A modified ultra-high performance concrete, its preparation method and application
By using a combination of fly ash ultrafine microspheres and graded microspheres in ultra-high performance concrete, the application challenges of fly ash in UHPC have been solved, achieving cost reduction and performance improvement, and making it suitable for engineering projects such as bridges and tunnels.
Patent Information
- Application Number
- CN202611128917.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
The existing preparation process for ultra-high performance concrete (UHPC) is complex and costly. Fly ash cannot meet the stringent requirements for workability and strength, and a dedicated gradation system has not been formed, resulting in limited improvement in strength and durability.
Using fly ash ultrafine microspheres as the core component, combined with graded microspheres of cement, silica fume and fly ash, and controlling their content in the gel material, along with steel fibers and water-reducing agents, the compressive strength and workability are improved through a simple preparation method.
It reduces production costs, improves compressive strength and workability, and realizes high-strength and easy-to-construct ultra-high-performance concrete, which is suitable for engineering applications.
Smart Images

Figure CN123106101A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of building materials and solid waste resource utilization technology, specifically to a modified ultra-high performance concrete, its preparation method, and its application. Background Technology
[0002] Ultra-high performance concrete (UHPC) is a revolutionary cement-based composite material characterized by ultra-high strength, high toughness, and high durability. It is a key material for promoting the transformation of buildings and infrastructure towards lightweight, long-life, and intelligent construction. However, its preparation process is complex and costly, which hinders its large-scale promotion.
[0003] my country's annual fly ash emissions are enormous, and its resource utilization has shifted from "end-of-pipe treatment" to a systematic project of "source carbon reduction and high-value conversion," which is a key path to achieving "dual carbon" goals and a circular economy. Currently, fly ash is difficult to effectively use in ultra-high performance concrete (UHPC), mainly due to the following technical obstacles: 1) Ordinary fly ash contains many impurities and has a wide particle size distribution, making it difficult to meet the stringent requirements of UHPC for workability and strength; 2) No dedicated gradation system has been formed, resulting in limited improvement in strength and durability.
[0004] Therefore, how to effectively utilize fly ash to improve the strength and workability of ultra-high performance concrete while reducing its production cost is a pressing technical problem that needs to be solved. Solving this problem is of great significance to the high-value utilization of solid waste and the development of high-performance building materials. Summary of the Invention
[0005] In view of this, one objective of this application is to provide a modified ultra-high performance concrete, which, due to the presence of more than 10 wt% fly ash ultrafine particles in its raw materials, can significantly reduce the production cost of ultra-high performance concrete, and can also improve the compressive strength (≥120MPa) and workability (e.g., spread ≥650mm) of ultra-high performance concrete, ensuring that the material meets the requirements of engineering applications.
[0006] Another objective of this application is to provide a method for preparing modified concrete that exceeds high performance.
[0007] Another objective of this application relates to the application of modified concrete beyond high-performance concrete.
[0008] Another object of this application is to provide an industrialized prefabricated component.
[0009] To achieve the above objectives, the first aspect of this application proposes a modified ultra-high performance concrete, wherein the raw materials of the modified ultra-high performance concrete include gel materials, aggregates, admixtures and fibers; the gel materials include fly ash ultrafine particles, and the mass content of the fly ash ultrafine particles in the gel materials is more than 10%.
[0010] In some embodiments, the fly ash ultrafine beads have a mass content of 10-20% in the gel material.
[0011] In some embodiments, the Dv50 particle size of the fly ash ultrafine particles is less than 10 μm.
[0012] In some embodiments, the gel material further includes graded microspheres of cement, silica fume, and fly ash.
[0013] In some embodiments, the mass ratio of the cement, silica fume, fly ash ultrafine beads, and fly ash graded microbeads is (65-80):(8-15):(10-20):(5-10).
[0014] In some embodiments, the fly ash grading microspheres have a Dv50 particle size greater than 10 μm and less than 20 μm.
[0015] In some embodiments, the aggregate comprises continuously graded quartz sand and / or continuously graded fine aggregate.
[0016] In some embodiments, the admixture includes a water-reducing agent.
[0017] In some embodiments, the water-reducing agent includes a polycarboxylate water-reducing agent.
[0018] In some embodiments, the solid content of the water-reducing agent is 1.5 to 2.5%.
[0019] In some embodiments, the fibers include steel fibers.
[0020] In some embodiments, the volume fraction of the steel fibers is 1.5 to 2.5%.
[0021] In some embodiments, the mass ratio of the gel material, aggregate, additives and fiber is (88-125):(110-130):(1.5-3.0):(1.5-3.0).
[0022] In some embodiments, the modified ultra-high performance concrete further includes water, and the mass ratio of the water to the gel material is 0.16 to 0.20, optionally 0.17 to 0.19.
[0023] In some embodiments, the modified ultra-high performance concrete has a 28-day compressive strength of over 120 MPa and a spread of over 650 mm.
[0024] The second aspect of this application discloses a method for preparing modified ultra-high performance concrete, comprising: The gel material and the aggregate are dry-mixed to obtain a dry-mixed material. Water and the additives are added to the dry mixture, followed by low-speed stirring to obtain a slurry; The fiber is added to the slurry, and then the mixture is stirred at high speed until it is uniform and free of agglomerates to obtain a mixture. The mixture is then shaped and cured.
[0025] In some embodiments, the dry mixing time is 60–90 seconds.
[0026] In some embodiments, the low-speed stirring time is 90–120 s.
[0027] In some embodiments, the low-speed stirring speed is 50–100 r / min.
[0028] In some embodiments, the high-speed stirring speed is 200–500 r / min.
[0029] In some embodiments, the high-speed stirring time is 60–90 seconds.
[0030] In some embodiments, the molding method includes vibration molding.
[0031] In some embodiments, the curing conditions include: a temperature of 18–22°C, a relative humidity of over 95%, and a curing time of 28 days.
[0032] In some implementations, the curing process does not require autoclaving.
[0033] The third aspect of this application relates to the application of modified ultra-high performance concrete prepared by the method described in the first aspect of this application or the second aspect of this application in bridges, tunnels, prefabricated buildings or high-strength precast components.
[0034] The fourth aspect of this application provides an industrialized precast component, including the modified ultra-high performance concrete described in the first aspect of this application, or the modified ultra-high performance concrete prepared by the preparation method of the modified ultra-high performance concrete described in the second aspect of this application.
[0035] In some embodiments, the industrialized prefabricated components include at least one of bridges, tunnels, prefabricated buildings, and high-strength prefabricated components.
[0036] The modified ultra-high performance concrete described in this application can bring at least the following beneficial effects: 1) High content of solid waste: The content of fly ash ultrafine particles in the raw materials is ≥10wt%, which greatly reduces costs; 2) Excellent strength: 28-day compressive strength ≥120MPa; 3) Good workability: Freshly mixed concrete has a spread of ≥650mm, self-leveling, and is easy to construct; 4) Microsphere synergistic enhancement: In the raw materials, the spherical microspheres (i.e. fly ash graded microspheres) have a rolling ball effect that improves fluidity, while the micro-aggregate effect of ultrafine fly ash microspheres improves density and durability.
[0037] In addition to the beneficial effects of the modified ultra-high performance concrete described in this application, the modified ultra-high performance concrete described in this application can also bring at least the following beneficial effects: The process is simple, requires no autoclaving, and standard curing is sufficient to meet the requirements, making it suitable for engineering applications.
[0038] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0039] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the following description of the embodiments taken in conjunction with the accompanying drawings. in: Figure 1 This is a flowchart illustrating a method for preparing modified ultra-high performance concrete, which is an exemplary embodiment of this application. Detailed Implementation
[0040] The embodiments of this application are described in detail below, with examples of these embodiments illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application.
[0041] In this application, the disclosure of numerical ranges includes all values throughout the range and the disclosure of further subdivisions of the range, including the endpoints and subranges given for these ranges.
[0042] Unless otherwise specified, all raw materials and equipment involved in this application are self-made through commercial means or known methods; and all methods involved are conventional methods unless otherwise specified.
[0043] The inventors discovered the following shortcomings in the related technology: 1) Ordinary fly ash contains many impurities and has a wide particle size distribution, making it difficult to meet the stringent requirements of ultra-high performance concrete (UHPC) for workability and strength; 2) The lack of a dedicated gradation system limits the improvement in strength and durability; 3) The preparation process of ultra-high performance concrete (UHPC) is complex and costly, which is not conducive to large-scale promotion.
[0044] Based on the above findings, the inventors accidentally discovered that fly ash ultrafine particles with a particle size ≤10μm possess high sphericity, high strength, good activity, and excellent flowability, making them an ideal functional component for preparing ultra-high performance concrete (UHPC). Using fly ash ultrafine particles as the core component of UHPC raw materials and controlling their dosage within a specific range can improve compressive strength and workability while reducing the production cost of UHPC. Furthermore, when fly ash ultrafine particles are used together with graded fly ash microspheres in UHPC, they exhibit a synergistic microsphere enhancement effect—the spherical microspheres' rolling effect improves flowability, while the micro-aggregate effect enhances density and durability.
[0045] Modified Ultra-High Performance Concrete The modified ultra-high performance concrete of this application embodiment includes gel material, aggregate, admixture and fiber as raw materials; the gel material includes fly ash ultrafine particles, and the mass content of the fly ash ultrafine particles in the gel material is more than 10%.
[0046] This modified ultra-high performance concrete, due to the presence of more than 10 wt% fly ash ultrafine particles in its raw materials, can significantly reduce the production cost of ultra-high performance concrete while improving its compressive strength and workability.
[0047] Without limitation, the mass content of the fly ash ultrafine particles in the gel material includes, but is not limited to, more than 12%, more than 15%, more than 18%, or more than 20%, and may be selected as 10-20%.
[0048] In some embodiments, the Dv50 particle size of the fly ash ultrafine particles is less than 10 μm, including but not limited to less than 8 μm, less than 6 μm, or less than 4 μm.
[0049] In some embodiments, the gel material further includes graded microspheres of cement, silica fume, and fly ash.
[0050] In the embodiments of this application, the type of cement is not limited and can be any cement well known in the art, such as at least one of silicate cement (P·I), silicate cement (P·II), slag silicate cement (P·S).
[0051] As an optional example, the silica fume is grade 92 silica fume with a silica content of 92 wt% or more.
[0052] In some embodiments, the mass ratio of the cement, silica fume, fly ash ultrafine beads, and fly ash graded microbeads is (65-80):(8-15):(10-20):(5-10).
[0053] Controlling the mass ratio of cement, silica fume, fly ash ultrafine particles, and fly ash graded microspheres in the gel material within the above-mentioned range can give modified ultra-high performance concrete good plasticity and high strength; exceeding the above range will reduce plasticity. For example, if the content of fly ash ultrafine particles is too low, the strength will decrease.
[0054] From the above mass ratio of cement, silica fume, fly ash ultrafine beads, and fly ash graded microspheres, it can be understood that: The gel material comprises, by weight, 65-80 parts of cement, 8-15 parts of silica fume, 10-20 parts of fly ash ultrafine beads, and 5-10 parts of fly ash graded microbeads.
[0055] Non-limiting, by weight, the content of cement in the gel material includes, but is not limited to, 67.5 parts, 70 parts, 72.5 parts, 75 parts or 77.5 parts, the content of silica fume includes, but is not limited to, 10 parts, 12 parts or 14 parts, the content of fly ash ultrafine beads includes, but is not limited to, 12 parts, 14 parts, 16 parts or 18 parts, and the content of fly ash graded microspheres includes, but is not limited to, 6.5 parts or 8 parts.
[0056] It is understood that the ratio of any content of the above-mentioned cement, silica fume, fly ash ultrafine beads, and fly ash graded beads is the mass ratio of cement, silica fume, fly ash ultrafine beads, and fly ash graded beads. For example, by mass parts, when the content of cement in the gel material is 72 parts, the content of silica fume is 12 parts, the content of fly ash ultrafine beads is 15 parts, and the content of fly ash graded beads is 7.5 parts, the mass ratio of cement, silica fume, fly ash ultrafine beads, and fly ash graded beads is 72:12:15:7.5, etc.
[0057] As an alternative example, the composition of the gel material, by weight, is: cement: 65-80 parts, silica fume: 8-15 parts, fly ash ultrafine beads: 10-20 parts, and fly ash graded microbeads: 5-10 parts.
[0058] In some embodiments, the Dv50 particle size of the fly ash grading microspheres is greater than 10 μm and less than 20 μm, including but not limited to 12 μm, 15 μm or 18 μm.
[0059] In some embodiments, the aggregate comprises continuously graded quartz sand and / or continuously graded fine aggregate.
[0060] In the embodiments of this application, there are no restrictions on the specific selection of continuously graded quartz sand and continuously graded fine aggregate.
[0061] In some embodiments, the admixture includes, but is not limited to, a water-reducing agent, which may be selected as a water-reducing agent.
[0062] In some embodiments, the water-reducing agent includes, but is not limited to, polycarboxylate water-reducing agents, and may be selected as polycarboxylate water-reducing agents.
[0063] In some embodiments, the solid content of the water-reducing agent is 1.5% to 2.5%, including but not limited to 1.8%, 2%, or 2.3%.
[0064] In some embodiments, the fiber includes steel fiber, which may be selected as steel fiber.
[0065] In the embodiments of this application, the specific type of steel fiber is not limited. Without limitation, the steel fiber includes, but is not limited to, at least one of ordinary carbon steel fiber, stainless steel fiber, galvanized steel fiber, and end-hooked low-carbon steel fiber.
[0066] In some embodiments, the volume fraction of the steel fibers is 1.5 to 2.5%, including but not limited to 1.8%, 2% or 2.3%.
[0067] In some embodiments, the mass ratio of the gel material, aggregate, additives and fiber is (88-125):(110-130):(1.5-3.0):(1.5-3.0).
[0068] Based on the above mass ratio of gelling material, aggregate, admixture, and fiber, it can be understood that: The modified ultra-high performance concrete comprises, by weight, 88-125 parts of gel material, 110-130 parts of aggregate, 1.5-3.0 parts of fiber, and 1.5-3.0 parts of water-reducing agent.
[0069] Non-limiting, by weight, the modified ultra-high performance concrete raw material may contain, but is not limited to, 95 parts, 100 parts, 105 parts, 110 parts, 115 parts or 120 parts of gel material, 115 parts, 120 parts or 125 parts of solid material, 1.8 parts, 2.1 parts, 2.4 parts or 2.7 parts of fiber, and 1.8 parts, 2.1 parts, 2.4 parts or 2.7 parts of water-reducing agent.
[0070] It is understood that the ratio of any content of the above-mentioned gel material, aggregate, admixture and fiber is the mass ratio of gel material, aggregate, admixture and fiber. For example, by mass parts, when the content of gel material in the modified ultra-high performance concrete is 110 parts, the content of solid material is 120 parts, the content of fiber is 2.2 parts, and the content of water-reducing agent is 2.1 parts, the mass ratio of gel material, aggregate, admixture and fiber is 110:120:2.2:2.1, etc.
[0071] In some embodiments, the modified ultra-high performance concrete further includes water, and the mass ratio of the water to the gel material (i.e., the water-cement ratio) is 0.16 to 0.20, for example 0.18, and optionally 0.17 to 0.19.
[0072] In the embodiments of this application, the type of water is not limited; it can be tap water, deionized water, etc., and tap water is optional.
[0073] In some embodiments, the modified ultra-high performance concrete has a 28-day compressive strength of over 120 MPa and a spread of over 650 mm.
[0074] As an optional example, the modified ultra-high performance concrete has a 28-day compressive strength of 120–300 MPa (e.g., 180 MPa or 250 MPa, etc.) and a spread of 650–1000 mm (e.g., 750 mm or 850 mm, etc.).
[0075] <Preparation Method of Modified Ultra-High Performance Concrete> The method for preparing modified ultra-high performance concrete according to the embodiments of this application can be used to prepare the modified ultra-high performance concrete according to the embodiments of this application.
[0076] The following describes a method for preparing modified ultra-high performance concrete according to an embodiment of this application, with reference to the accompanying drawings.
[0077] Figure 1 This is a flowchart illustrating a method for preparing modified ultra-high performance concrete, which is an exemplary embodiment of this application.
[0078] like Figure 1 As shown, the preparation method of this modified ultra-high performance concrete includes the following steps: S101. The gel material and the aggregate are dry-mixed to obtain a dry-mixed material.
[0079] In some embodiments, the method for preparing modified ultra-high performance concrete further includes a step of preparing all raw materials before step S101. For example, weighing the formula amounts of gelling materials (cement, silica fume, two-stage fly ash microspheres—ultrafine fly ash microspheres, graded fly ash microspheres), aggregates, fibers, and water, etc.
[0080] In some embodiments, the dry mixing time is 60 to 90 seconds, including but not limited to 70 seconds or 80 seconds.
[0081] S102. Water and the additive (e.g., water-reducing agent) are added to the dry mixture obtained in step S101, and then the mixture is stirred at low speed to obtain a slurry.
[0082] In some embodiments, the low-speed stirring time is 90 to 120 seconds, including but not limited to 100 seconds or 110 seconds.
[0083] In some embodiments, the low-speed stirring speed is 50 to 100 r / min, including but not limited to 60 r / min, 75 r / min or 85 r / min.
[0084] S103. Add the fiber (e.g., steel fiber) to the slurry obtained in step S102, and then stir at high speed until it is uniform and free of agglomeration to obtain a mixture.
[0085] In some embodiments, the high-speed stirring speed is 200 to 500 r / min, including but not limited to 300 r / min, 370 r / min or 450 r / min.
[0086] In some embodiments, the high-speed stirring time is 60 to 90 seconds, including but not limited to 70 seconds or 80 seconds.
[0087] S104. The mixture described in step S103 is molded and cured.
[0088] In some embodiments, the molding method includes vibration molding.
[0089] In some embodiments, the curing conditions include a temperature of 18–22°C, a relative humidity (RH) of 95% or higher, and a curing time of 28 days.
[0090] It is understood that the above maintenance is standard maintenance, and the temperature is not limited to 19℃ or 20℃, and the relative humidity (RH) is not limited to 96% or 98%.
[0091] In some implementations, the curing process does not require autoclaving. This simplifies the procedure.
[0092] In some embodiments, the method for preparing the modified ultra-high performance concrete further includes a demolding step between the molding and the curing.
[0093] As an optional example, the demolding time is 24-72 hours, such as 36 hours or 48 hours, and optionally 24 hours.
[0094] The modified ultra-high performance concrete of this application embodiment, or the modified ultra-high performance concrete prepared by the preparation method of the modified ultra-high performance concrete of this application embodiment, can be widely used in bridges, tunnels, prefabricated buildings or high-strength precast components.
[0095] The industrial prefabricated components of this application include the modified ultra-high performance concrete of this application, or the modified ultra-high performance concrete prepared by the preparation method of the modified ultra-high performance concrete of this application.
[0096] In some embodiments, the industrialized prefabricated components include, but are not limited to, at least one of bridges, tunnels, prefabricated buildings, and high-strength prefabricated components.
[0097] The following non-limiting embodiments further illustrate certain features of the present technology.
[0098] The performance testing methods are all national standard methods, specifically: The test method for spreadability is as follows: referring to GB / T 2419-2005 "Method for Determination of Flowability of Cement Mortar", the spreadability of freshly mixed UHPC slurry (the slurry obtained by wet mixing in step (2) of the following examples or comparative examples) is tested by using the table jumping method, and the average value of the diameters in two vertical directions is taken as the test result.
[0099] The test method for 28-day compressive strength is as follows: referring to GB / T 31387-2015 "Reactive Powder Concrete", prepare 100mm×100mm×100mm cube specimens, cure under standard conditions for 28 days, and test them using a pressure testing machine with a loading rate of 1.0MPa / s. Take the average value of 6 specimens as the test result.
[0100] The density test method is as follows: referring to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete", the apparent density method is used to test the bulk density of hardened concrete, and the mercury intrusion porosimetry method is used simultaneously to test the porosity and pore size distribution of the paste. The durability test method is as follows: referring to GB / T 50082-2009 "Standard for Test Methods of Long-Term Performance and Durability of Ordinary Concrete", the RCM method is used to test the chloride ion migration coefficient; the rapid freezing method is used to test the frost resistance grade; and the water penetration height method is used to test the permeability grade.
[0101] Example 1 (Modified Ultra-High Performance Concrete) The modified ultra-high performance concrete of this embodiment, by weight, comprises the following raw materials: 103 parts gel material, 120 parts aggregate, 2.0 parts fiber, 2.2 parts admixture, and the remainder is water.
[0102] in: The gel material, by weight, consists of: 72 parts cement, 10 parts silica fume, 15 parts fly ash ultrafine particles, and 6 parts fly ash graded microspheres. The cement is silicate cement (P·I), and the silica fume is grade 92 silica fume. The median volumetric particle size (Dv50) of the fly ash ultrafine particles is 6.2 μm, and the maximum particle size is ≤10 μm. The median volumetric particle size (Dv50) of the fly ash graded microspheres is 14.5 μm, and the maximum particle size is ≤20 μm.
[0103] The aggregate is continuously graded fine quartz sand, specifically: 60wt% of 0.15-0.6mm fine quartz sand and 40wt% of 0.6-1.25mm medium quartz sand, with continuous gradation and rounded particle shape.
[0104] The fiber is a hook-shaped low-carbon steel fiber with a volume fraction of 2%, a diameter of 0.20 mm, a length of 13 mm, and a tensile strength of ≥2850 MPa.
[0105] The admixture is a polycarboxylate-based high-performance water-reducing agent with a solid content of 2% and a water reduction rate of ≥42%. It is a standard type of retarded coagulation carboxylate water-reducing agent. The water used is tap water, and the mass ratio of water to gel material (i.e., the water-gel ratio) is 0.18.
[0106] (Preparation method of modified ultra-high performance concrete) The method for preparing modified ultra-high performance concrete in this embodiment includes the following steps: (1) Dry mixing: Put the concrete materials and aggregates of the formula into the mixer and dry mix at a speed of 120r / min for 80s to obtain dry mix.
[0107] (2) Wet mixing: Add water and additives to the dry mixture obtained in step (1), and stir at a low speed of 100r / min for 100s to obtain slurry.
[0108] (3) Fiber dispersion: Fiber is added to the slurry obtained in step (2), and the mixture is stirred at a high speed of 300 r / min for 70 s to obtain a mixture.
[0109] (4) Molding and curing Vibration molding: compact molding using a vibration table; Standard curing: Demold after 24 hours, and cure under standard conditions (20±2℃, RH≥95%) for 28 days.
[0110] The modified ultra-high performance concrete tested showed a spread of 680 mm, a 28-day compressive strength of 128 MPa, an apparent density of 2780 kg / m³, and a hardened paste porosity ≤2.1%. Its durability index, chloride ion migration coefficient (RCM method), was 0.62 × 10⁻⁶. - ¹² m² / s, freeze-thaw resistance grade reaches F1200, dynamic elastic modulus loss rate ≤6%, mass loss rate ≤0.8%, impermeability grade > P20.
[0111] Example 2 This embodiment is basically the same as embodiment 1, except that: The composition of the gel material by weight is as follows: 76.7 parts cement, 10 parts silica fume, 10.3 parts fly ash ultrafine beads, and 6 parts fly ash graded microbeads.
[0112] Example 3 This embodiment is basically the same as embodiment 1, except that: By weight, the composition of the gel material is as follows: 66.4 parts cement, 10 parts silica fume, 20.6 parts fly ash ultrafine beads, and 6 parts fly ash graded microbeads.
[0113] Example 4 This embodiment is basically the same as embodiment 1, except that: The composition of the gel material by weight is: 60 parts cement, 8 parts silica fume, 30 parts fly ash ultrafine beads, and 5 parts fly ash graded microbeads.
[0114] Example 5 This embodiment is basically the same as embodiment 1, except that: The volume fraction of the fiber (i.e., stainless steel fiber) is 1.5%, the solid content of the polycarboxylate superplasticizer is 2%, and the mass ratio of water to gel material (i.e., water-gel ratio) is 0.16.
[0115] Example 6 This embodiment is basically the same as embodiment 1, except that: The volume fraction of the fiber (i.e., stainless steel fiber) is 2.5%, the solid content of the polycarboxylate superplasticizer is 1.5%, and the mass ratio of water to gel material (i.e., water-gel ratio) is 0.20.
[0116] Comparative Example 1 This comparative example is basically the same as Example 1, except that: The gel material does not contain fly ash ultrafine beads or fly ash graded microbeads.
[0117] Tests showed that the prepared modified ultra-high performance concrete had a spread of 560 mm, a 28-day compressive strength of 108 MPa, and poor fluidity.
[0118] In this application, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0119] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A modified ultra-high performance concrete, characterized in that, The raw materials for the modified ultra-high performance concrete include gel materials, aggregates, admixtures, and fibers; the gel materials include fly ash ultrafine particles, and the mass content of the fly ash ultrafine particles in the gel materials is more than 10%.
2. The modified ultra-high performance concrete according to claim 1, characterized in that, The fly ash ultrafine particles in the gel material have a mass content of 10-20%; And / or, the Dv50 particle size of the fly ash ultrafine particles is less than 10 μm.
3. The modified ultra-high performance concrete according to claim 1, characterized in that, The gel material also includes graded microspheres of cement, silica fume, and fly ash; And / or, the aggregate comprises continuously graded quartz sand and / or continuously graded fine aggregate; And / or, the admixture includes a water-reducing agent; And / or, the fibers include steel fibers.
4. The modified ultra-high performance concrete according to claim 3, characterized in that, The mass ratio of the cement, silica fume, fly ash ultrafine beads, and fly ash graded microspheres is (65-80):(8-15):(10-20):(5-10). And / or, the Dv50 particle size of the fly ash grading microspheres is greater than 10 μm and less than 20 μm; And / or, the water-reducing agent includes a polycarboxylate water-reducing agent; And / or, the solid content of the water-reducing agent is 1.5% to 2.5%; And / or, the volume fraction of the steel fibers is 1.5 to 2.5%.
5. The modified ultra-high performance concrete according to claim 1, characterized in that, The mass ratio of the gel material, aggregate, additives, and fiber is (88-125):(110-130):(1.5-3.0):(1.5-3.0). And / or, the modified ultra-high performance concrete further includes water, and the mass ratio of the water to the gel material is 0.16 to 0.20, optionally 0.17 to 0.
19.
6. The modified ultra-high performance concrete according to any one of claims 1 to 5, characterized in that, The modified ultra-high performance concrete has a 28-day compressive strength of over 120 MPa and a spread of over 650 mm.
7. A method for preparing modified ultra-high performance concrete as described in any one of claims 1 to 6, characterized in that, include: The gel material and the aggregate are dry-mixed to obtain a dry-mixed material. Water and the additives are added to the dry mixture, followed by low-speed stirring to obtain a slurry; The fiber is added to the slurry, and then the mixture is stirred at high speed until it is uniform and free of agglomerates to obtain a mixture. The mixture is then shaped and cured.
8. The preparation method according to claim 7, characterized in that, The dry mixing time is 60–90 seconds; And / or, the low-speed stirring time is 90–120 s; And / or, the low-speed stirring speed is 50-100 r / min; And / or, the speed of the high-speed stirring is 200-500 r / min; And / or, the high-speed stirring time is 60–90 s; And / or, the molding method includes vibration molding; And / or, the conditions for maintenance include: a temperature of 18–22°C, a relative humidity of 95% or higher, and a maintenance time of 28 days; And / or, the curing process does not require autoclaving.
9. The application of the modified ultra-high performance concrete as described in any one of claims 1 to 5 or the modified ultra-high performance concrete prepared by the preparation method as described in any one of claims 6 to 8 in bridges, tunnels, prefabricated buildings or high-strength precast components.
10. An industrially manufactured prefabricated component, characterized in that, It includes the modified ultra-high performance concrete as described in any one of claims 1 to 5, or the modified ultra-high performance concrete prepared by the preparation method as described in any one of claims 6 to 8; Optionally, the industrialized prefabricated components include at least one of bridges, tunnels, prefabricated buildings, and high-strength prefabricated components.