A low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste and its preparation method

By introducing an internal curing component and a micro-expansion regulating component into sulfate-activated solid waste cementitious materials, the problem of large shrinkage and easy cracking of the material is solved, and the strength is improved and the carbon emissions are reduced. It is suitable for precast components, large-volume concrete and other projects.

CN123106142APending Publication Date: 2026-11-17GUIZHOU CSCEC SHUANGYUAN BUILDING MATERIALS CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611412645.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sulfate-activated solid waste cementitious materials suffer from large shrinkage and easy cracking in application, and existing control methods are difficult to effectively coordinate, which limits their promotion in projects with high volume stability requirements.

Method used

The combination of internal curing components and micro-expansion regulating components is adopted. The internal curing components are a composite of pre-wetted porous regenerated fine powder or superabsorbent resin and silica-alumina powder. The micro-expansion regulating components are calcium aluminate, calcium sulfoaluminate clinker powder or nano γ-Al2O3. The synergistic effect reduces shrinkage and improves crack resistance.

Benefits of technology

It significantly reduces the autogenous shrinkage and drying shrinkage of cementitious materials, prolongs the cracking time, and improves the strength and durability of hardened slurry. At the same time, it achieves efficient utilization of industrial solid waste and reduces carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106142A_ABST
    Figure CN123106142A_ABST
Patent Text Reader

Abstract

This invention discloses a low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste and its preparation method, relating to the field of cementitious material technology. Based on the total mass of the cementitious material, it comprises the following components: 25%–40% steel slag powder; 40%–60% blast furnace slag powder; 8%–15% desulfurized gypsum; 2%–6% composite sulfate activator; 1%–5% internal curing component; 0.5%–3% micro-expansion regulating component; and the balance being silicate cement clinker powder or no silicate cement clinker powder. The internal curing component is a pre-wetted porous recycled fine powder or a composite of highly absorbent resin and aluminosilicate powder. This invention simultaneously introduces an internal curing component and a micro-expansion regulating component into the sulfate-activated all solid waste system. These two components function and cooperate at different stages of shrinkage development. Later water release promotes continued hydration of blast furnace slag and steel slag, stabilizing micro-strain and reducing the likelihood of excessive expansion or shrinkage rebound in the later stages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cementitious materials technology, and in particular to a low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste and its preparation method. Background Technology

[0002] All-solid-waste cementitious materials, prepared by sulfate activation using industrial solid wastes such as steel slag, ore slag, and desulfurized gypsum as main raw materials, have become a research hotspot and development direction in the field of building materials because they can replace cement clinker in a large proportion, dispose of industrial solid waste, and significantly reduce carbon emissions.

[0003] However, this type of material has the following main problems in practical applications: (1) Steel slag-slag-desulfurized gypsum-based cementitious materials have large shrinkage and are prone to cracking. Studies have shown that the autogenous shrinkage and drying shrinkage of this type of material are usually 20% to 40% higher than those of ordinary Portland cement. In precast components and large-volume concrete projects with high requirements for volume stability, the risk of cracking is prominent, which seriously restricts its engineering promotion.

[0004] (2) The causes of shrinkage are complex, and a single method is insufficient for effective control. The main reasons for the excessive shrinkage in this type of system include: firstly, the rapid hydration of the system consumes water quickly, resulting in a rapid decrease in internal relative humidity and significant self-drying shrinkage; secondly, the formation time of ettringite (AFt) in the hydration products is not synchronized with the shrinkage development, and the early chemical shrinkage lacks effective compensation; thirdly, the hardened slurry has a fine capillary structure, and the capillary tension contributes significantly to the shrinkage. The intertwining of multiple shrinkage mechanisms means that shrinkage control must be implemented in a coordinated manner targeting different stages and different causes.

[0005] (3) Existing expansion agent compensation methods are not suitable for this system. Adding expansion agents (such as MgO, gypsum, calcium sulfoaluminate, etc.) to compensate for shrinkage by generating expansion products is a common method to reduce the shrinkage of cementitious materials. However, in sulfate-activated solid waste systems, the use of expansion agents alone often faces the problem of the timing of expansion and the development of shrinkage being out of sync: if expansion occurs too early, it will be consumed in the plastic stage; if it occurs too late, the high-incidence period of shrinkage will be missed, and it may even cause hidden dangers to the volume stability in the later stage.

[0006] (4) Existing internal curing methods have limited compensatory capacity in this system. Adding internal curing agents (such as superabsorbent resins, lightweight aggregates, etc.) to maintain internal humidity by releasing moisture is another commonly used method for shrinkage control. However, the liquid absorption capacity of ordinary superabsorbent resins is greatly reduced in the high ion concentration environment of cement pore liquid, making it difficult to stably play the role of internal curing; moreover, internal curing can only inhibit self-drying shrinkage and lacks the ability to compensate for chemical shrinkage and temperature drop shrinkage, and the shrinkage improvement is limited when used alone.

[0007] Therefore, developing a low-shrinkage sulfate-activated low-carbon cementitious material for solid waste with a synergistic effect of internal curing and micro-expansion mechanisms, which can significantly reduce shrinkage and improve crack resistance while maintaining strength and workability, is of great engineering significance. Summary of the Invention

[0008] The purpose of this invention is to provide a low-shrinkage sulfate-activated low-carbon cementitious material for solid waste and its preparation method, so as to solve the problems mentioned in the background art.

[0009] To achieve the above objectives, the present invention provides the following technical solution: a low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste, comprising the following components by total mass of the cementitious material: Steel slag powder 25%–40%; Slag powder 40%–60%; Desulfurized gypsum 8%–15%; Compound sulfate activator 2%–6%; Internal maintenance components: 1%–5%; Micro-expansion regulating components: 0.5%–3%; The remainder is silicate cement clinker powder or no silicate cement clinker powder is provided; The internal curing component is a composite of pre-wetted porous recycled fine powder or superabsorbent resin and silica-alumina powder. The internal curing component has an absorption ratio of 5-15 g / g in simulated cement pore liquid. The simulated cement pore liquid is a saturated calcium hydroxide solution at 25°C. The micro-expansion regulating component is at least one of calcium aluminate, calcium sulfoaluminate clinker powder, nano γ-Al2O3, or nano Al(OH)3.

[0010] Preferably, the porous recycled fine powder is recycled waste concrete fine powder or waste clay brick fine powder, with a specific surface area of ​​500-800 m². 2 / kg; the pre-wetting treatment method is as follows: spray water onto the porous regenerated fine powder and stir until the moisture content is 15% to 25%, then seal and age for 24 to 48 hours.

[0011] Preferably, the composite of the superabsorbent resin and the aluminosilicate powder comprises, by weight, 5-15 parts of sodium polyacrylate or polyacrylamide superabsorbent resin, 30-50 parts of activated metakaolin, and 10-20 parts of nano silica, prepared by dry mixing and granulation, with a particle size of 50-200 μm.

[0012] Preferably, the micro-expansion regulating component is calcium sulfoaluminate clinker powder or nano-γ-Al2O3 with a specific surface area of ​​400-700 m². 2 / kg.

[0013] Preferably, the composite sulfate activator comprises, by weight, 40-70 parts of anhydrous gypsum or hemihydrate gypsum, 10-30 parts of sodium sulfate, 5-15 parts of water glass, 1-5 parts of triethanolamine, and 2-8 parts of sodium aluminate.

[0014] Preferably, the specific surface area of ​​the steel slag powder is 450–650 m². 2 / kg, free CaO content ≤3.5%, free MgO content ≤3.0%; the specific surface area of ​​the slag powder is 400-550m². 2 / kg; the specific surface area of ​​the desulfurized gypsum is 350-500 m² / kg. 2 / kg.

[0015] Preferably, based on the total mass of the cementitious material, the internal curing component is 2% to 3.5%, and the micro-expansion regulating component is 1% to 2%.

[0016] Preferably, the mass ratio of the internal maintenance component to the micro-expansion regulation component is 1.67:1 to 2:1.

[0017] Preferably, the 28-day autogenous shrinkage of the cementitious material, as measured according to the method specified in GB / T50082, is ≤120×10⁻⁶. -6 90-day drying shrinkage ≤280×10 -6 .

[0018] A method for preparing a low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste includes the following steps: S1: Dry and grind steel slag, mineral slag, and desulfurized gypsum to the target specific surface area to obtain steel slag powder, mineral slag powder, and desulfurized gypsum powder; S2: Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; S3: Pre-wet or granulation pre-treatment is performed on the internal curing component to obtain the pre-wetted internal curing component; S4: Add the steel slag powder, blast furnace slag powder, desulfurized gypsum powder obtained in step S1, the composite sulfate activator obtained in step S2, the micro-expansion regulating component, and optional silicate cement clinker powder into a mixer, and mix under low shear for 5 to 25 minutes; then add the pre-wet internal curing component obtained in step S3, and continue to mix under low shear for 5 minutes, and discharge the material to obtain the low-shrinkage sulfate-activated all-solid waste low-carbon cementitious material. The mixer is a plow-type mixer or a double ribbon mixer, and the total mixing time in step S4 is 10 to 30 minutes.

[0019] The technical effects and advantages of this invention are as follows: (1) This invention introduces both an internal curing component and a micro-expansion regulating component into a sulfate-activated solid waste system. The two components play different roles and cooperate with each other at different stages of shrinkage development: In the early stage of molding, the pre-wetting moisture of the internal curing component inhibits early self-drying; during the high-incidence period of shrinkage (1-7 days), the micro-expansion regulating component generates ettringite under sulfate activation, producing 100-300×10 -6 The stable micro-expansion compensates for chemical shrinkage and temperature-induced shrinkage, while the internal curing components release water simultaneously to maintain hydration. Later water release promotes continued hydration of slag and steel slag, stabilizing micro-strain and reducing the likelihood of excessive expansion or shrinkage rebound in the later stages. Compared to cementitious materials with the same proportions but without internal curing components and micro-expansion regulating components, the cementitious material of this invention exhibits a 30%–47% reduction in autogenous shrinkage, a 25%–35% reduction in drying shrinkage, and a significantly prolonged time for ring-constrained cracking. (2) The internal curing component and the micro-expansion regulating component of the present invention have a positive synergistic effect when properly proportioned, rather than a simple superposition of their individual effects. Experiments show that the self-shrinkage of the cementitious material containing only the internal curing component is 118×10⁻⁶ after 28 days. -6 The value of only the micro-expansion regulating component is 146×10. -6 However, when the two are combined in an appropriate ratio, the concentration can be reduced to 98×10. -6 the following; (3) The present invention reduces shrinkage while increasing strength. The water released by the internal curing component provides additional water for the later hydration of slag and steel slag. The active aluminum phase in the micro-expansion control component participates in hydration to generate more CSH gel and ettringite. The needle-shaped ettringite crystals and flocculent CSH gel are evenly interwoven in the hardened slurry, with small pores and dense structure. The 28-day compressive strength of the cementitious material of the present invention is more than 5% higher than that of the unmodified system. (4) The internal curing component of the present invention has a stable liquid absorption ratio of 5-15 g / g and delayed water release behavior in simulated cement pore liquid. After pre-wetting treatment or composite modification, it will not excessively absorb mixing water and has good compatibility with polycarboxylate superplasticizer. The initial slump of fresh concrete prepared with the cementitious material of the present invention can reach more than 200 mm, and the loss after 1 hour is no more than 30 mm; the reduction in shrinkage and the reduction of cracks caused by structural densification simultaneously improve the durability properties of concrete such as impermeability and chloride ion penetration resistance. The electrical flux of the prepared C40 concrete is as low as 625C after 56 days. (5) The total amount of steel slag, blast furnace slag and desulfurized gypsum, three major industrial solid wastes, in the cementitious material of this invention can reach more than 90%. The internal curing components can also be made from construction solid wastes such as recycled fine powder from waste concrete, resulting in a high utilization rate of all solid wastes. The carbon emissions per cubic meter of concrete are reduced by more than 40% compared with ordinary silicate cement concrete. While disposing of industrial solid waste, it significantly reduces the carbon emissions of building materials and can be widely used in engineering fields with high requirements for volume stability, such as precast components, large-volume concrete, water conservancy projects, and road bridges. Attached Figure Description

[0020] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention, but do not constitute a limitation thereof. In the drawings: Figure 1 This is a comparison diagram of the shrinkage of the cementitious material of this invention and ordinary all-solid waste cementitious material; Figure 2 This is a water absorption-release curve of the internal maintenance component of the present invention; Figure 3 This is a diagram showing the expansion strain evolution of the micro-expansion controlled component of the present invention; Figure 4 This is a SEM microstructure image of the 28-day hydration product of the cementitious material of the present invention. Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] This invention provides, for example Figures 1-4 This paper presents a low-shrinkage sulfate-activated low-carbon cementitious material for solid waste and its preparation method.

[0023] In the following examples and comparative examples, the percentage of components is calculated based on the sum of the masses of each component of the cementitious material in that example or comparative example (i.e., the total mass of the cementitious material).

[0024] The following detailed description, with reference to specific embodiments, of low-shrinkage sulfate-activated low-carbon cementitious materials for all solid waste and their preparation methods.

[0025] I. Terminology Definitions and Testing Methods In this invention, the simulated cement pore liquid is a saturated calcium hydroxide solution at 25°C. The preparation method is as follows: add excess analytical grade calcium hydroxide to deionized water, let it stand at 25°C for more than 24 hours, and take the supernatant as the saturated calcium hydroxide solution.

[0026] The liquid absorption ratio is determined as follows: Weigh out a dry inner curing component with a mass of m0 (accurate to 0.01g), put it into a non-woven bag, completely immerse it in the simulated cement pore liquid, and let it stand at 25℃ until liquid absorption equilibrium is reached; take out the non-woven bag, suspend it to drain until no liquid drips, weigh the total mass, subtract the mass of the non-woven bag and record it as m1, then the liquid absorption ratio = (m1 - m0) / m0, unit g / g.

[0027] Determination of water release rate: The liquid-saturated internal curing component was placed in an environment simulating the temperature rise-fall process of large-volume concrete (heated to 60℃ and then naturally cooled to room temperature), and the mass percentage of water released within 48 hours after the cooling was completed was measured relative to the amount of liquid absorbed.

[0028] The compressive strength was determined according to GB / T17671 "Test Method for Strength of Cement Mortar (ISO Method)".

[0029] Autogenous shrinkage and drying shrinkage were determined according to the shrinkage test method specified in GB / T50082 "Standard for Test Methods of Long-Term Performance and Durability of Ordinary Concrete". The specimens were cementitious paste specimens. The autogenous shrinkage specimens were sealed after molding and the initial setting time was used as the measurement reference. The drying shrinkage specimens were moved into an environment with a temperature of (20±2)℃ and a relative humidity of (60±5)% after standard curing for 3 days.

[0030] The circular confinement cracking test was conducted according to the conventional method for the circular confinement test of concrete in this field: freshly mixed grout was poured into the annular space between the inner steel ring and the mold sleeve, and after molding, the surface was exposed and placed in a dry environment. The time from pouring to the appearance of the first visible crack in the circumferential specimen was recorded.

[0031] The 56-day electrical flux was determined according to the electrical flux method specified in GB / T50082.

[0032] II. Specifications and Models of Raw Materials in Each Example Steel slag powder: specific surface area 450-650 m² 2 / kg, free CaO content ≤3.5%, free MgO content ≤3.0%; in the examples, a specific surface area of ​​560m² was used. 2 / kg of steel slag powder.

[0033] Slag powder: specific surface area 400-550m² 2 / kg, and other technical indicators comply with the requirements of GB / T18046 "Granulated Blast Furnace Slag Powder for Cement, Mortar and Concrete"; the specific surface area used in the example is 500m². 2 / kg of slag powder.

[0034] Desulfurization gypsum: a byproduct of flue gas desulfurization in coal-fired power plants, with a specific surface area of ​​350–500 m². 2 / kg; In the examples, a specific surface area of ​​420m² was used. 2 / kg of desulfurized gypsum powder.

[0035] Composite sulfate activator: By weight, it comprises 40-70 parts anhydrous gypsum or hemihydrate gypsum, 10-30 parts sodium sulfate, 5-15 parts water glass, 1-5 parts triethanolamine, and 2-8 parts sodium aluminate; the components are mixed in proportion and co-ground to a specific surface area of ​​200-350 m². 2 / kg available.

[0036] Porous recycled fine powder: In this example, recycled fine powder from waste concrete with a specific surface area of ​​650 m² was used. 2 / kg.

[0037] Micro-expansion regulating components: Examples 1 and 3 used calcium sulfoaluminate clinker powder with a specific surface area of ​​550 m². 2 / kg; Example 2 uses nano-γ-Al2O3 with a specific surface area of ​​400-700 m². 2 Within the range of / kg.

[0038] Superabsorbent polymers: Sodium polyacrylate or polyacrylamide superabsorbent polymers; active metakaolin and nano silica are commercially available industrial-grade products.

[0039] III. Examples and Comparative Examples Example 1: A low-shrinkage sulfate-activated low-carbon cementitious material for solid waste, composed of the following components: 300g (28.8%) steel slag powder, 550g (52.9%) blast furnace slag powder, 120g (11.5%) desulfurized gypsum powder, 30g (2.9%) composite sulfate activator, 25g (2.4%) pre-wetted recycled fine powder, and 15g (1.4%) calcium sulfoaluminate clinker powder. The total mass of the cementitious material is 1040g, without silicate cement clinker powder.

[0040] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) Pre-wetting treatment of internal curing components: take a specific surface area of ​​650m² 2 / kg of waste concrete recycled fine powder was sprayed with water and stirred until the moisture content was 20%, then sealed and aged for 36 hours to obtain pre-wetted recycled fine powder; (4) Add the steel slag powder, slag powder, desulfurized gypsum powder obtained in step (1), the composite sulfate activator obtained in step (2), and calcium sulfoaluminate clinker powder into a twin-screw mixer at a speed of 45 rpm. Mix under low shear for 15 min. Then add the pre-wetted recycled fine powder obtained in step (3) and continue mixing under low shear for 5 min. Discharge the material to obtain a low-shrinkage sulfate-activated all-solid waste low-carbon cementitious material. The total mixing time in step (4) is 20 min.

[0041] Example 2: A low-shrinkage sulfate-activated low-carbon cementitious material for solid waste, composed of the following components: 300g (29.1%) steel slag powder, 550g (53.4%) blast furnace slag powder, 120g (11.7%) desulfurized gypsum powder, 30g (2.9%) composite sulfate activator, 20g (1.9%) composite of superabsorbent resin and silica-alumina powder, and 10g (1.0%) nano-γ-Al2O3. The total mass of the cementitious material is 1030g, without silicate cement clinker powder.

[0042] The composite of superabsorbent resin and aluminosilicate powder is prepared by dry mixing and granulation of 8 parts by weight of sodium polyacrylate superabsorbent resin, 45 parts by weight of active metakaolin, and 15 parts by weight of nano silica, with a particle size of 50-200 μm.

[0043] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) Preparation of internal curing components: Take sodium polyacrylate superabsorbent resin, active metakaolin and nano silica according to the above mass parts, and dry mix and granulate to obtain a composite of superabsorbent resin and silica-alumina powder with a particle size of 50-200 μm. (4) The steel slag powder, slag powder, desulfurized gypsum powder obtained in step (1), the composite sulfate activator obtained in step (2), and nano-γ-Al2O3 are added into a twin-ribbon mixer at a speed of 45 rpm. The mixture is first mixed under low shear for 15 min. Then, the composite of the superabsorbent resin and silica-alumina powder obtained in step (3) is added, and the mixture is mixed under low shear for another 5 min. The material is then discharged to obtain a low-shrinkage sulfate-activated all-solid waste low-carbon cementitious material. The total mixing time in step (4) is 20 min.

[0044] In this embodiment, the mass ratio of the internal maintenance component to the micro-expansion regulation component is 2:1.

[0045] Example 3: A low-shrinkage sulfate-activated low-carbon cementitious material for solid waste, composed of the following components: 300g (28.4%) steel slag powder, 550g (52.1%) blast furnace slag powder, 120g (11.4%) desulfurized gypsum powder, 30g (2.8%) composite sulfate activator, 35g (3.3%) pre-wetted recycled fine powder, and 20g (1.9%) calcium sulfoaluminate clinker powder. The total mass of the cementitious material is 1055g, without silicate cement clinker powder.

[0046] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) Pre-wetting treatment of internal curing components: take a specific surface area of ​​650m² 2 / kg of waste concrete recycled fine powder was sprayed with water and stirred until the moisture content was 20%, then sealed and aged for 36 hours to obtain pre-wetted recycled fine powder; (4) Add the steel slag powder, slag powder, desulfurized gypsum powder obtained in step (1), the composite sulfate activator obtained in step (2), and calcium sulfoaluminate clinker powder into a twin-screw mixer at a speed of 45 rpm. Mix under low shear for 15 min. Then add the pre-wetted recycled fine powder obtained in step (3) and continue mixing under low shear for 5 min. Discharge the material to obtain a low-shrinkage sulfate-activated all-solid waste low-carbon cementitious material. The total mixing time in step (4) is 20 min.

[0047] In this embodiment, the mass ratio of the internal maintenance component to the micro-expansion regulation component is 1.75:1.

[0048] Comparative Example 1: A sulfate-activated solid waste cementitious material, composed of the following components: 300g steel slag powder, 550g blast furnace slag powder, 120g desulfurized gypsum powder, and 30g composite sulfate activator, without internal curing components or micro-expansion regulating components.

[0049] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) Put the steel slag powder, slag powder, desulfurized gypsum powder and the composite sulfate activator obtained in step (1) into a double-screw mixer, mix them evenly, and discharge them to obtain the final product.

[0050] Comparative Example 2: A sulfate-activated solid waste cementitious material, composed of the following components: 300g steel slag powder, 550g blast furnace slag powder, 120g desulfurized gypsum powder, 30g composite sulfate activator, and 25g pre-wetted recycled fine powder; only internal curing components are added, and no micro-expansion regulating components are added.

[0051] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) Pre-wetting treatment of internal curing components: take a specific surface area of ​​650m² 2 / kg of waste concrete recycled fine powder was sprayed with water and stirred until the moisture content was 20%, then sealed and aged for 36 hours to obtain pre-wetted recycled fine powder; (4) Add the steel slag powder, slag powder, desulfurized gypsum powder and composite sulfate activator obtained in step (2) into a double-screw mixer at a speed of 45 rpm. First, mix at low shear for 15 min; then add the pre-wetted regenerated fine powder obtained in step (3) and continue mixing at low shear for 5 min. Discharge the material to obtain the final product.

[0052] Comparative Example 3: A sulfate-activated solid waste cementitious material, composed of the following components: 300g steel slag powder, 550g blast furnace slag powder, 120g desulfurized gypsum powder, 30g composite sulfate activator, and 15g calcium sulfoaluminate clinker powder; only micro-expansion regulating components are added, and no internal curing components are added.

[0053] The preparation method is as follows: (1) Steel slag, mineral slag, and desulfurized gypsum were dried and ground separately to obtain a specific surface area of ​​560 m². 2 / kg steel slag powder, specific surface area 500m² 2 / kg of slag powder and a specific surface area of ​​420m² 2 / kg of desulfurized gypsum powder; (2) Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; (3) The steel slag powder, slag powder, desulfurized gypsum powder obtained in step (1), the composite sulfate activator obtained in step (2), and calcium sulfoaluminate clinker powder are put into a double-screw mixer, mixed evenly, and discharged to obtain the product.

[0054] IV. Performance Testing and Results 1. Physical and mechanical properties and shrinkage properties The 28-day compressive strength, autogenous shrinkage, drying shrinkage, and ring-constrained cracking time of the cementitious materials obtained in Examples 1-3 and Comparative Examples 1-3 were tested according to the aforementioned test method. The results are shown in Table 1.

[0055] Table 1 Physical and mechanical properties and shrinkage data of cementitious materials

[0056] As shown in Table 1, the 28-day autogenous shrinkage of each embodiment of the present invention is no higher than 120 × 10⁻⁶. -6 The drying shrinkage after 90 days is no higher than 280×10. -6 It meets the performance specifications.

[0057] Compared with Comparative Example 1, Example 1 showed an 8.9% increase in 28-day compressive strength and a 28-day autogenous shrinkage of 162 × 10⁻⁶. -6 Reduced to 98×10 -6 The decrease was 39.5%, and the 90-day drying shrinkage was 356×10. -6 Reduced to 258×10 -6 The decrease was 27.5%, and the time for ring cracking was extended from 28 days to more than 56 days.

[0058] Example 2 uses a combination of superabsorbent resin composite and nano-γ-Al2O3, which has the largest reduction in shrinkage and a ring cracking time of more than 63 days, making it the preferred solution of the present invention.

[0059] Comparing Example 1 with Comparative Example 2 (containing only internal curing components) and Comparative Example 3 (containing only micro-expansion regulating components), it can be seen that: the 28-day autogenous shrinkage of Comparative Example 2 is 118 × 10⁻⁶. -6 Comparative Example 3 is 146 × 10 -6 All were significantly higher than 98×10 in Example 1. -6The drying shrinkage and cracking time also showed the same pattern. That is, while both single-component internal curing components and single-component micro-expansion regulating components can improve shrinkage to some extent, the improvement after combining the two exceeds the simple sum of their individual effects, indicating a significant positive synergistic effect between the internal curing components and the micro-expansion regulating components. Figure 1 As shown.

[0060] 2. Liquid absorption and water release behavior of internal maintenance components Following the aforementioned methods for determining liquid absorption ratio and water release rate, the two types of internal curing components used in this invention were tested, with unmodified ordinary superabsorbent polymer (SAP) used as a comparison. The results are shown in Table 2 and... Figure 2 As shown.

[0061] Table 2. Liquid absorption and water release behavior of internal curing components

[0062] As shown in Table 2, ordinary superabsorbent polymers exhibit a liquid absorption ratio of only 2.1 g / g in simulated cement slurry, and the particles collapse, failing to provide adequate internal curing. However, after modification with aluminosilicate powder or the use of pre-wetted porous recycled fine powder, the liquid absorption ratio reaches 5–15 g / g, and the absorbed water is released with a delayed effect during the temperature drop phase (water release rate exceeding 62% after 48 hours), meeting the requirement for replenishing moisture during the concrete shrinkage-sensitive period. This is precisely why this invention limits the internal curing component to pre-wetted porous recycled fine powder or a composite of superabsorbent polymer and aluminosilicate powder, and limits the liquid absorption ratio to 5–15 g / g.

[0063] 3. Micro-expansion regulation of component expansion strain The expansion strain of the cementitious materials of Examples 1, 2, and Comparative Example 1 (without micro-expansion regulating components) at different ages was measured, and the results are shown in Table 3 and... Figure 3 As shown.

[0064] Table 3. Expansion strain of components with micro-expansion regulation (unit: ×10⁻) 6 )

[0065] As shown in Table 3, after incorporating the micro-expansion regulating component, the cementitious material produced 100–300 × 10⁻⁶ particles within 3–7 days. -6 The stable micro-expansion occurred precisely during the most intense stages of autogenous contraction and temperature-induced contraction, with the expansion timeline synchronized with the contraction development; after 14 days, the expansion strain tended to stabilize, without any excessive expansion in the later stages. In contrast, Comparative Example 1, without the addition of micro-expansion regulating components, showed no effective expansion at any age.

[0066] 4. Microstructure analysis Figure 4This is a SEM image of the hardened slurry of the cementitious material obtained in Example 1 after 28 days. Needle-shaped ettringite (AFt) crystals and flocculent CSH gel are uniformly interwoven, with fine and evenly distributed pores and no obvious cracks at the particle edges. In contrast, the hardened slurry of Comparative Example 1 shows more microcracks and unfilled pores. The comparison of microstructures indicates that the water released by the internal curing component promotes the later-stage hydration of slag and steel slag, while the AFt generated by the micro-expansion regulating component fills and refines the pore structure; both contribute to the densification of the hardened slurry structure.

[0067] The synergistic effect of the internal maintenance component and the micro-expansion regulation component in this invention can be divided into three stages: Stage 1 (0-1d, early molding stage): The pre-wetting moisture in the internal curing component provides a local water source around the particles, inhibiting early self-drying; the micro-expansion regulating component has not yet reacted in large quantities, and the system is mainly characterized by plastic shrinkage.

[0068] Phase Two (1–7 days, peak period of intensity development and shrinkage): The micro-expansion regulating component reacts rapidly under sulfate activation to generate AFt, producing stable micro-expansion to compensate for chemical shrinkage and temperature-induced shrinkage; simultaneously, the internal curing component gradually releases moisture as the internal relative humidity decreases, maintaining continuous hydration. The two work synergistically to minimize net shrinkage.

[0069] Phase 3 (7–28 days, late hydration period): The moisture released by the internal curing components promotes the late hydration of slag and steel slag, generating more CSH gel to fill the pores, further compacting the structure, making the compensated micro-strain tend to stabilize, and preventing excessive expansion or shrinkage rebound in the later stage.

[0070] C40 concrete was prepared using the cementitious material from Example 2, with the following mix proportions: cementitious material 380 kg / m³, sand 720 kg / m³, crushed stone 1100 kg / m³, water-cement ratio 0.38, and polycarboxylate superplasticizer 1.6 kg / m³.

[0071] Test results: Initial slump 215mm, 1-hour slump 200mm; 28-day compressive strength 48.6MPa; 56-day electrical flux 625C; 90-day drying shrinkage 268×10⁻⁶. -6 No cracks were observed in the circular restraint cracking test after more than 63 days. Compared with ordinary Portland cement concrete of the same strength grade, carbon emissions were reduced by 42%.

[0072] The above results indicate that the cementitious material of the present invention, after pre-wetting treatment or composite modification, does not excessively absorb mixing water, has good compatibility with polycarboxylate superplasticizer, and the reduction of shrinkage and densification of structure simultaneously improve the durability properties of concrete, such as impermeability and chloride ion penetration resistance, thus meeting the conditions for industrial application.

[0073] In other embodiments, the porous recycled fine powder can also be made from waste clay brick fine powder. Waste clay brick fine powder and waste concrete recycled fine powder both belong to the category of recycled fine powder from construction solid waste. They have a porous structure and pozzolanic activity. After undergoing the same pre-wetting treatment (spraying water and stirring until the moisture content is 15% to 25%, then sealing and aging for 24 to 48 hours), they can also play the same internal curing role. Those skilled in the art can implement this invention without creative effort based on the description of this invention.

[0074] In other embodiments, the micro-expansion regulating component can also be calcium aluminate or nano-Al(OH)3. Calcium aluminate, nano-Al(OH)3, and the calcium sulfoaluminate clinker powder and nano-γ-Al2O3 used in the examples are all active aluminum sources. Under sulfate activation, they can all generate micro-expansion by forming ettringite in the early stage, and their mechanisms of action are consistent. Their specific surface area is also controlled at 400-700 mm². 2 / kg is sufficient.

[0075] The compound sulfate activator can be flexibly adjusted within a limited ratio range. For example, in a specific ratio, 55 parts of hemihydrate gypsum, 20 parts of sodium sulfate, 10 parts of water glass, 3 parts of triethanolamine, and 5 parts of sodium aluminate are mixed and ground together by mass.

[0076] In cases where improved early strength is required, silicate cement clinker powder can be used to supplement the excess cementitious material. That is, silicate cement clinker powder can replace part of the steel slag powder or slag powder. Its incorporation does not affect the synergistic effect of the internal curing components and the micro-expansion regulating components.

[0077] The cementitious material of this invention can be widely used in engineering fields such as precast components, large-volume concrete, water conservancy projects, and road and bridge projects where high volume stability is required.

[0078] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste, characterized in that, The total mass of the cementitious material includes the following components: Steel slag powder 25%–40%; Slag powder 40%–60%; Desulfurized gypsum 8%–15%; Compound sulfate activator 2%–6%; Internal maintenance components: 1%–5%; Micro-expansion regulating components: 0.5%–3%; The remainder is silicate cement clinker powder or no silicate cement clinker powder is provided; The internal curing component is a composite of pre-wetted porous recycled fine powder or superabsorbent resin and silica-alumina powder. The internal curing component has an absorption ratio of 5-15 g / g in simulated cement pore liquid. The simulated cement pore liquid is a saturated calcium hydroxide solution at 25°C. The micro-expansion regulating component is at least one of calcium aluminate, calcium sulfoaluminate clinker powder, nano γ-Al2O3, or nano Al(OH)3.

2. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The porous recycled fine powder is recycled waste concrete fine powder or waste clay brick fine powder, with a specific surface area of ​​500-800 m². 2 / kg; the pre-wetting treatment method is as follows: spray water onto the porous regenerated fine powder and stir until the moisture content is 15% to 25%, then seal and age for 24 to 48 hours.

3. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The composite of the superabsorbent resin and the silica-alumina powder comprises, by weight, 5-15 parts of sodium polyacrylate or polyacrylamide superabsorbent resin, 30-50 parts of active metakaolin, and 10-20 parts of nano silica, and is prepared by dry mixing and granulation, with a particle size of 50-200 μm.

4. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The micro-expansion regulating component is calcium sulfoaluminate clinker powder or nano-γ-Al2O3, with a specific surface area of ​​400–700 m². 2 / kg.

5. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The composite sulfate activator, by weight, comprises: 40-70 parts anhydrous gypsum or hemihydrate gypsum, 10-30 parts sodium sulfate, 5-15 parts water glass, 1-5 parts triethanolamine, and 2-8 parts sodium aluminate.

6. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The specific surface area of ​​the steel slag powder is 450-650 m². 2 / kg, free CaO content ≤3.5%, free MgO content ≤3.0%; the specific surface area of ​​the slag powder is 400-550m². 2 / kg; the specific surface area of ​​the desulfurized gypsum is 350-500 m² / kg. 2 / kg.

7. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, Based on the total mass of the cementitious material, the internal curing component is 2% to 3.5%, and the micro-expansion regulating component is 1% to 2%.

8. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The mass ratio of the internal maintenance component to the micro-expansion regulation component is 1.67:1 to 2:

1.

9. The low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to claim 1, characterized in that, The 28-day autogenous shrinkage of the cementitious material is ≤120×10⁻⁶. -6 90-day drying shrinkage ≤280×10 -6 .

10. A method for preparing a low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste, characterized in that, The preparation of the low-shrinkage sulfate-activated low-carbon cementitious material for all solid waste according to any one of claims 1 to 9 includes the following steps: S1: Dry and grind steel slag, mineral slag, and desulfurized gypsum to the target specific surface area to obtain steel slag powder, mineral slag powder, and desulfurized gypsum powder; S2: Mix the components of the composite sulfate activator in proportion and co-mill until the specific surface area is 200-350 m². 2 / kg, to obtain a composite sulfate activator; S3: Pre-wet or granulation pre-treatment is performed on the internal curing component to obtain the pre-wetted internal curing component; S4: Add the steel slag powder, blast furnace slag powder, desulfurized gypsum powder obtained in step S1, the composite sulfate activator obtained in step S2, the micro-expansion regulating component, and optional silicate cement clinker powder into a mixer, and mix under low shear for 5 to 25 minutes; then add the pre-wet internal curing component obtained in step S3, and continue to mix under low shear for 5 minutes, and discharge the material to obtain the low-shrinkage sulfate-activated all-solid waste low-carbon cementitious material. The mixer is a plow-type mixer or a double ribbon mixer, and the total mixing time in step S4 is 10 to 30 minutes.