil well cement, silane-modified rubber powder, and silane-modified carbon fiber to obtain a solid premix. Other preparation steps are the same as in Example 1.
[0122] Microsilicon does not undergo wet depolymerization, and its secondary aggregates D 50 20–25 μm, D 90 The size is 45–55 μm; hollow glass microspheres D 50 The density is 40 μm; the D of silane-modified rubber powder 50 45–60 μm, D 90 It has a fine particle size of 90–110 μm.
[0123] In this comparative example, the particle size distribution of the three types of particles—hollow glass microspheres, silane-modified rubber powder, and microsilica—is in the range of approximately 20–60 μm, which cannot be compared with D. 50 To form G-grade oil well cement with a particle size of 15–25 μm, a three-level particle size distribution consisting of submicron-sized filler particles, main skeleton particles, and flexible coarse particles is created, resulting in a particle size mismatch. This is achieved by using the maximum density difference... Δρ =max(| ρ 上 - ρ 中 |,| ρ 中 - ρ 下 |,| ρ 上 - ρ 下 |) Evaluation of particle size compatibility effect by free liquid, rheology, thickening time and permeability after curing.
[0124] Comparative Example 11 The following ingredients were added: 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of water loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 0.5 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 37.5 parts by weight of water for slurry preparation. The resulting cement slurry had a density of 1.42 ± 0.02 g / cm³. 3 .
[0125] The preparation method of this comparative example is the same as that of Example 1.
[0126] Comparative Example 12 The following ingredients were added: 100 parts by weight of Grade G oil well cement, 15 parts by weight of hollow glass microspheres, 10 parts by weight of microsilica, 1 part by weight of fluid loss reducer, 0.5 parts by weight of drag reducer, 5 parts by weight of anti-gas channeling agent, 0.1 parts by weight of defoamer, 5 parts by weight of silane-modified rubber powder, 14 parts by weight of latex, 0.4 parts by weight of silane-modified carbon fiber, and 35.0 parts by weight of water for slurry preparation. The resulting cement slurry had a density of 1.42 ± 0.02 g / cm³. 3 .
[0127] The preparation method of this comparative example is the same as that of Example 1.
[0128] The invention will now be illustrated using a supercritical carbon dioxide coaxial closed-circuit geothermal well with a depth of approximately 2500m as an example. The wellbore diameter at the second opening is approximately 241.3mm, and the outer diameter of the production casing is approximately 177.8mm. The production casing is constructed using carbon dioxide corrosion-resistant materials and features airtight threaded connections. The cement slurry design and cementing operations were verified based on measured well temperature, well diameter, drilling fluid properties, formation pressure bearing capacity, and predetermined return height.
[0129] When determining the preparation method of elastic self-healing cement slurry for supercritical carbon dioxide coaxial closed geothermal wells, it is necessary to systematically design the performance of elastic self-healing cement slurry based on the actual engineering boundary conditions of the well. Specifically, based on measured or relevant data, parameters such as well depth, well diameter, casing size, formation fracture pressure, bottom hole static temperature, and circulating temperature are obtained. Based on annular hydraulic calculations and cementing engineering software simulations, the key performance indicators of the cement slurry are determined. Specific performance indicators include: cement slurry density, thickening time, rheology, water loss, compressive strength, and elastic properties.
[0130] S1. Determine the design boundary of cement slurry. In this invention, the bottom hole circulating temperature is 180℃, the bottom hole static temperature is 200℃, the bottom hole total pressure is 50MPa, and the carbon dioxide partial pressure is 15MPa.
[0131] During performance testing, the prepared elastic self-healing cement slurry was tested using a simulation of the aforementioned supercritical carbon dioxide coaxial closed geothermal well, as detailed below: The simulated formation water contained 80g NaCl, 10g CaCl2, 5g MgCl2·6H2O, 3g KCl and 2g NaHCO3 per liter, with a total mineralization of 100g / L and a pH of 5.5±0.2 before carbon dioxide was introduced.
[0132] The temperature cycle ranged from 30℃ to 180℃, and the pressure cycle ranged from 10MPa to 50MPa, with 10 cycles in total. The heating and cooling rates were both 3℃ / min, and the pressure increase and decrease rates were both 1MPa / min. The high-temperature and low-temperature ends were each held at temperature for 2 hours and pressure for 2 hours. This evaluation path covers the high-temperature and high-pressure conditions during the cementing and operation of supercritical carbon dioxide geothermal wells, as well as the repeated start-up and shutdown conditions simulated by temperature and pressure cycles between 30℃, 10MPa and 180℃, 50MPa.
[0133] The specific temperature and pressure cycling procedure is as follows: First, maintain the temperature and pressure at 30℃ and 10MPa for 2 hours; then, increase the temperature and pressure to 180℃ and 50MPa at a heating rate of 3℃ / min and a pressurization rate of 1MPa / min, and maintain the temperature and pressure at 180℃ and 50MPa for 2 hours; then, decrease the temperature and pressure to 30℃ and 10MPa at a cooling rate of 3℃ / min and a pressurization rate of 1MPa / min, and maintain the temperature and pressure at 30℃ and 10MPa for 2 hours, completing one temperature and pressure cycle; repeat the same procedure 10 times.
[0134] For the aforementioned supercritical carbon dioxide coaxial closed geothermal well, the target slurry density of the elastic self-healing cement slurry is 1.35 g / cm³. 3 ~1.49g / cm 3The pumpable time at 180℃ is no less than 180 min; the curing and carbon dioxide exposure cycles are 24 h, 7 d, 28 d, and 90 d. Its performance indicators are: water loss at 180℃ high temperature and high pressure no greater than 50 mL / 30 min, thickening time 180–300 min, and maximum density difference between the upper / middle / lower parts no greater than 0.03 g / cm³. 3 The 24-hour compressive strength is not less than 14 MPa, the 28-day elastic modulus is not more than 6 GPa, the ultimate strain is not less than 0.5%, the permeability is not more than 0.1 mD, the bonding strength of the casing-elastic self-healing cement stone interface is not less than 2.0 MPa, the leakage rate under a pressure difference of 5 MPa after 10 temperature and pressure cycles is not more than 0.1 mL / min, and the sealing recovery rate after 28 days of self-healing curing is not less than 80%.
[0135] It should be noted that in this invention, the target slurry density is obtained through volume balance calculation based on the well conditions of the target well. Furthermore, according to the design formula of this invention, a small amount of slurry is prepared, and the actual density and basic properties of the actual slurry are measured to verify whether the elastic self-healing cement slurry of the target slurry density meets the requirements. The final target slurry density is 1.35 g / cm³. 3 ~1.49g / cm 3 It meets the usage requirements.
[0136] S2. Lower the casing and install the cyclone stabilizer. like Figure 1 As shown, the system adopts a coaxial double-string structure. Specifically, the coaxial double-string is installed inside the wellbore, including a casing 2 and an inner tube 3. The casing 2 is a 3Cr CO2-resistant gas-tight casing. The inner tube 3 is placed inside the casing 2 and installed coaxially. An inner tube channel is formed inside the inner tube 3, serving as an injection channel for low-temperature, high-pressure CO2. An annular channel is formed between the outer wall of the inner tube 3 and the inner wall of the casing 2, serving as a reflux channel for heated CO2. The annular channel and the inner tube channel form a dual-flow separation of injection and reflux. A vortex stabilizer 6 is provided on the outer wall of the casing 2 to ensure that the string is centered. The periphery is filled with cement slurry prepared according to this invention to form an elastic self-healing cement stone 4, which serves as a permanent sealing layer between the casing 2 and the formation 5, preventing gas from escaping along the annulus. A gas-tight threaded connection component 7 is provided at the connection of adjacent casing 2 sections to seal and connect the casing sections into a continuous casing string and prevent high-pressure CO2 from leaking along the threaded connection. Finally, the well bottom is sealed using a closed-loop bottomhole assembly 8, while the wellhead is temporarily sealed using a corrosion-resistant sealing wellhead 1. Through the coordinated action of these components, a closed annular space sealing barrier is formed, achieving effective isolation of reservoir fluids and safe CO2 injection.
[0137] When installing the vortex centralizer 6, both elastic and rigid vortex centralizers are installed on the outer wall of casing 2. The elastic vortex centralizer is installed in the wellbore deviation section, wellbore diameter section, and sections prone to eccentricity where casing resistance is high, to improve throughput and repositioning capabilities through its elastic deformation. The rigid vortex centralizer is installed in the target cement-sealed section where the wellbore diameter is relatively regular and stable radial support is required to maintain annular clearance. Specifically, the vortex centralizer 6 is densely installed in the wellbore deviation section, the easily eccentric section, the target cement-sealed section, and locations where displacement efficiency is expected to be low, to achieve a casing centering accuracy of over 75%. The elastic vortex centralizer uses the integral spiral elastic casing centralizer from Feizhe Petroleum Equipment (Liaoning) Co., Ltd., and the rigid vortex centralizer uses the company's resin spiral rigid casing centralizer. The specific specifications of the vortex centralizer are selected based on the casing outer diameter and the actual drilled well diameter. The spiral guide ribs are spirally distributed on the vortex centralizer body at a 45°±2° angle to the axis of casing 2. The starting force, lowering force, resetting force, and passability are inspected according to API Spec 10D / ISO 10427-1. The installation spacing of the vortex centralizer 6 is 3m in the well inclination change section, the easily eccentric section, and the target sealing section, and 6m in other well sections. The final spacing is verified by casing centering calculation. The vortex blades of the vortex centralizer 6 generate a circumferential velocity component in the upward-flowing cement slurry, improving the flow in the narrow annulus and drilling fluid replacement. This avoids the problem of casing eccentricity, insufficient flow velocity in the narrow annulus, and drilling fluid residue forming localized non-cemented zones, which, even with good elasticity of the cement slurry, make it difficult to form a continuous and uniform annular sealing barrier.
[0138] like Figure 4 As shown, the vortex stabilizer 6 keeps the casing 2 centered during cementing operations and guides the cement slurry to generate axial upward and circumferential vortex flow in the annulus through the spiral guide bar, reducing the narrow edge stagnation zone in the annulus, improving the displacement effect of drilling fluid at the narrow edge, thereby reducing drilling fluid residue, and enabling the cement slurry to form a relatively uniform, annular, and continuous elastic self-healing cement stone between the casing 2 and the well wall, and reducing the risk of interface channel formation, thus achieving reliable isolation of formation fluids.
[0139] S3. Implement pre-fluid isolation and cement slurry replacement. During construction, to ensure that flocculation or abnormal thickening does not occur in the on-site contact ratio of drilling fluid, pre-flush fluid, and cement slurry, the rheological compatibility of this mixture was first evaluated. Compatibility tests were conducted at volume ratios of drilling fluid:pre-flush:cement slurry of 100:0:0, 75:25:0, 50:50:0, 0:75:25, 0:50:50, and 0:0:100. The appearance and relative deviation of rheological parameters before and after mixing were used as judgment indicators. The requirements were no visible flocculation, no abnormal thickening, and a rheological parameter deviation of no more than 20%. The test results were used to determine the suitability of the pre-flush formulation and to assess the risk of abnormal thickening or blockage during pumping and displacement. The cement slurry pumping flow rate was set at 1.0 m³ / h. 3 / min, displacement fluid discharge rate set to 1.2m 3 The design annular Reynolds number is not less than 2100, and the maximum construction pump pressure is set at 35MPa, which shall not exceed the allowable pressure values of the formation, casing, wellhead and surface pipelines.
[0140] After the drilling fluid performance is adjusted and wellbore stability is confirmed, a pre-fluid compatible with the existing drilling fluid and cement slurry is pumped into the annulus between casing 2 and inner casing 3 via a cementing equipment. This pre-fluid flows along the same path as the subsequent cement slurry into the annulus between the outer wall of casing 2 and the wellbore. The pre-fluid serves to isolate the drilling fluid from the cement slurry. The pre-fluid is a BCS-010L type fatty acid glyceride cementing flushing agent from Tianjin Zhongyou Boxing Engineering Technology Co., Ltd., with a 5% NaCl aqueous solution as the base fluid. The BCS-010L dosage is set at 3.5% of the base fluid mass. The pre-fluid volume is 1.2 times the effective contact volume within the casing and annulus, ensuring a contact time of at least 10 minutes. It should be noted that the drilling fluid is already present in the wellbore during drilling and casing installation.
[0141] like Figure 2 As shown, the cement slurry prepared in the example is then continuously pumped into the annular channel between casing 2 and inner tube 3 through a cementing equipment. Displacement fluid is also pumped into the annular channel between casing 2 and inner tube 3. The displacement fluid then presses the pre-filled fluid and cement slurry into the annular region between the outer wall of casing 2 and the wellbore in the pumping sequence, causing the cement slurry to rise along the annular region to the designed height. The displacement fluid used is a water-based displacement fluid prepared with GL-2 type ultra-high temperature cementing separator from Sichuan Hongsheng Petroleum Engineering Technology Service Co., Ltd. A 5% NaCl aqueous solution is used as the base fluid, and the displacement fluid is added at 1.5% of the base fluid mass. The mixture is stirred at 800±50 r / min for 10 min, allowed to stand for hydration for 45 min, and then circulated and stirred for another 5 min before use, resulting in a density of 1.10±0.02 g / cm³. 3 .
[0142] S4. After setting and forming elastic self-healing cement stone. After the replacement is completed, close the corresponding valves and allow it to solidify according to the time determined by the thickening test. Figure 3 As shown, during the cement slurry curing process, the anti-gas channeling agent, latex, and water loss reducing agent work together to reduce gas intrusion and filtrate precipitation during the transition period; after curing, as... Figure 3 As shown in Figure a, in the initial cemented state, a uniform and continuous annular cementation is formed between the casing 2 and the well wall. The high-strength hollow glass microspheres and the elastic self-healing cement stone matrix jointly bear the annular pressure. Microsilica fills the pores, silane-modified rubber powder and latex form an elastic buffer phase, and silane-modified carbon fibers cross potential cracks and limit crack propagation.
[0143] like Figure 3 As shown in b, after the wellbore undergoes temperature and pressure cycles, microcracks or microannular gaps may form at the interface due to the difference in thermal expansion between the casing and the elastic self-healing cement stone, as well as the effects of alternating stress. At this time, the elastic components in the elastic self-healing cement stone maintain a tight fit with the casing interface, preventing further expansion of the microannular gaps. Simultaneously, the incompletely hydrated cement particles exposed on the fracture surface continue to undergo hydration reactions. Microsilica reacts with calcium hydroxide released during cement hydration to produce pozzolanic reactions, and the resulting hydrated calcium silicate gel and other products deposit and fill the pores within the fracture channels. The flexible phase formed by silane-modified rubber powder and latex maintains the adhesion between the fracture surface and the interface, while silane-modified carbon fibers limit the further opening of the cracks. The synergistic effect of continuous reaction filling, elastic adhesion, and fiber-limited crack control allows the damaged elastic self-healing cement stone to automatically restore its sealing integrity, effectively blocking potential channels for CO2 or formation fluids to escape along the annulus.
[0144] S5. Conduct cementing quality and thermo-pressure cycle integrity evaluation. Samples of the elastic self-healing cement stone of this invention were prepared, and their compressive strength, elastic modulus, permeability, interfacial bonding strength, and crack self-healing ability were tested under carbon dioxide environment and designed temperature and pressure cycling conditions according to step S1. If local channeling, interfacial debonding, or unacceptable pressure maintenance were found, remedial cementing was performed according to the test location, and the well was re-accepted.
[0145] Each test group used 3 parallel samples for measurement, and the results are expressed as the average value. The test results are shown in Tables 1 to 3.
[0146] Table 1 Performance data of Examples 1 to 3 and Comparative Examples 1 to 2
[0147] Table 2 Performance data of Comparative Examples 3 to 7
[0148] Table 3 Performance data of Comparative Examples 8 to 12
[0149] In the present invention, except for the variables to be investigated, the raw material batches, grouting water, grout density, mixing procedures, curing regimes, and temperature / pressure / carbon dioxide exposure conditions of each group in Example 1 and Comparative Examples 1 to 12 are kept consistent. If the density of the elastic self-healing cement grout changes due to the reduction or replacement of components, the grouting water volume is adjusted or an isodense group is set to correct for the influence of density differences on the comparison results.
[0150] As shown in Tables 1-3, the water loss at 180℃ and high pressure in Examples 1-3 were 27 mL / 30 min, 24 mL / 30 min, and 31 mL / 30 min, respectively; the thickening times were 236 min, 221 min, and 248 min, respectively; the free liquid volume was 0 in all cases; and the maximum density difference between the upper, middle, and lower parts was 0.01 g / cm³. 3 0.02g / cm 3 and 0.02g / cm 3 All examples have a stable construction window. The thickening times for Examples 4 and 5 are 213 min and 209 min, respectively. Comparative Examples 1, 2, 4, 5, 7, 8, and 10 show significant deterioration in at least one of the following: water loss, free liquid, or settling stability; the thickening time for Comparative Example 9 is shortened to 165 min, which is detrimental to the on-site safety margin.
[0151] The mechanical property results in Tables 1-3 show that the 24-hour compressive strengths of Examples 1-3 are 19.6 MPa, 21.8 MPa, and 17.4 MPa, respectively, and the 28-day compressive strengths are 31.8 MPa, 34.2 MPa, and 28.7 MPa, respectively; the 28-day elastic modulus is 4.8-5.7 GPa, the ultimate strain is 0.55%-0.71%, and the interfacial bonding strength between the sleeve and the elastic self-healing cement stone is 2.86-3.28 MPa. Example 1 achieves a better balance between strength, low elastic modulus, deformation capacity, and interfacial bonding strength; due to the omission of key components, deviations in dosage, or particle size mismatch, at least one property of each comparative example is significantly lower than that of Example 1.
[0152] The crack self-healing test employed displacement-controlled loading to create a through or semi-through crack with an initial width of 200±20μm on a cylindrical specimen. The sides of the specimen were sealed with epoxy resin, leaving only the two ends of the crack as fluid inlets and outlets. Under a fixed pressure difference of 5MPa, the permeability k0 of the intact specimen and the permeability k after the crack were measured sequentially. 裂 The cracked sample was then placed in simulated formation water at 180℃, a total pressure of 50MPa, and a CO2 partial pressure of 15MPa for 28 days for repair and curing. After cooling and depressurization, the permeability k after repair was measured using the same apparatus and pressure difference. 修Three parallel samples were prepared for each formulation, and the criterion for a valid sample was that the crack width deviation should not exceed 20 μm.
[0153] Sealing recovery rate =
[0154] The results of CO2 resistance, thermo-pressure cycling, and self-healing performance in Tables 1-3 show that the compressive strength retention rates of Examples 1-3 after 28 days of CO2 exposure were 91.5%, 93.0%, and 88.2%, respectively, and the mass change rates were -0.8%, -0.6%, and -1.2%, respectively. The leakage rates after 10 thermo-pressure cycles were 0.018 mL / min, 0.026 mL / min, and 0.032 mL / min, respectively, and the 28-day seal recovery rates were 88.6%, 85.4%, and 87.2%, respectively. Example 1 showed the lowest leakage and the highest seal recovery rate. The seal recovery rates of Comparative Examples 1-12 ranged from 37.5% to 73.2%, and each example showed deficiencies in at least one of the following: construction stability, elastic deformation, interfacial bonding, and CO2 resistance or cyclic sealing performance.
[0155] As shown in Tables 1-3, Examples 1-3 of this invention are all based on the operating conditions of supercritical carbon dioxide geothermal wells under high temperature of 180℃, pressure of 50MPa, carbon dioxide-salt water corrosion, and repeated temperature and pressure cycles. The core technology is not a simple superposition of single additives, but rather a synergistic combination of high-pressure-bearing hollow glass microspheres, microsilica, and EPDM silane-modified rubber powder with three-stage particle size matching; styrene-butadiene latex, silane-modified rubber powder, and silane-modified carbon fiber elastic bridging; and reduced water loss, prevention of gas channeling, and interface sealing. These technologies collectively solve the technical problem of failure of the elastic self-healing cement stone seal integrity under high temperature and high pressure alternating conditions in supercritical carbon dioxide geothermal wells.Specifically, microsilica, Grade G oil well cement / hollow glass microspheres, and silane-modified rubber powder constitute a three-dimensional particle size distribution system. Microsilica fills the secondary pores between Grade G oil well cement particles and hollow glass microspheres to reduce permeability. Hollow glass microspheres provide pressure support while reducing slurry density. Silane-modified rubber powder, as a flexible third-scale particle, avoids competition for adsorbents from fine powders and buffers concentrated stress. As shown in Comparative Example 2, omitting microsilica alone causes a sharp increase in permeability to 0.146 mD, while replacing hollow glass microspheres with conventional weight-reducing agents significantly reduces compressive strength; for example, in Comparative Example 7, the 24-hour compressive strength is only 14.9. MPa; Simultaneously, silane-modified rubber powder and styrene-butadiene latex form a dispersed flexible phase and a continuous polymer film in the elastic self-healing cement stone. Taking Example 1 as an example, compared with Comparative Example 1, the elastic modulus decreased from 10.6 GPa to 4.8-5.7 GPa, and the ultimate strain increased from 0.22% to 0.55%-0.71%. Meanwhile, silane-modified carbon fibers bridged across cracks, limiting crack propagation and forming a crack-resistant network with flexible phase buffering, fiber bridging constraint, and interface film sealing. In Comparative Example 6, even without silane-modified carbon fibers, the elastic modulus was still as high as 5.9 GPa and the ultimate strain was only 0.44%. In Comparative Example 3, even without silane-modified rubber powder, the leakage rate after temperature and pressure cycling was as high as 0.620 mL / min, far exceeding the 0.018 mL / min of Example 1, indicating the synergistic effect between the elastic phase and the fiber. In terms of crack self-healing, unhydrated cement particles and micro Silicon continuously undergoes hydration and volcanic ash reaction at the crack surface to generate CSH gel that fills the channels. Silane-modified rubber powder and latex polymer film utilize their low glass transition temperature and high elasticity to achieve adhesion to the crack surface. Silane-modified carbon fiber restricts the repeated opening and closing of the crack during thermo-pressure cycling, preventing the repair product from peeling off. As a result, the leakage of Example 1 after 10 thermo-pressure cycles was only 0.018 mL / min, and the 28-day seal recovery rate reached 88.6%. In contrast, Comparative Example 5, which omitted both rubber powder and latex, had a recovery rate of only 43.6%, and Comparative Example 3, which omitted silane-modified rubber powder, had a recovery rate of only 54.7%, both significantly lower than Example 1. Furthermore, the water loss reducing agent, the gas channeling prevention agent, and the latex together control the filtrate precipitation, shorten the static gelation transition, and form an interfacial film during the coagulation period. As a result, the water loss of Example 1 was only 27 mL / 30 min, the free liquid was 0, and the density difference between the upper and lower parts was only 0.01 g / cm. 3 This ensures efficient replacement and annular sealing. The combination of this invention maintains the density and pressure-bearing capacity of the elastic self-healing cement stone while reducing density, and achieves micro-crack self-healing and seal restoration through continuous hydration and filling with volcanic ash reaction products, flexible phase bonding, and fiber-limited cracking. Comparative Examples 1 to 12, through isodense replacement, omission of single components, out-of-range dosage, and particle size mismatch, disrupted the above synergistic relationship, failing to simultaneously meet the comprehensive performance requirements in terms of workability, elasticity, resistance to carbon dioxide corrosion, and thermo-pressure cyclic sealing, and thus cannot adapt to the harsh operating conditions of supercritical carbon dioxide geothermal wells.
[0156] It should be noted that the following parameters need to be recorded during the actual construction process: For solid-phase premixing, the equipment, rotation speed, time, and feeding sequence should be recorded; for liquid-phase preparation, the actual water volume, stirring speed, and time should be recorded; for high-shear dispersion, the rotation speed or shear rate and duration should be recorded; for glass microsphere addition, the number of batches, low-shear rotation speed, and time should be recorded.
[0157] For casing centering, the centering degree, centralizer model, and spacing should be recorded; for vortex structures, the blade angle, number, and installation position should be recorded; for pre-fluid, the type, volume, contact time, and compatibility results should be recorded; for pumping and displacement, the discharge rate, annular flow regime or Reynolds number, and maximum pump pressure should be recorded; for curing after condensation, the time, temperature, and pressure should be recorded; for quality evaluation, the logging method, pressure integrity test, and acceptance criteria should be recorded.
[0158] The above-described embodiments are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various improvements and substitutions without departing from the principles of the present invention, and these improvements and substitutions should also be considered within the scope of protection of the present invention.
Claims
1. An elastic self-healing cement grout, characterized in that, This includes G-grade oil well cement, auxiliary materials, and water for grout preparation; Based on the weight of Grade G oil well cement, the percentage of each component in the auxiliary materials is as follows: hollow glass microspheres 10%–20%, microsilica 8%–12%, water loss reducer 0.67%–1.33%, drag reducer 0.3%–0.67%, anti-gas channeling agent 3%–7%, defoamer 0.05%–0.2%, silane-modified rubber powder 1%–4%, latex 10%–18%, and silane-modified carbon fiber 0.2%–0.8%.
2. The elastic self-healing cement grout according to claim 1, characterized in that, The percentage of each component in the auxiliary materials by weight of G-grade oil well cement is as follows: hollow glass microspheres 12%–18%, microsilica 10%–12%, fluid loss reducer 1%–1.17%, drag reducer 0.5%–0.67%, anti-gas channeling agent 5%–6%, defoamer 0.1%–0.15%, silane-modified rubber powder 1.5%–3%, latex 12%–16%, and silane-modified carbon fiber 0.3%–0.6%.
3. The elastic self-healing cement grout according to claim 1, characterized in that, Hollow glass microspheres are sodium-calcium borosilicate hollow glass beads. The D of the hollow glass microspheres... 10 The size ranges from 15μm to 25μm.
4. The elastic self-healing cement grout according to claim 1, characterized in that, Grade G oil well cement D 50 The diameter of primary particles in microsilicon ranges from 15μm to 25μm; the average diameter of primary particles in microsilicon ranges from 0.15μm to 0.20μm.
5. The elastic self-healing cement grout according to claim 1, characterized in that, Silane-modified rubber powder is obtained by modifying rubber powder after vulcanization with a methacryloyloxy silane coupling agent.
6. The elastic self-healing cement grout according to claim 5, characterized in that, The methacryloyloxy silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane, and the D of the rubber powder is... 50 The size ranges from 90μm to 120μm.
7. The elastic self-healing cement grout according to claim 1, characterized in that, Silane-modified carbon fiber is obtained by oxidizing carbon fiber and then impregnating it with an amino-based silane coupling agent.
8. The elastic self-healing cement grout according to claim 7, characterized in that, The amino-based silane coupling agent is γ-aminopropyltriethoxysilane, and the length of the carbon fiber is 2.5 mm to 3.5 mm.
9. A method for preparing the elastic self-healing cement grout according to any one of claims 1 to 8, characterized in that, Includes the following steps: Weigh each component according to the mass fraction; disperse the water loss reducing agent in external water to obtain an aqueous solution of the water loss reducing agent, and disperse the drag reducing agent in external water to obtain an aqueous solution of the drag reducing agent; Divide the water used for slurry preparation into two portions; disperse the microsilica in one portion of water and disperse evenly to obtain the microsilica slurry. G-grade oil well cement, microsilica slurry, silane-modified rubber powder, and silane-modified carbon fiber are mixed in the first stage to obtain a solid premix. Another portion of the slurry preparation water, latex, water loss reducing agent aqueous solution, drag reducing agent aqueous solution, anti-gas channeling agent and defoamer are mixed a second time to form a liquid phase material; The solid premix and liquid material are first stirred at 3800 r / min to 4200 r / min. After the first stirring is completed, the speed is increased to 11500 r / min to 12500 r / min for the second stirring. After the second stirring is completed, the speed is reduced to 550 r / min to 650 r / min, hollow glass microspheres are added, and a third stirring is carried out to obtain elastic self-healing cement slurry.
10. The application of the elastic self-healing cement slurry according to any one of claims 1 to 8 in a supercritical carbon dioxide geothermal well, characterized in that, The application method is as follows: pre-filled fluid, elastic self-healing cement slurry and displacement fluid are pumped sequentially into the annulus channel of the coaxial double-tube column in the supercritical carbon dioxide geothermal well. The displacement fluid is used to press the pre-filled fluid and elastic self-healing cement slurry into the annulus area between the outer wall of the coaxial double-tube column and the formation (5). The elastic self-healing cement slurry returns to the required position along the annulus area. After solidification, elastic self-healing cement stone (4) is formed. The coaxial double column includes a sleeve (2) and an inner tube (3). The inner tube (3) is coaxially sleeved inside the sleeve (2). An annular channel is formed between the outer wall of the inner tube (3) and the inner wall of the sleeve (2). A vortex stabilizer (6) is located on the outer wall of the sleeve (2) to keep the coaxial double column in the center position.