A fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs and its preparation method
By using low-content composite additives and a short-time peak sintering process, a fine-grained core-shell structure is constructed, which solves the problems of oxidation resistance and long-term reliability of base metal internal electrode MLCCs under reducing atmosphere, and achieves improved high dielectric properties and temperature stability, making it suitable for existing BME-MLCC production.
Patent Information
- Application Number
- CN202611425985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to improve the reduction resistance and long-term reliability of base metal internal electrode MLCCs while maintaining high dielectric properties and temperature stability. In particular, when the dielectric layer is thinned, excessive additive doping can lead to abnormal grain growth, reduced grain boundary density, and local electric field concentration, affecting the insulation stability and long-term reliability of the capacitor.
By employing low-content composite reliability additives, including magnesium sources, manganese sources, rare earth oxides, and glass sintering aids, and combining short-time peak sintering with rapid cooling heat treatment processes, an oxygen vacancy migration barrier network is constructed to form a fine-grained core-shell structure, which inhibits abnormal grain growth. Furthermore, the dielectric layer is sintered in a reducing atmosphere and then oxidized to improve its reliability.
It achieves high dielectric properties and X7R temperature stability with lower additive dosage and thermal budget, while improving the reduction resistance and long-term reliability of MLCCs, reducing the leakage current growth rate of the dielectric layer, and improving batch consistency and production stability.
Smart Images

Figure CN123106201A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of electronic ceramic materials and multilayer ceramic capacitors, specifically relating to a reduction-resistant, high-insulation, and high-reliability X7R type barium titanate-based dielectric ceramic material and its preparation method suitable for multilayer ceramic capacitors with nickel or nickel alloy base metal internal electrodes, and relates to capacitor material technology. Background Technology
[0002] With the rapid development of electronic information technology, the trend towards miniaturization, lightweighting, and high performance in electronic products is becoming increasingly significant. Multilayer ceramic capacitors (MLCCs) are widely used in electronic devices due to their small size and high reliability. MLCCs mainly consist of three parts: an internal electrode, a dielectric layer, and terminal electrodes. A monolithic structure MLCC is fabricated by stacking and sintering ceramic dielectric layers with metal internal electrodes and coating both ends with terminal electrodes. Based on the temperature characteristics of different dielectric materials, MLCCs can be divided into Class I and Class II ceramic capacitors. Class I ceramic capacitors (such as C0G materials) have high temperature stability, and their capacitance remains essentially constant over a wide temperature range, making them commonly used in compensation circuits and high-frequency circuits. Class II ceramic capacitors have a high dielectric constant, but their temperature stability is relatively poor; their dielectric constant changes non-linearly with temperature variations, making them suitable for applications such as smoothing, coupling, and energy storage circuits. According to the standards of the Electronic Industries Association (EIA), the temperature characteristics of Class II ceramic capacitors are further classified. X7R type ceramic materials have a temperature range of -55℃ to 125℃ and a capacitance temperature change rate (TCC) of less than ±15%, meeting temperature stability requirements. Therefore, they are widely used in industrial and consumer electronics. Based on different metal internal electrodes, MLCCs can be divided into base metal internal electrode multilayer ceramic capacitors (BME-MLCCs) and noble metal internal electrode ceramic capacitors (PME-MLCCs). BME-MLCCs often use relatively inexpensive metals such as Cu and Ni as internal electrodes and require sintering in a reducing atmosphere with low oxygen partial pressure.
[0003] Base metal internal electrodes are inexpensive, offering a significant cost advantage, and nickel electrodes possess a series of unique advantages, such as low resistivity, low migration rate, and high electrochemical stability. In recent years, with the increasing demand for MLCCs, the cost-effective base metal internal electrode (BME-MLCC) has gradually replaced noble metal internal electrode (PME-MLCC). However, in actual production, base metal internal electrode MLCCs also face certain technical challenges. Because nickel and copper are easily oxidized during sintering in air, high-temperature sintering in a reducing atmosphere is necessary to prevent electrode oxidation and loss of conductivity. However, barium titanate-based ceramic materials are prone to TiO2 oxidation during sintering in a reducing atmosphere. 4+Restored to Ti 3+ This phenomenon generates freely moving weakly bound electrons and oxygen vacancies, causing the ceramic dielectric material to become n-type semiconducting, leading to increased dielectric loss and decreased insulation resistance, thereby affecting the electrical performance and long-term stability of the capacitor.
[0004] To improve the insulation performance of dielectrics and solve the semiconductorization problem of BaTiO3 ceramics sintering under low oxygen partial pressure atmospheres, early researchers such as Herbert proposed to compensate for electrons and reduce electron concentration through acceptor doping. Simultaneously, they believed that acceptor doping could pin oxygen vacancies, inhibiting their migration and thus improving insulation resistance. Elements such as iron (Fe), cobalt (Co), and manganese (Mn) readily enter Ti sites and undergo substitution due to their similar ionic radii to titanium (Ti). However, acceptor doping cannot eliminate oxygen vacancies; instead, it may create new oxygen vacancies. This does not effectively solve the problem of insulation resistance degradation caused by oxygen vacancy generation and migration. Later researchers discovered that rare earth elements with ionic radii between barium (Ba) and titanium (Ti) have "amphotericidal effects," capable of entering both A-sites and B-sites in the BaTiO3 perovskite structure, simultaneously generating donor and acceptor effects to compensate for oxygen vacancies and free electrons, while also forming defect associations to inhibit oxygen vacancy migration.
[0005] Chinese patent application (201811033254.8) discloses a method for improving the reduction resistance of barium titanate dielectric materials through variable valence ion doping. Based on BaTiO3, one or more variable valence ion compounds selected from SnO2, MnO2, or NH4VO3 are added to prepare a dielectric material with a dielectric constant similar to that at room temperature, but with higher dielectric loss (1.0%~4.0%) and insulation resistivity (10⁻⁶ Ω·cm). 9 The dielectric constant (Ω·cm) is relatively low. Chinese Patent No. (202110649477.2) discloses a method for preparing reduction-resistant X8R type BaTiO3-based ceramic materials. By adding Bi2O3, MgO, and ZrO2 to BaTiO3, materials with dielectric constants ranging from 669 to 2020 and insulation resistivity ranging from 1.22 to 4.84 × 10⁻⁶ are prepared. 13 The barium titanate-based dielectric ceramic material has a dielectric constant that meets the EIA X7R and X8R standards and has a temperature stability of Ω·cm. However, its dielectric constant varies widely, with the highest being only 2020, and no long-term reliability test has been conducted on the ceramic material.
[0006] Current research on reduction-resistant BaTiO3 dielectric ceramics faces the challenge of simultaneously achieving high dielectric properties, high insulation resistivity, low loss, temperature stability, and long-term reliability. Especially with the continuous thinning of the dielectric layer, excessive additive doping can introduce excessive second phases and inactive grain boundary phases, increasing formulation costs and process fluctuations. Furthermore, prolonged high-temperature sintering can easily lead to abnormal grain growth, reduced grain boundary density, and localized electric field concentration, thus exacerbating insulation degradation under high-temperature DC bias. Therefore, it is necessary to improve the material's reduction resistance, insulation stability, and long-term reliability while maintaining X7R's temperature stability and high dielectric properties, by synergistically controlling grain growth and core-shell-grain boundary structure through short-time peak sintering and rapid cooling, while minimizing the total additive dosage and sintering heat budget. Summary of the Invention
[0007] The purpose of this invention is to provide a fine-grained, grain boundary-type, reduction-resistant, high-reliability MLCC dielectric ceramic. By establishing a quantifiable correlation between microstructure parameters and long-term reliability, this material no longer relies solely on traditional Mg / Mn / single rare earth electron compensation. Instead, it incorporates magnesium sources, manganese sources, rare earth oxides, grain growth inhibitors, and glass sintering aids. After sintering and re-oxidation in a reducing atmosphere, the average sintered grain size of the dielectric ceramic is 0.12–0.50 μm, and the area of abnormally coarse grains larger than twice the average grain size does not exceed 15%. By constructing an oxygen vacancy migration barrier network in the BaTiO3 grain shell and grain boundary regions, the reliability of the dielectric layer under reduction sintering, re-oxidation, and high-temperature DC bias conditions is improved.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: using BaTiO3 with a wavelength of 80 nm to 150 nm as the main material, BaTiO3 accounts for 98.20 wt% to 98.80 wt% of the total mass of the ceramic material; the remainder is a composite reliability additive, which accounts for 1.20 wt% to 1.80 wt% of the total mass of the ceramic material, and includes at least a magnesium source, a manganese source, an A-site regulator, rare earth oxides, and a glass sintering aid.
[0009] 1. This invention uses BaTiO3 as the main component, with BaTiO3 accounting for 98.20 wt% to 98.80 wt% of the total mass of the ceramic material. The total amount of composite reliability additives is only 1.20 wt% to 1.80 wt%. Under low doping conditions, dielectric properties, reduction resistance and long-term reliability can be balanced, avoiding the adverse effects of excessive additives on the dielectric properties of the BaTiO3 matrix.
[0010] 2. This invention employs a heat treatment process combining short-time peak sintering and rapid cooling. While ensuring ceramic densification, it shortens the time the material spends in the rapid grain growth temperature range, thereby inhibiting abnormal grain growth and maintaining a fine-grained core-shell structure and high grain boundary density. Compared to long-duration high-temperature holding sintering, this process is advantageous for achieving a synergistic improvement in X7R temperature stability, reduction resistance, and long-term reliability under conditions of lower thermal budget and lower additive dosage.
[0011] 3. This invention forms a high-resistivity migration barrier layer at the grain boundary by using a grain boundary passivation aid, which can reduce the leakage current growth rate of thin dielectric layer MLCCs under high temperature, high humidity or high DC bias environments and improve reliability.
[0012] 4. The present invention uses low-content composite doping, which helps to reduce the formation of the second phase, the increase of inactive phase at grain boundaries and the decrease in dielectric constant caused by excessive additives, thereby reducing production costs and improving the insulation stability of ceramic materials after sintering in a reducing atmosphere while maintaining a high dielectric constant.
[0013] 5. The dielectric ceramic prepared using the formula and process of this invention, under preferred embodiments, can achieve a dielectric constant of 2600–3000 at 25 °C and 1 kHz, tanδ ≤ 1.2%, and an insulation resistivity ≥ 2.0 × 10⁻⁶. 12 Ω·cm, and meets the X7R temperature characteristics in the range of -55 ℃ to 125 ℃.
[0014] The present invention has fewer types and less total amount of additives, and the formulation is relatively simple. It can reduce the weighing error, composition fluctuation and process sensitivity caused by the addition of a large number of multiple components, which is beneficial to improving the batch consistency and sintering stability of materials, and is applicable to the existing BME-MLCC production process. Attached Figure Description
[0015] Figure 1 is a schematic flowchart of the preparation method of the reduction-resistant high-performance X7R type ceramic material of the present invention.
[0016] Figure 2 is a characteristic curve of the dielectric constant of the samples in Examples 1-8 of the present invention as a function of temperature.
[0017] Figure 3 is a characteristic curve of the dielectric constant of the samples in Examples 1-8 of the present invention as a function of temperature.
[0018] Figure 4 shows the HALT lifetime of the samples in Examples 1-8 of the present invention (samples under test conditions of 210℃ and 1KV / mm until failure).
[0019] Figure 5 This is the EDS scan result of the sample in Example 4 of the present invention.
[0020] Figure 6This is the SEM result of the sample in Example 4 of this invention.
[0021] Figure 7 This is the STEM-EDS line scan result of the sample in Example 8 of the present invention (proving the core-shell structure formed by elemental segregation). Detailed Implementation
[0022] Examples 1-8 Step 1: Ingredient preparation; accurately weigh and prepare the ingredients according to the mass ratio of each ingredient in Table 1; Step 2: Ball milling; Place the prepared powder into a ball mill jar, mix deionized water, zirconium balls and powder in a mass ratio of 2:1:1, and ball mill for 10 hours at a speed of 280 rpm. Step 3: Granulation and molding; The ball-milled powder is dried in a 100℃ oven, and 15% polyvinyl alcohol by mass is added for granulation. The granulation size is controlled at 80~250 mesh, and it is pressed into a green body with a diameter of 1 cm and a thickness of 0.1 cm under 12MPa. Step 4: Place the green body obtained in Step 3 in a reducing atmosphere of 1-2% H2-98-99% N2, heat it to 1280-1320 ℃ at a heating rate of 3 ℃ / min, and hold it for 5-15 min; then cool it down to 1100-1200 ℃ rapidly and hold it at this temperature for 2 h; after the holding period, cool it to room temperature at a cooling rate of 4 ℃ / min. Step 5: Re-oxidation; The sample obtained in Step 4 is sintered for 2 hours at 900~1050℃ under the protection of N2 atmosphere containing O2 (oxygen content of 10~200ppm) to obtain the final anti-reduction ceramic material. The specific ingredients are shown in Table 1, the specific processes of different embodiments are shown in Table 2, and the performance test results of the obtained material (dielectric loss, dielectric constant, insulation resistivity and capacitance temperature change rate) are shown in Table 3.
[0023] Table 1. Batching table (wt%) of fine-grained, reduction-resistant, high-reliability X7R type ceramic material in Examples 1-8
[0024] Table 2. Short-time peak value-rapid cooling process for examples 1-8 of the fine-grained, reduction-resistant, high-reliability X7R type ceramic material.
[0025] Table 3 Performance Table of Fine-Grained, Reduction-Resistant, High-Reliability X7R Type Ceramic Materials (Examples 1-8)
Claims
1. A fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs, characterized in that, The main material is BaTiO3 with a particle size of 80–150 nm, which accounts for 98.20 wt%–98.80 wt% of the total mass of the ceramic material; the remainder is a composite reliability additive, which accounts for 1.20 wt%–1.80 wt% of the total mass of the ceramic material. The composite reliability additive includes at least a magnesium source, a manganese source, rare earth oxides, and silicon dioxide. After reduction sintering and re-oxidation, the dielectric ceramic forms a fine-grained core-shell-grain boundary structure with an average grain size of 0.12–0.50 μm.
2. The fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs according to claim 1, characterized in that, The magnesium source is MgCO3, the manganese source is MnCO3, the A-site regulator is SrCO3, and the sintering aid is SiO2; based on the total mass of the ceramic material, the content of MgCO3 is 0.28 wt% to 0.45 wt%, the content of MnCO3 is 0.10 wt% to 0.15 wt%, the content of SrCO3 is 0.22 wt% to 0.35 wt%, and the content of SiO2 is 0.25 wt% to 0.30 wt%.
3. The fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs according to claim 1 or 2, characterized in that, The rare earth oxides must be selected from two or more of Yb2O3, Dy2O3 and Ho2O3, and the total content of the rare earth oxides is 0.35 wt% to 0.55 wt%.
4. The fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs according to any one of claims 1 to 3, characterized in that, The grain size distribution D90 / D10 of the dielectric ceramic is 1.5 to 3.5, and the area of abnormally coarse grains with a size greater than twice the average grain size does not exceed 15%.
5. The fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs according to any one of claims 1 to 4, characterized in that, The dielectric ceramic exhibits a dielectric constant of 2600–2810 at 25 °C and 1 kHz, a dielectric loss tanδ ≤ 1.2%, and an insulation resistivity ≥ 2.0 × 10⁻⁶. 12 Ω·cm, and meets the X7R temperature characteristics in the range of -55 to 125 ℃.
6. A method for preparing a fine-grained, reduction-resistant, high-reliability dielectric ceramic for MLCCs according to any one of claims 1 to 5, characterized in that, The short-peak rapid sintering process includes the following steps: Step 1: Ingredient preparation, ball milling and molding; Weigh BaTiO3 and composite reliability additives according to the raw material ratio described in any one of claims 1 to 3, ball mill and mix them evenly, then dry, granulate and press to obtain green body; Step 2: Short-time peak rapid sintering; The green body obtained in Step 1 is placed in a reducing atmosphere of 1% H2-99% N2 to 2% H2-98% N2, and heated to 1280-1320 ℃ at a heating rate of 3 ℃ / min, and held at the peak temperature for only 5-15 min; After the peak holding is completed, the temperature is immediately and rapidly cooled to 1100-1200 ℃, and held at this temperature for 2 h; After the holding is completed, the temperature is cooled to room temperature at a cooling rate of 4 ℃ / min. Step 3: Re-oxidation; The sample obtained in Step 2 is placed in an N2 atmosphere containing O2 and re-oxidized at 900-1050 °C for 2 h to obtain fine-grained, reduction-resistant, and highly reliable dielectric ceramic for MLCCs.
7. The preparation method according to claim 6, characterized in that, The short-time peak rapid sintering shortens the residence time of the dielectric ceramic in the high-temperature grain rapid growth range by holding it at a peak temperature range of 1280–1320 °C for only 5–15 min and then immediately and rapidly reducing it to 1100–1200 °C, thereby suppressing abnormal grain growth and maintaining a fine-grained core-shell structure and a high grain boundary density.
8. The preparation method according to claim 6 or 7, characterized in that, In step 1, deionized water, zirconium balls, and powder are mixed in a mass ratio of 2:1:1 and ball-milled at 280 rpm for 10 h. The ball-milled powder is dried at 100 ℃, and 15% polyvinyl alcohol is added for granulation. The granulation size is controlled between 80 and 250 mesh, and the powder is dry-pressed under 12 MPa pressure.
9. The preparation method according to any one of claims 6 to 8, characterized in that, The oxygen content in the N2 atmosphere containing O2 in step 3 is 10-200 ppm.
Citation Information
Patent Citations
Method for improving reducibility resistance of barium titanate dielectric material through valence variation ion doping
CN108975907A
Anti-reduction X8R type BaTiO3-based dielectric ceramic material and preparation method thereof
CN113277847A