Infrared detector and manufacturing method thereof
By using InGaAsSb material without AlSb as the barrier layer and InAs/InAsSb superlattice as the absorption layer in an infrared detector, combined with the MOCVD process, the problems of high oxidation difficulty and cost in the prior art are solved, and efficient Infrared detector preparation reduces the dark current and production costs of the device.
Patent Information
- Application Number
- CN202411507907.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing InAs/InAsSb superlattice infrared detectors have problems of difficulty and high cost in growth and processing, which limits their large-scale application promotion.
An infrared detector was prepared by a metal organic chemical vapor deposition (MOCVD) process using N-type InGaAsSb material without AlSb as the electron barrier layer, and an N-type InGaAs/InAsSb or N-type InGaAs/InAsSb superlattice as the absorbing layer. The bandwidth of the barrier layer is achieved is greater than that of the absorbing layer and the valence band is flush.
It effectively reduces the dark current of the device, improves stability and reliability, reduces the difficulty of material growth and processing, and prepares MOCVD through mainstream industrial methods, significantly reduces costs and improves yield.
Smart Images

Figure CN119050181A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of optoelectronic technology, and in particular, relates to an infrared detector and a manufacturing method thereof. Background Art
[0002] Infrared radiation detection is an important part of infrared technology and is widely used in thermal imaging, satellite remote sensing, gas monitoring, optical communications, spectral analysis and other fields. Antimonide type II superlattice infrared detectors are considered to be one of the most ideal choices for preparing third-generation infrared detectors due to their good uniformity, low Auger recombination rate, and large wavelength adjustment range. They have now entered the mass production stage.
[0003] There are two main types of antimonide type II superlattices, one is InAs / GaSb superlattice, and the other is InAs / InAsSb superlattice. InAs / InAsSb superlattice has a long minority carrier lifetime, low dark current, and simple growth, which has certain advantages over InAs / GaSb superlattice, especially in the medium-wave detection band (3~5 microns). However, InAs / InAsSb superlattice must be combined with an electron barrier layer to achieve high performance. An ideal electron barrier refers to a barrier for electron transport at the interface of the two materials while hole transport is unimpeded, which requires that the bandwidth of the barrier is larger than the absorption zone, and the barrier valence band is flush with the absorption zone.
[0004] In the prior art, the electron barriers of InAs / InAsSb superlattices are all materials containing AlSb, such as AlAsSb, AlGaAsSb or AlAsSb / InAsSb superlattices. However, Al-containing materials are very easy to oxidize, which increases the difficulty of growing and processing infrared detectors and affects the stability of the device. Moreover, materials containing AlSb are difficult to prepare by metal organic chemical vapor deposition (MOCVD), the mainstream material growth method in the industry, and can only be prepared by molecular beam epitaxy (MBE), which is costly and limits its large-scale application and promotion. Summary of the invention
[0005] In order to solve the technical problems existing in the above-mentioned prior art, an infrared detector based on InAs / InAsSb superlattice but with a barrier layer free of AlSb and grown by MOCVD and a method for manufacturing the same are provided according to an embodiment of the present invention.
[0006] According to one aspect of an embodiment of the present invention, the absorption layer of the infrared detector provided is an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice, and the barrier layer of the infrared detector is an N-type InGaAsSb material.
[0007] In an example of the infrared detector provided in the above aspect, the bandwidth of the barrier layer is greater than the bandwidth of the absorption layer, and the valence band of the barrier layer is flush with the valence band of the absorption layer.
[0008] In an example of the infrared detector provided in the above aspect, the infrared detector also includes a substrate, a first contact layer, a second contact layer, a first electrode and a second electrode; wherein the first contact layer, the absorption layer, the barrier layer, and the second contact layer are stacked in sequence on the substrate in a direction away from the substrate, the first electrode is in contact with the first contact layer, and the second electrode is arranged on the second contact layer.
[0009] In an example of the infrared detector provided in the above aspect, the absorption layer, the barrier layer and parts of the second contact layer are etched away to form a mesa structure exposing the first contact layer, and the first electrode is arranged on the exposed first contact layer.
[0010] In an example of the infrared detector provided in the above aspect, the substrate is an N-type InAs substrate or an N-type GaSb substrate, and / or the first contact layer is an N-type InAs material or an N-type InAsSb material, and / or the second contact layer is a P-type InGaAsSb material or an N-type InAs / InAsSb superlattice.
[0011] According to another aspect of an embodiment of the present invention, a method for manufacturing an infrared detector includes: using N-type InAs / InAsSb superlattice or N-type InGaAs / InAsSb superlattice to form an absorption layer of the infrared detector; using N-type InGaAsSb material to form a barrier layer of the infrared detector.
[0012] In an example of the method for manufacturing an infrared detector provided in the above another aspect, a bandwidth of the barrier layer is greater than a bandwidth of the absorption layer, and a valence band of the barrier layer is flush with a valence band of the absorption layer.
[0013] In an example of a method for manufacturing an infrared detector provided in the above-mentioned other aspect, before forming the absorption layer, the manufacturing method further includes: forming a first contact layer on a substrate; using an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice to form the absorption layer of the infrared detector, specifically including: using an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice to form the absorption layer on the first contact layer; using an N-type InGaAsSb material to form a barrier layer of the infrared detector, specifically including: using an N-type InGaAsSb material to form the barrier layer on the absorption layer; after forming the barrier layer, the manufacturing method further includes: forming a second contact layer on the barrier layer; forming a first electrode in contact with the first contact layer, and forming a second electrode on the second contact layer.
[0014] In an example of a method for manufacturing an infrared detector provided in the above-mentioned other aspect, the forming of a first electrode in contact with the first contact layer and the forming of a second electrode on the second contact layer specifically include: partially etching the second contact layer, the barrier layer and the absorption layer to form a mesa structure exposing the first contact layer; depositing a first electrode on the exposed first contact layer, and depositing a second electrode on the second contact layer.
[0015] In an example of a method for manufacturing an infrared detector provided in the above-mentioned other aspect, the substrate is an N-type InAs substrate or an N-type GaSb substrate, and / or the first contact layer is an N-type InAs material or an N-type InAsSb material, and / or the second contact layer is a P-type InGaAsSb material or an N-type InAs / InAsSb superlattice.
[0016] Beneficial effects: The infrared detector according to the embodiment of the present invention uses InGaAsSb material as the electron barrier layer of the In(Ga)As / InAsSb superlattice absorption layer, which can achieve an effect similar to that of the AlSb barrier layer and can effectively reduce the dark current of the device. Furthermore, the infrared detector according to the embodiment of the present invention does not contain Al at all, thus avoiding the oxidation of Al-containing materials, and the device structure only contains four elements, In, Ga, As, and Sb, which has a simple structure, reduces the difficulty of material growth and processing, and improves the stability and reliability of the device. Furthermore, the infrared detector according to the embodiment of the present invention can be prepared using the mainstream material growth method MOCVD in the industry, which can significantly reduce costs and improve yields compared to the conventional preparation method MBE of antimonide detectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The above and other aspects, features and advantages of the embodiments of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which: Figure 1 is a schematic structural diagram of an infrared detector according to an embodiment of the present invention; Figure 2 The InGaAsSb barrier layer and the InGaAs / InAsSb superlattice absorption layer of the infrared detector according to the embodiment of the present invention, and the conduction band of the InAs and GaSb materials are E C and valence band E V Schematic diagram of relative position comparison; Figure 3 is a schematic diagram comparing dark current data of 77K of a specific example of an infrared detector according to an embodiment of the present invention and dark current data of a traditional infrared detector; Figures 4a to 4d 4 is a process diagram of an infrared detector according to an embodiment of the present invention. DETAILED DESCRIPTION
[0018] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.
[0019] As used herein, the term "including" and its variations represent open terms, meaning "including but not limited to". The terms "based on", "according to", etc. mean "based at least in part on", "based at least in part on". The terms "embodiment", "one example", "one embodiment" and "an embodiment" mean "at least one embodiment". The terms "another embodiment", "another embodiment", "another example", "yet another example" mean "at least one other embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other definitions may be included below, whether explicit or implicit. Unless the context clearly indicates otherwise, the definition of a term is consistent throughout the specification.
[0020] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the solutions according to the present invention are shown in the drawings, while other details that are not very relevant are omitted.
[0021] As described in the background technology, existing infrared detectors based on In(Ga)As / InAsSb superlattice all use materials containing AlSb, such as AlAsSb, AlGaAsSb or AlAsSb / InAsSb superlattice. Since Al-containing materials are very easy to oxidize, this increases the difficulty of growing and processing infrared detectors and affects the stability of the device. Moreover, materials containing AlSb are difficult to prepare by MOCVD, the mainstream material growth method in the industry, and can only be prepared by MBE, which has high cost and low yield, limiting its large-scale application and promotion.
[0022] Therefore, in order to solve the above technical problems, an infrared detector and a method for manufacturing the same are provided according to an embodiment of the present invention. In the infrared detector, an Al-free InGaAsSb material is used as an electron barrier layer, and an InAs / InAsSb superlattice or an InGaAs / InAsSb superlattice is used as an absorption layer. The core idea of the present invention is as follows: Figure 2 See Figure 2 , InAs and GaSb form a type II energy band arrangement, that is, the valence band of GaSb ( E V ) is higher than the conduction band of InAs ( E C ); On the other hand, In(Ga)As / InAsSb superlattice will form microstrips (such as Figure 2 According to the principle of quantum mechanics, the superlattice microstrip E V It must be in InAs E V and GaSb E V Due to the valence band of InGaAsSb bulk material E V From InAs E V to GaSb E V Through continuous adjustment, the valence band can be aligned with the valence band of the In(Ga)As / InAsSb superlattice absorption layer, and the effective bandwidth can be larger than the effective bandwidth of the In(Ga)As / InAsSb superlattice, thereby realizing an ideal electron barrier.
[0023] Therefore, according to an embodiment of the present invention, an Al-free In(Ga)As / InAsSb antimonide superlattice infrared detector is provided. The InGaAsSb electron barrier can effectively suppress dark current, and there are only four elements, In, Ga, As, and Sb, in the device structure. The structure is simple, which reduces the difficulty of material growth and processing and improves the stability and reliability of the device.
[0024] The structure of the infrared detector according to the embodiment of the present invention is described in detail below. Figure 1 is a schematic structural diagram of an infrared detector according to an embodiment of the present invention.
[0025] See also Figure 1 As shown, the infrared detector according to an embodiment of the present invention includes: a substrate 10; a first contact layer 11, an absorption layer 12, a barrier layer 13 and a second contact layer 14 stacked on the substrate 10 from bottom to top (that is, stacked in sequence in a direction away from the substrate 10); a first electrode 15 and a second electrode 16, the first electrode 15 is in contact with the first contact layer 11, and the second electrode 16 is arranged on the second contact layer 14.
[0026] In one example, the substrate 10 may be an N-type InAs substrate or an N-type GaSb substrate.
[0027] In one example, the first contact layer 11 may be made of N-type InAs or N-type InAsSb material, the thickness of the first contact layer 11 may be 0.2 µm to 0.5 µm, the doping source may be Si or Te, and the doping concentration may be 1×10 18 cm -3 ~1×10 19 cm -3 .
[0028] In one example, the absorption layer 12 may be an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice, the thickness of the absorption layer 12 may be 2µm to 5µm, the doping source may be Si or Te, and the doping concentration may be 1×10 15 cm -3 ~1×10 17 cm -3 , the corresponding bandwidth can be 0.2eV~0.3eV.
[0029] In one example, the barrier layer 13 may be made of N-type InGaAsSb material, the thickness of the barrier layer 13 may be 0.1 μm to 0.5 μm, the doping source may be Si or Te, and the doping concentration may be 1×10 15 cm -3 ~1×10 17 cm -3 , the corresponding bandwidth can be 0.4eV~0.6eV.
[0030] In one example, the second contact layer 14 may be a P-type InGaAsSb material or an N-type InAs / InAsSb superlattice, the thickness of the second contact layer 14 may be 0.2 μm to 0.5 μm, the doping source may be Zn, Be, Si or Te, and the doping concentration may be 1×10 18 cm -3 ~1×10 19 cm -3 , the corresponding bandwidth can be 0.2eV~0.6eV.
[0031] The energy band of the infrared detector according to the embodiment of the present invention is described in detail below. Existing infrared detectors based on In(Ga)As / InAsSb superlattice all use materials containing AlSb as barrier layers. In the infrared detector according to the embodiment of the present invention, InGaAsSb material is used as the electron barrier of the InGaAs / InAsSb superlattice. Its energy band arrangement and physical principle are as follows: Figure 2 shown.
[0032] Figure 2 The InGaAsSb barrier layer 13 and the InGaAs / InAsSb superlattice absorption layer 12 of the infrared detector according to the embodiment of the present invention, and the conduction band of the InAs and GaSb materials are E C and valence band E V Schematic diagram of relative position comparison.
[0033] Reference Figure 2 , In(Ga)As / InAsSb superlattice microstrip E V Position in InAs E V and GaSb E v The valence band of InGaAsSb material E V The position can be obtained from the InAs E V to GaSb E V Continuously adjustable, so that its valence band can be achieved E V In(Ga)As / InAsSb superlattice absorber layer E VThe effective bandwidth is greater than that of the In(Ga)As / InAsSb superlattice. In this way, the InGaAsSb material can serve as an ideal electron barrier for the InGaAs / InAsSb superlattice. Through the flexible combination of the absorption layer superlattice components and thickness, the absorption wavelength can be flexibly adjusted between 4 microns and 6 microns, covering the mid-wave infrared range.
[0034] Figure 3 77K dark current of a specific example of an infrared detector according to an embodiment of the present invention is compared with the dark current data of a traditional infrared detector. In a specific example of an infrared detector according to an embodiment of the present invention, the thickness of the InGaAs / InAsSb superlattice absorption layer 12 is 2µm, and the thickness of the InGaAsSb barrier layer 13 is 200nm. For comparison, an infrared detector is provided, which also uses the InGaAs / InAsSb superlattice for the absorption layer, but uses the AlGaAsSb material with a thickness of 200nm for the barrier layer. Figure 3 As shown, with the InGaAsSb barrier layer, the dark current at 77K is only 4.3×10 -9 A / cm 2 However, the traditional AlGaAsSb barrier layer has poor material quality, difficult to control the band alignment, and a dark current as high as 2.3×10 -3 A / cm 2 Therefore, it can be seen that the InGaAsSb barrier layer used in the present invention has a huge advantage over the traditional technology in suppressing dark current.
[0035] The manufacturing process of the infrared detector according to the embodiment of the present invention is described in detail below. Figures 4a to 4d 4 is a process diagram of an infrared detector according to an embodiment of the present invention.
[0036] Reference Figure 4a , providing a substrate 10. In one example, the substrate 10 can be an N-type InAs substrate or an N-type GaSb substrate.
[0037] Reference Figure 4b A first contact layer 11, an absorption layer 12, a barrier layer 13, and a second contact layer 14 are sequentially grown on the substrate 10 from bottom to top to form a stacked layer.
[0038] In one example, a metal organic chemical vapor deposition (MOCVD) process is used to sequentially grow a first contact layer 11, an absorption layer 12, a barrier layer 13, and a second contact layer 14 from bottom to top on the substrate 10. Specifically, metal organic chemical vapor deposition (MOCVD) is used as the growth process, and the growth sources are TMIn, TMGa, TMSb, and AsH 3, n-type doping source is SiH 4 , the p-type doping source is DEZn, the growth temperature is set to about 600°C, and the reaction chamber pressure is set to 200Torr. After the impurities on the surface of the substrate 10 are removed by high temperature treatment, the following are grown on the substrate 10 from bottom to top: (1) First contact layer 11. In one example, the first contact layer 11 is made of N-type InAs material, has a thickness of 0.2 µm, and is doped with Si at a doping concentration of 1×10 18 cm -3 .
[0039] (2) Absorption layer 12. In one example, the absorption layer 12 is an N-type InGaAs / InAsSb superlattice with a thickness of 2 µm and is doped with Si at a doping concentration of 5×10 15 cm -3 , corresponding to a bandwidth of 0.2 eV.
[0040] (3) Barrier layer 13. In one example, the barrier layer 13 is made of N-type InGaAsSb material with a thickness of 0.1 µm and is doped with Si at a doping concentration of 2×10 15 cm -3 , corresponding to a bandwidth of 0.4 eV.
[0041] (4) Second contact layer 14. In one example, the second contact layer 14 is made of P-type InGaAsSb material with a thickness of 0.2 µm and is doped with Zn at a doping concentration of 1×10 18 cm -3 , corresponding to a bandwidth of 0.6 eV.
[0042] Here, the MOCVD process is used as the growth process of the first contact layer 11, the absorption layer 12, the barrier layer 13, and the second contact layer 14, and the obtained infrared detector has a cutoff wavelength of about 6µm. Since the MOCVD process has large production capacity and low cost, the use of this process can reduce costs and improve the cost performance of infrared detectors.
[0043] In another example, a molecular beam epitaxy (MBE) process is used as a growth process, the growth sources are solid elemental sources Ga, In, As, and Sb, the n-type doping source is Te, and the growth temperature is about 400° C. After the substrate 10 is degassed and doped, the following are grown on the substrate 10 from bottom to top: (1) First contact layer 11. In one example, the first contact layer 11 is made of N-type InAsSb material with a thickness of 0.5 µm and is doped with Te at a doping concentration of 1×10 19 cm -3 .
[0044] (2) Absorption layer 12. In one example, the absorption layer 12 is an N-type InAs / InAsSb superlattice with a thickness of 5 µm and is doped with Te at a doping concentration of 1×10 17 cm -3 , corresponding to a bandwidth of 0.3 eV.
[0045] (3) Barrier layer 13. In one example, the barrier layer 13 is made of N-type InGaAsSb material with a thickness of 0.5 µm and is doped with Te at a doping concentration of 5×10 16 cm -3 , corresponding to a bandwidth of 0.6 eV.
[0046] (4) Second contact layer 14. In one example, the second contact layer 14 is an N-type InAs / InAsSb superlattice with a thickness of 0.5 µm and is doped with Te at a doping concentration of 1×10 19 cm -3 , corresponding to a bandwidth of 0.3 eV.
[0047] When the MBE process is used as the growth process, the cutoff wavelength of the obtained infrared detector is about 4µm. Since the MBE process can form a steep interface, the performance of the short-wave infrared detector obtained by this process is higher.
[0048] Reference Figure 4c , the second contact layer 14 , the barrier layer 13 , and the absorption layer 12 are partially etched to form a mesa structure A exposing the first contact layer 11 .
[0049] In one example, the second contact layer 14 , the barrier layer 13 , and the absorption layer 12 are partially etched by an inductively coupled plasma etching (ICP) process to expose the first contact layer 11 , thereby forming a mesa structure A.
[0050] In another example, the second contact layer 14 , the barrier layer 13 , and the absorption layer 12 are partially etched by a wet etching process to expose the first contact layer 11 , thereby forming a mesa structure A.
[0051] Reference Figure 4d , a first electrode 15 is deposited on the first contact layer 11 , and a second electrode 16 is deposited on the second contact layer 14 .
[0052] In one example, the first electrode 15 is deposited on the exposed first contact layer 11 by electron beam evaporation, and the second electrode 16 is deposited on the second contact layer 14. The first electrode 15 and the second electrode 16 are both a combination of Ti (500Å) / Pt (500Å) / Au (3000Å).
[0053] In another example, the first electrode 15 is deposited on the exposed first contact layer 11 by electron beam evaporation, and the second electrode 16 is deposited on the second contact layer 14. The first electrode 15 and the second electrode 16 are both a combination of Ti (200Å) / Pt (400Å) / Au (2000Å).
[0054] In summary, according to the infrared detector and its manufacturing method of the embodiments of the present invention, the device structure adopts the In(Ga)As / InAsSb superlattice absorption region, but the barrier layer does not contain Al at all, thus avoiding the oxidation of Al-containing materials. There are only four elements, In, Ga, As, and Sb, in the device structure. The structure is simple, which reduces the difficulty of material growth and processing, and can be prepared by MOCVD, the mainstream material growth method in the industry. Compared with the conventional preparation method MBE of antimonide detectors, it can greatly reduce costs and improve yields.
[0055] The terms "exemplary," "example," and the like used throughout this specification mean "used as an example, instance, or illustration" and do not mean "preferred" or "advantageous" over other embodiments. The detailed description includes specific details for the purpose of providing an understanding of the described techniques. However, these techniques can be implemented without these specific details. In some instances, in order to avoid obscuring the concepts of the described embodiments, well-known structures and devices are shown in block diagram form.
[0056] The optional implementation modes of the embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above implementation modes. Within the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all belong to the protection scope of the embodiments of the present invention.
[0057] The above description of the contents of this specification is provided to enable any person of ordinary skill in the art to implement or use the contents of this specification. Various modifications to the contents of this specification will be apparent to those of ordinary skill in the art, and the general principles defined herein may be applied to other variations without departing from the scope of protection of the contents of this specification. Therefore, the contents of this specification are not limited to the examples and designs described herein, but are consistent with the widest range of principles and novel features disclosed herein.
Claims
1. An infrared detector, It is characterized in that The absorption layer (12) of the infrared detector is an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice, and the barrier layer (13) of the infrared detector is an N-type InGaAsSb material.
2. The infrared detector according to claim 1, It is characterized in that The bandwidth of the barrier layer (13) is greater than the bandwidth of the absorption layer (12), and the valence band of the barrier layer (13) is flush with the valence band of the absorption layer (12).
3. The infrared detector according to claim 1 or 2, It is characterized in that The infrared detector further comprises a substrate (10), a first contact layer (11), a second contact layer (14), a first electrode (15) and a second electrode (16); wherein the first contact layer (11), the absorption layer (12), the barrier layer (13) and the second contact layer (14) are sequentially stacked on the substrate (10) in a direction away from the substrate (10), the first electrode (15) is in contact with the first contact layer (11), and the second electrode (16) is arranged on the second contact layer (14).
4. The infrared detector according to claim 3, It is characterized in that Parts of the absorption layer (12), the barrier layer (13) and the second contact layer (14) are etched away to form a mesa structure (A) exposing the first contact layer (11); the first electrode (15) is arranged on the exposed first contact layer (11).
5. The infrared detector according to claim 3, It is characterized in that The substrate (10) is an N-type InAs substrate or an N-type GaSb substrate, and / or the first contact layer (11) is an N-type InAs material or an N-type InAsSb material, and / or the second contact layer (14) is a P-type InGaAsSb material or an N-type InAs / InAsSb superlattice.
6. A method for manufacturing an infrared detector, It is characterized in that include: The absorption layer (12) of the infrared detector is formed by using an N-type InAs / InAsSb superlattice or an N-type InGaAs / InAsSb superlattice; The barrier layer (13) of the infrared detector is made of N-type InGaAsSb material.
7. The method for manufacturing the infrared detector according to claim 6, It is characterized in that The bandwidth of the barrier layer (13) is greater than the bandwidth of the absorption layer (12), and the valence band of the barrier layer (13) is flush with the valence band of the absorption layer (12).
8. The method for manufacturing the infrared detector according to claim 6 or 7, It is characterized in that Before forming the absorption layer (12), the manufacturing method further comprises: forming a first contact layer (11) on the substrate (10); The method of using N-type InAs / InAsSb superlattice or N-type InGaAs / InAsSb superlattice to form the absorption layer (12) of the infrared detector specifically comprises: using N-type InAs / InAsSb superlattice or N-type InGaAs / InAsSb superlattice to form the absorption layer (12) on the first contact layer (11); The method of using N-type InGaAsSb material to form the barrier layer (13) of the infrared detector specifically comprises: using N-type InGaAsSb material to form the barrier layer (13) on the absorption layer (12); After the barrier layer (13) is fabricated, the fabrication method further comprises: fabricating a second contact layer (14) on the barrier layer (13); forming a first electrode (15) in contact with the first contact layer (11), and depositing a second electrode (16) on the second contact layer (14).
9. The method for manufacturing the infrared detector according to claim 8, It is characterized in that The forming of a first electrode (15) in contact with the first contact layer (11), and forming a second electrode (16) on the second contact layer (14) specifically comprises: Partially etching the second contact layer (14), the barrier layer (13) and the absorption layer (12) to form a mesa structure (A) exposing the first contact layer (11); A first electrode (15) is deposited on the exposed first contact layer (11), and a second electrode (16) is deposited on the second contact layer (14).
10. The method for manufacturing the infrared detector according to claim 8, It is characterized in that The substrate (10) is an N-type InAs substrate or an N-type GaSb substrate, and / or the first contact layer (11) is an N-type InAs material or an N-type InAsSb material, and / or the second contact layer (14) is a P-type InGaAsSb material or an N-type InAs / InAsSb superlattice.
Citation Information
Patent Citations
Single-barrier type InGaAsSb infrared detector
CN105932092A
Mid-infrared vertical cavity laser
CN110959234A
Superlattice absorber for detector
CN113646906A
Infrared detector and manufacturing method thereof
CN116387381A
Superlattice material for infrared detection and infrared detector
CN118658910A
Cited By
Short-wave dual-band infrared detector based on indium phosphide substrate and preparation method of short-wave dual-band infrared detector
CN119907317A
Infrared detector and manufacturing method thereof
CN120152401A
Flexible InP-based semiconductor film structure and preparation method thereof