Electromagnetic pure iron material coated with wear-resistant coating on surface and heat treatment method

Through the controlled temperature increase and cooling process under the protection of hydrogen and nitrogen, the problem of damage to the magnetic properties of electromagnetic pure iron materials by the surface coated wear-resistant coating is solved, and the magnetic performance recovery, hardness and wear resistance after coating are achieved. Take into account both.

CN119040849AActive Publication Date: 2024-11-29CHINA NAT PETROLEUM CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310620285.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The surface coated wear-resistant coating has damaged the magnetic properties of electromagnetic pure iron materials under high temperature conditions, resulting in a significant decline in its magnetic properties, and the existing heat treatment process cannot effectively recover.

Method used

The vacuum heat treatment furnace is used for heating, insulation and cooling treatment. Through the use of hydrogen and nitrogen protective gases, the heating and cooling rates are controlled, internal stress is reduced, oxidation is prevented, and the magnetic properties of the coating are restored.

Benefits of technology

It effectively reduces the internal stress after the coating, restores the coercive force and maximum magnetic permeability of the electromagnetic pure iron material, and maintains high hardness and wear resistance, achieving both hardness, wear resistance and magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040849A_ABST
    Figure CN119040849A_ABST
Patent Text Reader

Abstract

According to the electromagnetic pure iron material coated with the wear-resistant coating on the surface and the heat treatment method, through the vacuum heat treatment process under the hydrogen and nitrogen conditions, the surface of the coated electromagnetic pure iron can be prevented from being oxidized; meanwhile, the adverse effects of serious reduction of the magnetic performance of the electromagnetic pure iron caused by abnormal grain growth, structural deformation, internal stress increase and the like of the coating process under the high-temperature condition on the electromagnetic pure iron are reduced; the coercive force, the maximum magnetic conductivity and other magnetic properties of the coated electromagnetic pure iron material are effectively improved, the high hardness and the strong wear resistance of the coated electromagnetic pure iron material can be kept, the electromagnetic pure iron material with the good magnetic properties, the high hardness and the strong wear resistance is finally obtained, and the application field of the electromagnetic pure iron material is further expanded. The pressure of the hydrogen and the pressure of the nitrogen in the vacuum heat treatment furnace are kept constant all the time, so that the electromagnetic pure iron surface coated with the wear-resistant coating is under the vacuum reduction condition, the coating cannot be oxidized, concentrated in stress and the like, and the hardness and the wear resistance of the coating cannot be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heat treatment technology for soft magnetic materials, and relates to an electromagnetic pure iron material with a wear-resistant coating on the surface and a heat treatment method. Background Art

[0002] The main chemical composition of industrial electromagnetic pure iron is iron. It is a high-quality steel with an iron content of more than 99.5%, and low carbon, sulfur and phosphorus content. It has high saturation magnetic induction intensity Bs and magnetic permeability H, low coercive force Hc, good cold and hot processing performance, low price, simple heat treatment process, etc. It is widely used as the shell, valve core, movable iron core and other parts of the solenoid valve in the electrical, telecommunications, electronic defense and other industries.

[0003] However, the content of alloy elements in electromagnetic pure iron materials is almost zero, resulting in extremely low hardness and poor wear and corrosion resistance. Surface coating of TiN wear-resistant coating is an effective way to increase the hardness of electromagnetic pure iron and improve its wear and corrosion resistance. However, due to the high hardness and excellent wear and corrosion resistance of TiN wear-resistant coating process is often completed under high temperature process conditions (chemical vapor deposition process, temperature 900-1000℃), although this coating improves the hardness and wear and corrosion resistance of electromagnetic pure iron, it is easy to cause its grain growth and stress increase, resulting in serious damage to its magnetic properties, such as a sharp increase in coercive force, a significant decrease in maximum magnetic flux, etc., and it is impossible to achieve a balance between hardness, wear and corrosion resistance and magnetic properties.

[0004] Studies have shown that metal heat treatment processes can eliminate internal stress in materials and prevent structural deformation, and are an effective means of restoring the magnetic properties of electromagnetic pure iron materials. However, existing heat treatment processes only meet the recovery of the magnetic properties of electromagnetic pure iron materials that have been heat treated under low-temperature process conditions such as surface nitriding and surface nickel plating. Due to the lower process temperature conditions, processes such as surface nitriding and surface nickel plating have relatively little damage to the magnetic properties of electromagnetic pure iron materials. In contrast, surface coating with a wear-resistant coating has serious damage to its magnetic properties due to its high temperature, and a corresponding effective heat treatment process has not yet been reported.

[0005] Therefore, in view of the problem that the magnetic properties of electromagnetic pure iron materials with wear-resistant coating on the surface decrease significantly under current high temperature conditions, there is an urgent need in this field to develop a heat treatment process that can effectively improve the magnetic properties of electromagnetic pure iron materials with wear-resistant coating on the surface, so as to achieve the hardness, corrosion resistance and wear resistance of the electromagnetic pure iron material after coating, as well as magnetic properties, extend the service life of the electromagnetic pure iron material products and further expand its application range. Summary of the invention

[0006] The purpose of the present invention is to solve the problem in the prior art that the magnetic properties of electromagnetic pure iron materials are seriously damaged due to the high temperature of the surface coating of wear-resistant coating, resulting in a significant decrease in the magnetic properties of the electromagnetic pure iron materials, and to provide an electromagnetic pure iron material with a surface coating of wear-resistant coating and a heat treatment method.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] The present invention provides a heat treatment method for an electromagnetic pure iron material coated with a wear-resistant coating on its surface, comprising the following steps:

[0009] Placing electromagnetic pure iron with a wear-resistant coating on the surface into a heating device;

[0010] A protective gas is introduced into the heating device to perform heating, heat preservation and temperature reduction treatments in sequence;

[0011] The temperature in the heating device drops to the set temperature, the protective gas is stopped, and the temperature in the heating device is cooled to room temperature to obtain the electromagnetic pure iron material.

[0012] Preferably, the wear-resistant coating is a TiN coating, and the TiN coating is made by a chemical vapor deposition method.

[0013] Preferably, the heating device is a vacuum heat treatment furnace, and the vacuum degree of the vacuum heat treatment furnace is 10 -1 Pa~10 -2 Pa.

[0014] Preferably, the protective gas is hydrogen and nitrogen; the flow rate of hydrogen is 450 sccm to 700 sccm, and the flow rate of nitrogen is 450 sccm to 700 sccm.

[0015] Preferably, the heating and insulation process is as follows: the temperature in the heating device is increased to 500°C to 550°C at a rate of 3°C / min to 7°C / min, and then the temperature is increased to 720°C to 820°C at a heating rate of 2°C / min to 6°C / min and the first insulation is carried out for 30min to 60min; after the first insulation, the temperature is increased to 860°C to 900°C at a heating rate of 2°C / min to 6°C / min and the second insulation is carried out for 3.5h to 6h.

[0016] Preferably, the cooling process is as follows: after the second insulation is completed, the temperature in the heating device is cooled to 650℃~700℃ at a cooling rate of 0.5℃ / min~1.5℃ / min; then cooled to 450℃~500℃ at 3℃ / min~5℃ / min, and then cooled to 100℃~150℃ by furnace cooling, and the introduction of protective gas is stopped.

[0017] Preferably, the pressure in the heating device is 2300Pa to 5000Pa.

[0018] Preferably, the protective gas pressure in the heating device is constant.

[0019] Preferably, the hardness of the electromagnetic pure iron after heat treatment is 1500HV-1700HV, the friction coefficient of the wear-resistant coating is 0.30-0.35, the coercive force of the wear-resistant coating is 22.5A / m-25.4A / m, and the magnetic permeability of the wear-resistant coating is 14.5mH / m-16.3mH / m.

[0020] The electromagnetic pure iron material proposed by the present invention is prepared by adopting a heat treatment method of the electromagnetic pure iron material with a wear-resistant coating on the surface.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention proposes a heat treatment method for an electromagnetic pure iron material with a wear-resistant coating on its surface, which places the electromagnetic pure iron with a wear-resistant coating on its surface into a heating device to prevent oxidation of the electromagnetic pure iron surface after coating, and reduce the adverse effects of abnormal grain growth and increased internal stress on the electromagnetic pure iron caused by the coating process under high temperature conditions, which seriously reduce the magnetic properties of the electromagnetic pure iron. Through the unique heat treatment process design during the heating and cooling process, the internal stress of the electromagnetic pure iron with a wear-resistant coating on its surface is effectively reduced, thereby achieving significant recovery of magnetic properties such as coercive force and maximum magnetic permeability of the electromagnetic pure iron material after coating, and maintaining high hardness and strong wear resistance of the electromagnetic pure iron after coating, and finally obtaining an electromagnetic pure iron material with good magnetic properties, high hardness and strong wear resistance, further expanding its application field.

[0023] Furthermore, the high vacuum condition can prevent the wear-resistant coating on the surface of the electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause the matrix to oxidize, thereby negatively affecting the magnetic properties of the electromagnetic pure iron.

[0024] Furthermore, the presence of protective gas can make the electromagnetic pure iron material heated more evenly; heating to a certain temperature at a certain heating rate and keeping it warm, and further increasing the temperature and keeping it warm, can make the grains grow fully and evenly, further reduce the internal stress, further improve the soft magnetic properties, further reduce the coercive force and further increase the maximum magnetic permeability.

[0025] Furthermore, slowly heating up and keeping the high temperature section warm can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, while making the internal structure of the electromagnetic pure iron more balanced, reducing the internal stress to a minimum, further reducing the coercive force, and increasing the maximum magnetic permeability to a maximum value.

[0026] Furthermore, slow cooling can prevent stress concentration and cracking of the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, minimizing the impact on its magnetic properties.

[0027] Furthermore, the cooling rate in the low-temperature section is accelerated, which can prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix from causing lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0028] Furthermore, the pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron coated with the wear-resistant coating is under vacuum reduction conditions, and the coating will not be oxidized or stress concentrated, thereby ensuring that the hardness and wear resistance of the coating will not decrease, thereby achieving a balance between hardness, wear resistance and magnetic properties of the electromagnetic pure iron material coated with the wear-resistant coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 The present invention is a flow chart of a heat treatment method for electromagnetic pure iron material with a wear-resistant coating on its surface.

[0031] Figure 2 Schematic diagram of the heat treatment process curve of Example 1 of the present invention.

[0032] Figure 3 This is a hardness test diagram of the electromagnetic pure iron material of Example 1 of the present invention.

[0033] Figure 4 This is a test diagram of the friction coefficient of the electromagnetic pure iron material of Example 1 of the present invention.

[0034] Figure 5 This is a coercive force test diagram of the electromagnetic pure iron material of Example 1 of the present invention.

[0035] Figure 6 This is a maximum magnetic permeability test diagram of the electromagnetic pure iron material of Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0037] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0039] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0040] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0041] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0042] As used herein, the term "electromagnetic pure iron" refers to high-quality steel with an iron content of more than 99.5%, which is a low-carbon, low-sulfur and low-phosphorus iron. The corresponding national standard is GB6983-2008 electromagnetic pure iron.

[0043] As used herein, the terms "include", "comprises", and "comprising" are interchangeable and include not only closed definitions, but also semi-closed and open definitions. In other words, the terms include "consisting of", "consisting essentially of".

[0044] As used herein, the term "vacuum heat treatment furnace" refers to a device for performing heat treatments such as normalizing, annealing, tempering, and normalizing on metal materials under a vacuum environment.

[0045] As used herein, the term "coercive force" refers to the fact that after a magnetic material is saturated magnetized, a magnetic field of a certain magnitude is added in the opposite direction of the original magnetizing field to make the magnetic induction intensity return to zero. This magnetic field is called the coercive magnetic field, also known as coercive force, and its symbol is Hc.

[0046] As used herein, the term "maximum magnetic permeability" refers to the maximum value of the magnetic permeability at each point on the basic magnetization curve, and the symbol is μm.

[0047] As used herein, the term "sccm" is a unit of volume flow, ie, standard-state cubic centimeter per minute.

[0048] As used herein, the term "protective gas" refers to a gas having a purity of 99.99%.

[0049] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0050] The present invention provides a heat treatment method for an electromagnetic pure iron material with a wear-resistant coating on its surface, such as Figure 1 As shown, the following steps are included:

[0051] Step 1, placing electromagnetic pure iron with a wear-resistant coating on the surface into a heating device;

[0052] The wear-resistant coating is a TiN coating, which is prepared by a chemical vapor deposition method.

[0053] The heating device is a vacuum heat treatment furnace, and the vacuum degree of the vacuum heat treatment furnace is 10 -1 Pa~10 -2 Pa.

[0054] The protective gases are hydrogen and nitrogen; the hydrogen flow rate is 450 sccm to 700 sccm, and the nitrogen flow rate is 450 sccm to 700 sccm.

[0055] Step 2, introducing protective gas into the heating device, and performing heating, heat preservation and cooling treatment in sequence;

[0056] The heating and insulation process is as follows: the temperature in the heating device is increased to 500℃~550℃ at a rate of 3℃ / min~7℃ / min, and then the temperature is increased to 720℃~820℃ at a heating rate of 2℃ / min~6℃ / min and the first insulation is carried out for 30min~60min; after the first insulation, the temperature is increased to 860℃~900℃ at a heating rate of 2℃ / min~6℃ / min and the second insulation is carried out for 3.5h~6h.

[0057] The cooling process is as follows: after the second insulation is completed, the temperature in the heating device is cooled to 650℃~700℃ at a cooling rate of 0.5℃ / min~1.5℃ / min; then cooled to 450℃~500℃ at 3℃ / min~5℃ / min, and then cooled to 100℃~150℃ by furnace cooling, and the introduction of protective gas is stopped.

[0058] Step 3: The temperature in the heating device drops to the set temperature, the protective gas is stopped, and the temperature in the heating device is cooled to room temperature to obtain the electromagnetic pure iron material.

[0059] The pressure inside the heating device is 2300Pa~5000Pa.

[0060] The protective gas pressure in the heating device is constant.

[0061] The hardness of the electromagnetic pure iron after heat treatment is 1500HV-1700HV, the friction coefficient of the wear-resistant coating is 0.30-0.35, the coercive force of the wear-resistant coating is 22.5A / m-25.4A / m, and the magnetic permeability of the wear-resistant coating is 14.5mH / m-16.3mH / m.

[0062] Example 1

[0063] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -1 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0064] S2, introduce protective gases 500sccm of hydrogen and 450sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 2300Pa; start the heating program and heat up to 500℃ at a rate of 3℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature stage is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 720℃ at a heating rate of 2℃ / min and keep warm for 30min; further increase the temperature and keep warm, so that the grains can grow fully and evenly, the internal stress is further reduced, the soft magnetic properties are further improved, the coercive force is further reduced and the maximum magnetic permeability is further increased.

[0065] S3, after the insulation is completed, the temperature is increased to 860℃ at a heating rate of 2℃ / min and kept warm for 3.5h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0066] S4, after the insulation is completed, the temperature is lowered to 650℃ at a cooling rate of 0.5℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0067] S5, and then cool down to 450℃ at 3℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0068] S6, after cooling to 450°C, adopt furnace cooling to 100°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0069] Test: The hardness, friction coefficient and magnetic properties of the electromagnetic pure iron material coated with a wear-resistant coating after heat treatment obtained in Example 1 were compared with the electromagnetic pure iron material coated with a wear-resistant coating on the surface without heat treatment. The test results are as follows: Figure 2-6 shown. Figure 2This is a schematic diagram of the heat treatment process curve for electromagnetic pure iron materials. The heat treatment process includes controllable heating, insulation and cooling processes under a certain vacuum degree and with hydrogen and nitrogen as protective gases.

[0070] Hardness test:

[0071] Method: A comparative test was conducted on the hardness of an electromagnetic pure iron material coated with a wear-resistant coating on the surface after heat treatment obtained in Example 1 and an electromagnetic pure iron material coated with a wear-resistant coating on the surface without heat treatment.

[0072] Coating hardness test method: Use MVS-1000D1 digital microhardness tester to test hardness, diamond indenter, load 300mN, hold pressure for 10s, measure 8 points and take the average value of the results.

[0073] Results: Figure 3 The hardness of the electromagnetic pure iron material coated with a wear-resistant coating on the surface after heat treatment is 1700 HV.

[0074] Friction performance test:

[0075] Method: The friction performance of the electromagnetic pure iron material coated with a wear-resistant coating on the surface after heat treatment obtained in Example 1 is compared with the friction performance of the electromagnetic pure iron material coated with a wear-resistant coating on the surface without heat treatment.

[0076] Friction performance test method: Rtec friction and wear tester was used to test the wear resistance of the sample. Test mode: 6mm SiC ball was used to perform XY bidirectional linear non-lubricated reciprocating friction on the sample at room temperature. The specific test parameters were: normal load 5-20N, friction speed 20mm / s, friction distance 5mm, time 20min, frequency 2Hz. Each sample was tested 3 times and the average value of the results was taken.

[0077] Results: Figure 4 The friction coefficient of the electromagnetic pure iron material with the surface coated with the wear-resistant coating after heat treatment is 0.30.

[0078] Magnetic properties test:

[0079] Method: The magnetic properties (coercive force Hc, maximum magnetic permeability μm) of the electromagnetic pure iron material coated with a wear-resistant coating after heat treatment obtained in Example 1 are compared with the same electromagnetic pure iron material coated with a wear-resistant coating but not heat treated.

[0080] Magnetic property test method: A magnetic property tester is used to detect the coercive force Hc and the maximum magnetic permeability μm of the electromagnetic pure iron material with a wear-resistant coating on the surface after heat treatment.

[0081] Results: Figure 5The coercive force Hc of the electromagnetic pure iron material with the surface coated with the wear-resistant coating after heat treatment is 22.5 A / m.

[0082] like Figure 6 The maximum magnetic permeability μm of the electromagnetic pure iron material with the surface coated with the wear-resistant coating after heat treatment is 16.3 mH / m.

[0083] Example 2

[0084] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -1 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0085] S2, introduce protective gases 600sccm of hydrogen and 400sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 3000Pa; start the heating program and heat up to 520℃ at a rate of 4℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 770℃ at a heating rate of 3℃ / min and keep warm for 35min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0086] S3, after the insulation is completed, the temperature is increased to 870℃ at a heating rate of 3℃ / min and kept for 4h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0087] S4, after the insulation is completed, the temperature is lowered to 670℃ at a cooling rate of 0.7℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface of the electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal structure of the electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0088] S5, and then cool down to 470℃ at 5℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0089] S6, after cooling to 470°C, adopt furnace cooling to 100°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, so as to achieve the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0090] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1500HV; the friction coefficient of the coating is 0.35; the coercive force Hc of the coating is 25.4A / m; and the maximum magnetic permeability μm of the coating is 14.5mH / m.

[0091] Example 3

[0092] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -1 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0093] S2, introduce protective gases 550sccm of hydrogen and 500sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 2500Pa; start the heating program and heat up to 530℃ at a rate of 5℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 780℃ at a heating rate of 5℃ / min and keep warm for 35min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0094] S3, after the insulation is completed, the temperature is increased to 880℃ at a heating rate of 4℃ / min and kept for 4h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0095] S4, after the insulation is completed, the temperature is lowered to 680℃ at a cooling rate of 0.8℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0096] S5, and then cool down to 480℃ at 4℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0097] S6, after cooling to 480°C, adopt furnace cooling to 120°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, so as to achieve the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0098] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1593HV; the friction coefficient of the coating is 0.34; the coercive force Hc of the coating is 25.1A / m; and the maximum magnetic permeability μm of the coating is 14.9mH / m.

[0099] Example 4

[0100] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -1 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0101] S2, introduce protective gases 600sccm of hydrogen and 550sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 3000Pa; start the heating program and heat up to 550℃ at a rate of 5℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 800℃ at a heating rate of 5℃ / min and keep warm for 35min; further increase the temperature and keep warm, so that the grains can grow fully and evenly, the internal stress is further reduced, the soft magnetic properties are further improved, the coercive force is further reduced and the maximum magnetic permeability is further increased.

[0102] S3, after the insulation is completed, the temperature is increased to 900℃ at a heating rate of 4℃ / min and kept for 4h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0103] S4, after the insulation is completed, the temperature is lowered to 690℃ at a cooling rate of 1.2℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface of the electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal structure of the electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0104] S5, and then cool down to 500℃ at 4℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating and the stress state of the base electromagnetic pure iron are balanced as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0105] S6, after cooling to 500°C, adopt furnace cooling to 120°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0106] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1579HV; the friction coefficient of the coating is 0.32; the coercive force Hc of the coating is 24.7A / m; and the maximum magnetic permeability μm of the coating is 15.1mH / m.

[0107] Example 5

[0108] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -1 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0109] S2, introduce protective gases 700sccm of hydrogen and 600sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 4000Pa; start the heating program and heat up to 550℃ at a rate of 7℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 820℃ at a heating rate of 5℃ / min and keep warm for 60min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0110] S3, after the insulation is completed, the temperature is increased to 900℃ at a heating rate of 6℃ / min and kept for 6h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0111] S4, after the insulation is completed, the temperature is lowered to 680℃ at a cooling rate of 1.5℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface of the electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of the electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0112] S5, and then cool down to 460℃ at 5℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0113] S6, after cooling to 500°C, adopt furnace cooling to 150°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized or stressed, thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0114] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1660HV; the friction coefficient of the coating is 0.32; the coercive force Hc of the coating is 23.5A / m; and the maximum magnetic permeability μm of the coating is 15.5mH / m.

[0115] Example 6

[0116] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -2 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0117] S2, introduce protective gases 600sccm of hydrogen and 700sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 2000Pa; start the heating program and heat up to 500℃ at a rate of 3℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 720℃ at a heating rate of 6℃ / min and keep warm for 20min; further increase the temperature and keep warm, so that the grains can grow fully and evenly, the internal stress is further reduced, the soft magnetic properties are further improved, the coercive force is further reduced and the maximum magnetic permeability is further increased.

[0118] S3, after the insulation is completed, the temperature is increased to 860℃ at a heating rate of 3℃ / min and kept for 3h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0119] S4, after the insulation is completed, the temperature is lowered to 700℃ at a cooling rate of 0.5℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0120] S5, and then cool down to 450℃ at 3℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0121] S6, after cooling to 450°C, adopt furnace cooling to 100°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0122] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1675HV; the friction coefficient of the coating is 0.33; the coercive force Hc of the coating is 23.2A / m; and the maximum magnetic permeability μm of the coating is 15.6mH / m.

[0123] Example 7

[0124] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -2 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0125] S2, introduce protective gases 700sccm of hydrogen and 500sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 2500Pa; start the heating program and heat up to 520℃ at a rate of 4℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 770℃ at a heating rate of 3℃ / min and keep warm for 35min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0126] S3, after the insulation is completed, the temperature is increased to 870℃ at a heating rate of 4℃ / min and kept for 4h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0127] S4, after the insulation is completed, the temperature is lowered to 690℃ at a cooling rate of 0.7℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0128] S5, and then cool down to 470℃ at 3℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating is balanced with the stress state of the base electromagnetic pure iron as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0129] S6, after cooling to 470°C, adopt furnace cooling to 120°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, so as to achieve the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0130] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1682HV; the friction coefficient of the coating is 0.34; the coercive force Hc of the coating is 24.4A / m; and the maximum magnetic permeability μm of the coating is 15.2mH / m.

[0131] Example 8

[0132] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -2 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0133] S2, introduce protective gases 600sccm of hydrogen and 700sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 3000Pa; start the heating program and heat up to 530℃ at a rate of 5℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 790℃ at a heating rate of 5℃ / min and keep warm for 45min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0134] S3, after the insulation is completed, the temperature is increased to 880℃ at a heating rate of 5℃ / min and kept for 5h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0135] S4, after the insulation is completed, the temperature is lowered to 680℃ at a cooling rate of 1.0℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface coating of electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal organizational structure of electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0136] S5, and then cool down to 490℃ at 4℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating and the stress state of the base electromagnetic pure iron are balanced as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0137] S6, after cooling to 490°C, adopt furnace cooling to 130°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0138] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1688HV; the friction coefficient of the coating is 0.32; the coercive force Hc of the coating is 23.1A / m; and the maximum magnetic permeability μm of the coating is 15.7mH / m.

[0139] Example 9

[0140] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -2 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0141] S2, introduce protective gases 500sccm of hydrogen and 800sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 4000Pa; start the heating program and heat up to 540℃ at a rate of 6℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 810℃ at a heating rate of 5℃ / min and keep warm for 50min; further increase the temperature and keep warm, the grain growth can be sufficient and uniform, the internal stress can be further reduced, the soft magnetic properties can be further improved, the coercive force can be further reduced, and the maximum magnetic permeability can be further increased.

[0142] S3, after the insulation is completed, the temperature is increased to 890℃ at a heating rate of 5℃ / min and kept for 4h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0143] S4, after the insulation is completed, the temperature is lowered to 670℃ at a cooling rate of 1.3℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface of the electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal structure of the electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0144] S5, and then cool down to 460℃ at 4℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating and the stress state of the base electromagnetic pure iron are balanced as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0145] S6, after cooling to 460°C, adopt furnace cooling to 130°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is under vacuum reduction conditions, and the coating will not be oxidized, stress concentrated, etc., thereby ensuring that the hardness and wear resistance of the coating will not be reduced, so as to achieve the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0146] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1684HV; the friction coefficient of the coating is 0.33; the coercive force Hc of the coating is 23.2A / m; and the maximum magnetic permeability μm of the coating is 15.8mH / m.

[0147] Example 10

[0148] S1, the electromagnetic pure iron material coated with CVD TiN wear-resistant coating on the surface is placed in a vacuum heat treatment furnace, and the vacuum system is turned on to pre-evacuate the vacuum furnace, and the vacuum degree is 10 -2 Pa; High vacuum conditions can prevent the wear-resistant coating on the surface of electromagnetic pure iron from oxidizing, and prevent oxygen from penetrating into the electromagnetic pure iron matrix to cause matrix oxidation, which will have a negative impact on the magnetic properties of electromagnetic pure iron.

[0149] S2, introduce protective gases 600sccm of hydrogen and 900sccm of nitrogen respectively, and maintain the pressure in the vacuum heat treatment furnace at 5000Pa; start the heating program and heat up to 550℃ at a rate of 7℃ / min; the presence of protective gas can make the electromagnetic pure iron material heated more evenly; the heating rate in the low temperature section is faster, the grain growth rate is faster, the grain boundaries are reduced, the stress is reduced, and the coercive force is reduced; then heat up to 820℃ at a heating rate of 6℃ / min and keep warm for 60min; further increase the temperature and keep warm, so that the grains can grow fully and evenly, the internal stress is further reduced, the soft magnetic properties are further improved, the coercive force is further reduced and the maximum magnetic permeability is further increased.

[0150] S3, after the insulation is completed, the temperature is increased to 900℃ at a heating rate of 6℃ / min and kept for 6h; the high temperature stage is slowly heated and kept warm, which can fully release the internal stress of the wear-resistant coating on the surface of the electromagnetic pure iron, and at the same time make the internal structure of the electromagnetic pure iron more balanced, reduce the internal stress to the minimum, further reduce the coercive force, and increase the maximum magnetic permeability to the maximum value.

[0151] S4, after the insulation is completed, the temperature is lowered to 650℃ at a cooling rate of 1.5℃ / min; slow cooling can prevent stress concentration and coating cracking on the surface of the electromagnetic pure iron caused by rapid cooling; at the same time, it can prevent drastic changes in the internal structure of the electromagnetic pure iron, and the structural changes are smooth and slow, and the impact on its magnetic properties is minimized.

[0152] S5, and then cool down to 500℃ at 5℃ / min; the cooling rate in the low temperature section is accelerated to prevent the dispersion strengthening effect caused by the precipitation of dispersed phases in the matrix, which may lead to lattice distortion and reduced magnetic properties; at the same time, the stress state of the surface wear-resistant coating and the stress state of the base electromagnetic pure iron are balanced as soon as possible, thereby minimizing the impact on the magnetic properties of the electromagnetic pure iron.

[0153] S6, after cooling to 500°C, adopt furnace cooling to 150°C, stop introducing hydrogen and nitrogen until cooling to room temperature, and obtain the electromagnetic pure iron material with wear-resistant coating on the surface after heat treatment. The pressure of hydrogen and nitrogen in the vacuum heat treatment furnace is kept constant, so that the surface of the electromagnetic pure iron with wear-resistant coating is placed under vacuum reduction conditions, and the coating will not be oxidized or stressed, thereby ensuring that the hardness and wear resistance of the coating will not be reduced, thereby achieving the balance of hardness, wear resistance and magnetic properties of the electromagnetic pure iron material with wear-resistant coating on the surface.

[0154] The results show that the hardness of the electromagnetic pure iron with the wear-resistant coating on the surface after heat treatment is 1689HV; the friction coefficient of the coating is 0.32; the coercive force Hc of the coating is 23.0A / m; and the maximum magnetic permeability μm of the coating is 15.9mH / m.

[0155] Comparative Examples 1-5

[0156] An electromagnetic pure iron material with a surface coated with a wear-resistant coating is prepared under a heat treatment process different from that of the electromagnetic pure iron material with a surface coated with a wear-resistant coating in Example 1.

[0157] The electromagnetic pure iron materials with surface coatings of wear-resistant coatings as described in Comparative Examples 1-5 were prepared in a similar manner to Example 1, except that the parameters in the coating preparation process as shown in Table 1 were changed, and the hardness, friction coefficient and magnetic properties of the materials were measured.

[0158] Table 1 Electromagnetic pure iron materials with surface coating of wear-resistant coating under heat treatment process different from that in Example 1

[0159]

[0160] It can be seen from Table 1 that the hardness of the electromagnetic pure iron material with a wear-resistant coating on the surface prepared by the heat treatment process adopted in the embodiment (the material hardness of 1500HV in Example 2) is significantly greater than the hardness of the electromagnetic pure iron material with a wear-resistant coating on the surface in Comparative Examples 1-5 (such as the material hardness of 1270HV in Comparative Example 5).

[0161] It can be seen from Table 1 that the friction coefficient of the electromagnetic pure iron material with a wear-resistant coating on the surface prepared by the heat treatment process used in the embodiment (the friction coefficient of the material in Example 2 is 0.35) is significantly smaller than the hardness of the electromagnetic pure iron material with a wear-resistant coating on the surface in Comparative Examples 1-5 (such as the friction coefficient of the material in Comparative Example 1 is 0.41).

[0162] It can be seen from Table 1 that the coercive force of the electromagnetic pure iron material with a surface coated with a wear-resistant coating prepared by the heat treatment process adopted in the embodiment (material Hc=25.4A / m in Example 2) is significantly smaller than the coercive force of the electromagnetic pure iron material with a surface coated with a wear-resistant coating in Comparative Examples 1-5 (such as material Hc=29.5A / m in Comparative Example 1).

[0163] It can be seen from Table 1 that the maximum magnetic permeability of the electromagnetic pure iron material with a surface coated with a wear-resistant coating prepared by the heat treatment process used in the embodiment (material μm=14.5mH / m in Example 2) is significantly greater than the maximum magnetic permeability of the electromagnetic pure iron material with a surface coated with a wear-resistant coating in Comparative Examples 1-5 (such as the material hardness material μm=12.7mH / m in Comparative Example 3).

[0164] Therefore, compared with comparative examples 1-5, the electromagnetic pure iron material with a surface coated with a wear-resistant coating prepared by the heat treatment process described in Example 1 of the present invention has excellent hardness, friction resistance and magnetic properties.

[0165] The heat treatment method of an electromagnetic pure iron material coated with a wear-resistant coating on its surface described in the present invention can not only prevent the surface oxidation of the electromagnetic pure iron after coating through a vacuum heat treatment process under hydrogen + nitrogen conditions, but also reduce the adverse effects of abnormal grain growth, structural deformation, increased internal stress, etc. on the electromagnetic pure iron caused by the coating process under high temperature conditions, which lead to a serious decrease in the magnetic properties of the electromagnetic pure iron; effectively improve the magnetic properties of the electromagnetic pure iron material after coating, such as the coercive force and maximum magnetic permeability, and maintain the high hardness and strong wear resistance of the electromagnetic pure iron after coating, and finally obtain an electromagnetic pure iron material with good magnetic properties, high hardness and strong wear resistance, thereby further expanding its application field.

[0166] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A heat treatment method for electromagnetic pure iron material with a wear-resistant coating on the surface, characterized in that: The following steps are involved: Placing electromagnetic pure iron with a wear-resistant coating on the surface into a heating device; A protective gas is introduced into the heating device to perform heating, heat preservation and temperature reduction treatments in sequence; The temperature in the heating device drops to the set temperature, the protective gas is stopped, and the temperature in the heating device is cooled to room temperature to obtain the electromagnetic pure iron material.

2. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1 is characterized in that: The wear-resistant coating is a TiN coating, which is prepared by a chemical vapor deposition method.

3. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1 is characterized in that: The heating device is a vacuum heat treatment furnace, and the vacuum degree of the vacuum heat treatment furnace is 10 -1 Pa~10 -2 Pa.

4. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1 is characterized in that: The protective gases are hydrogen and nitrogen; the hydrogen flow rate is 450 sccm to 700 sccm, and the nitrogen flow rate is 450 sccm to 700 sccm.

5. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1 is characterized in that: The heating and insulation process is as follows: the temperature in the heating device is increased to 500℃~550℃ at a rate of 3℃ / min~7℃ / min, and then the temperature is increased to 720℃~820℃ at a heating rate of 2℃ / min~6℃ / min and the first insulation is carried out for 30min~60min; after the first insulation, the temperature is increased to 860℃~900℃ at a heating rate of 2℃ / min~6℃ / min and the second insulation is carried out for 3.5h~6h.

6. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 5, characterized in that: The cooling process is as follows: after the second insulation is completed, the temperature in the heating device is cooled to 650℃~700℃ at a cooling rate of 0.5℃ / min~1.5℃ / min; then cooled to 450℃~500℃ at 3℃ / min~5℃ / min, and then cooled to 100℃~150℃ by furnace cooling, and the introduction of protective gas is stopped.

7. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1 is characterized in that: The pressure inside the heating device is 2300Pa~5000Pa.

8. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1, characterized in that: The protective gas pressure in the heating device is constant.

9. The heat treatment method of electromagnetic pure iron material with a wear-resistant coating on the surface according to claim 1, characterized in that: The hardness of the electromagnetic pure iron after heat treatment is 1500HV-1700HV, the friction coefficient of the wear-resistant coating is 0.30-0.35, the coercive force of the wear-resistant coating is 22.5A / m-25.4A / m, and the magnetic permeability of the wear-resistant coating is 14.5mH / m-16.3mH / m.

10. An electromagnetic pure iron material, characterized in that: The electromagnetic pure iron material with a surface coated with a wear-resistant coating is prepared by the heat treatment method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for improving magnetic performance of neodymium-iron-boron magnetic material

    CN106876072A

  • Low-carbon steel low temperature annealing magnetic heat treatment technology

    CN111763806A

  • Vacuum annealing method for magnetic material

    CN112359186A

  • Corrosion-resistant titanium nitride wear-resistant coating, preparation method thereof and product comprising coating

    CN113235069A

  • Method and apparatus for providing a conductive, amorphous non-stick coating