A lightweight ultra-low carbon magnesia-carbon brick, its preparation method and application
By preparing lightweight ultra-low carbon magnesia-carbon bricks, the problem of insufficient oxidation resistance and thermal shock stability of low carbon magnesia-carbon bricks is solved by utilizing elemental silicon, silicon carbide and intermetallic compound reinforcing phases in silicon wire cutting waste. This achieves lightweighting and high-value utilization of waste materials, making it suitable for modern high-temperature industries.
Patent Information
- Application Number
- CN202611211926.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing low-carbon magnesia-carbon bricks have poor oxidation resistance, insufficient thermal shock stability, and large self-weight, making it difficult to achieve high-value utilization of silicon wire cutting waste and failing to meet the energy-saving, long-life, and environmental protection requirements of modern high-temperature industries.
Lightweight ultra-low carbon magnesia-carbon bricks are prepared by using fused magnesia particles, porous magnesia aggregate, and pretreated silicon wire cutting waste as raw materials, combined with phenolic resin as a binder, and through heat treatment. The elemental silicon, silicon carbide, and intermetallic compounds in the silicon wire cutting waste are used to form SiO2, MgSiO3, and SiC reinforcing phases, which fill the pores of the brick body, replace traditional additives, and optimize the microstructure.
It significantly improves the oxidation resistance and thermal shock stability of ultra-low carbon magnesia-carbon bricks, achieves lightweighting, reduces self-weight, is suitable for modern steel smelting and refining processes, realizes the high-value utilization of silicon wire cutting waste, and has significant economic and environmental benefits.
Abstract
Description
Technical Field
[0001] This invention relates to the field of refractory materials technology, and in particular to a lightweight ultra-low carbon magnesia-carbon brick, its preparation method, and its application. Background Technology
[0002] With the global energy structure shifting towards cleaner and lower-carbon energy, the photovoltaic industry has experienced explosive growth. Crystalline silicon solar cells, with their high conversion efficiency and stable performance, occupy more than 90% of the photovoltaic market share. During the diamond wire cutting process of crystalline silicon rods, a large amount of silicon wire cutting waste is generated. This waste mainly consists of elemental silicon, silicon carbide, silicon dioxide, and a small amount of ferric oxide. According to industry statistics, approximately 3-5 tons of silicon cutting waste are generated for every 1MW of photovoltaic modules produced, and my country's annual silicon cutting waste emissions exceed one million tons. Direct dumping, landfilling, or incineration of this solid waste not only results in the loss of valuable resources such as high-purity silicon but also pollutes soil, water, and air, causing serious environmental pressure and becoming a key bottleneck restricting the green development of the photovoltaic industry. Therefore, achieving high-value and resource-based utilization of silicon cutting waste has become a research hotspot of common concern in the photovoltaic and materials fields.
[0003] Magnesia-carbon refractories, combining the high refractoriness of magnesium oxide with the excellent thermal conductivity and slag erosion resistance of graphite, are core refractory materials for equipment used in high-temperature industries such as steel smelting and refining. Traditional magnesia-carbon bricks typically contain 10%–20% carbon. While offering excellent performance, they are prone to carburizing into molten steel during the smelting of high-quality clean steel, reducing the steel's cleanliness and failing to meet the requirements of high-end steel production. Ultra-low carbon magnesia-carbon bricks (carbon content ≤3%) effectively solve the carburization problem, becoming the preferred refractory material for high-quality steel smelting. However, the reduced carbon content leads to a series of performance defects in ultra-low carbon magnesia-carbon bricks: firstly, a significant decrease in oxidation resistance, with graphite easily oxidized and decarburized at high temperatures, resulting in a loose material structure and a sharp drop in strength; secondly, poor thermal shock stability, making them prone to cracking and spalling due to drastic temperature fluctuations during service, shortening their service life; and thirdly, the high density of traditional dense fused magnesia aggregate results in a high self-weight of the refractory material, increasing the furnace load and hindering equipment lightweighting and energy conservation.
[0004] Currently, the industry typically adds metallic silicon powder and aluminum powder to improve the oxidation resistance of magnesia-carbon bricks, but these additives are costly and have limited effectiveness. Some technologies optimize the microstructure by introducing composite additives, but these generally suffer from complex processes, limited improvement in high-temperature performance, and difficulty in large-scale production. Furthermore, existing (low-carbon) magnesia-carbon bricks mostly use fully dense fused magnesia aggregate, making it difficult to balance lightweighting and thermal shock resistance, and thus failing to meet the multiple demands of modern high-temperature industries for energy saving, long service life, and environmental protection.
[0005] Elemental Si in silicon wire cutting waste can be preferentially oxidized at high temperatures compared to graphite, significantly improving the material's oxidation resistance. The SiC component itself can enhance the strength and oxidation resistance of refractory materials. SiO2 reacts with C in the material matrix to form a SiC reinforcing phase. Using silicon wire cutting waste in ultra-low carbon magnesia-carbon bricks can both dispose of industrial solid waste and reduce raw material costs, while also improving the overall performance of refractory materials, achieving "waste treatment and turning waste into treasure." However, existing technologies have not yet formed a mature, stable, and industrially producible process for preparing lightweight ultra-low carbon magnesia-carbon bricks using silicon-containing wire cutting waste and porous magnesia aggregate. Problems such as unclear additive dosage, unreasonable heat treatment regime, and unoptimized aggregate structure limit the widespread application of this technology.
[0006] Therefore, there is an urgent need to develop an ultra-low carbon magnesia-carbon brick containing silicon wire cutting waste and its preparation method. Summary of the Invention
[0007] In view of this, the purpose of this invention is to propose a lightweight ultra-low carbon magnesia-carbon brick, its preparation method and application, so as to solve the problems of poor oxidation resistance, insufficient thermal shock stability and large self-weight of existing low carbon magnesia-carbon bricks, and at the same time realize the high-value utilization of silicon wire cutting waste, which has significant economic, environmental and social benefits.
[0008] To achieve the above objectives, the present invention provides a lightweight ultra-low carbon magnesia-carbon brick, comprising raw material component A and a binder. By mass percentage, raw material component A comprises the following components: 89-96% fused magnesia particles and / or porous magnesia aggregate, 1-3% graphite, and 1-8% pretreated silicon wire cutting waste. The binder is added at 2-4% of raw material component A. The pretreated silicon wire cutting waste is composed of four main components: elemental silicon, silicon carbide, silicon dioxide, and ferric oxide, with other impurities accounting for ≤2%.
[0009] The pretreated silicon wire cutting waste is obtained by heat treatment of silicon wire cutting waste. By mass percentage, the pretreated silicon wire cutting waste contains 30-40% elemental silicon, 25-35% silicon carbide, 15-20% silicon dioxide, and 5-13% ferric oxide. The ultra-low carbon magnesia-carbon brick matrix contains SiO2, MgSiO3, SiC, and Fe-Si intermetallic reinforcing phases generated from the reaction of silicon wire cutting waste, replacing commonly used additives Si and SiC. The reinforcing phases fill the pores of the brick body.
[0010] The binder includes phenolic resin.
[0011] The purity of the fused magnesia particles is ≥97%, and the particle size distribution consists of three grades: 5~3mm, 3~1mm, and 1~0mm, with each grade containing 40%, 20%, and 40%, respectively.
[0012] The porous magnesium oxide aggregate is made by using fused magnesia B as raw material, adding 8-16% foaming agent, pressing it into shape under a pressure of 180-220MPa, and then holding it at 1500-1700℃ for 2-4 hours.
[0013] The fused magnesia B is selected from 200-mesh fused magnesia, and the foaming agent includes industrial SiC.
[0014] When fused magnesia particles and porous magnesia aggregate are used together, porous magnesia aggregate replaces 25-60% of the 3-1 mm and / or 5-3 mm fused magnesia particles.
[0015] The present invention also provides a method for preparing the aforementioned lightweight ultra-low carbon magnesia-carbon brick, comprising the following steps:
[0016] S1. Raw material pretreatment: Heat-treat the silicon wire cutting waste to remove impurities;
[0017] S2. Batching and mixing: Weigh out the fused magnesia particles of each grade according to the proportion, add the binder and mix for 10-15 minutes; then add graphite and pretreated silicon wire cutting waste, and continue mixing until uniform to obtain the mixture;
[0018] S3. Compression molding: The mixture is pressed into shape at 180~250MPa;
[0019] S4. Drying and heat treatment: First, dry at 200℃ for 8~10h; then, under a carbon-protected atmosphere, keep at 1600℃ for 1~3h to obtain ultra-low carbon magnesia-carbon bricks.
[0020] The carbon embedding protection is as follows: the sample is placed in a graphite crucible, and then the graphite crucible containing the sample is placed in a corundum crucible. The gap between the corundum crucible and the graphite crucible is filled with graphite powder. Both crucibles are sealed with lids and then placed in a furnace for heat treatment.
[0021] The present invention also provides the application of the lightweight ultra-low carbon magnesia-carbon brick in smelting furnaces and refining furnaces.
[0022] The beneficial effects of this invention are as follows: In the ultra-low carbon magnesia-carbon brick matrix of this invention, elemental silicon from silicon wire cutting waste provides oxidation resistance, while direct introduction or in-situ formation of silicon carbide reinforcement and in-situ formation of Fe-Si intermetallic compound reinforcement phases achieve a synergistic improvement in toughness and thermal shock resistance, while simultaneously achieving weight reduction. It easily replaces commonly used additives such as Si and SiC, and can be applied in modern steel smelting and refining processes (such as converters, electric furnaces, and ladle refining furnaces). This invention solves the problems of poor oxidation resistance, insufficient thermal shock stability, and high weight of existing low-carbon magnesia-carbon bricks, while simultaneously realizing the high-value utilization of silicon wire cutting waste, resulting in significant economic, environmental, and social benefits. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.
[0024] It should be noted that, unless otherwise defined, the technical or scientific terms used in this invention should have the ordinary meaning understood by one of ordinary skill in the art to which this invention pertains. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed following the word and their equivalents, without excluding other elements or objects.
[0025] Raw material information
[0026] Magnesia aggregate: fused magnesia particles are selected, with a three-stage gradation of 5~3mm, 3~1mm and 1~0mm, and the contents of each stage are 40%, 20% and 40% respectively. The MgO content is ≥96% and the impurity content is low. As the main skeleton structure of ultra-low carbon magnesia-carbon bricks, it provides high-temperature structural strength and volume stability.
[0027] Fused magnesia fine powder: 200 mesh fused magnesia fine powder with MgO content ≥97% is used to fill the gaps between aggregates, improve the density of the green body, and enhance the bonding strength of the matrix.
[0028] Carbon raw materials: Natural graphite with a fixed carbon content of ≥98% is selected as the carbon source for ultra-low carbon magnesia-carbon bricks, which improves the material's resistance to slag erosion, thermal conductivity and thermal shock resistance.
[0029] Pre-treated silicon wire cutting waste: This refers to the solid waste generated from the diamond wire cutting process of photovoltaic silicon wafers, which is pre-treated at high temperature to remove impurities.
[0030] The main components are: elemental Si (30%–40%), SiC (25%–35%), SiO2 (15%–20%), and Fe2O3 (5%–13%), with impurities ≤2%. As an antioxidant and silicon source, elemental silicon preferentially oxidizes to improve the oxidation resistance of low-carbon magnesia-carbon bricks, SiC enhances their high-temperature strength and thermal shock resistance, SiO2 can react with C to form SiC in situ, and Fe2O3 can react with C and Si components to form intermetallic compounds Fe-Si, thereby achieving synergistic effects.
[0031] Industrial silicon carbide: SiC content ≥98%, used as a foaming agent for preparing porous magnesium oxide aggregate, generates gas through high-temperature reaction to form a porous structure.
[0032] Binder: Thermosetting phenolic resin is selected, which has high residual carbon rate and high bonding strength. Before adding it, it is preheated to 40-60℃ to make the mixing more uniform and the green body stronger.
[0033] Preparation process
[0034] Pre-processing:
[0035] 1) Use 200-mesh fused magnesia powder as raw material, add 8%~16% industrial silicon carbide as foaming agent, and dry mix for 15 minutes until uniform.
[0036] 2) The uniformly mixed raw materials were pressed into cylindrical samples with a diameter of 50 mm × 50 mm under a pressure of 200 MPa.
[0037] 3) Keep warm at 1550℃ for 3 hours to produce porous magnesium oxide aggregate, which is then crushed and set aside for later use.
[0038] Preparation process of ultra-low carbon magnesia-carbon bricks:
[0039] 1) Raw material pretreatment: Silicon wire cutting waste is pretreated at high temperature to remove impurities and moisture, resulting in powder mainly composed of elemental Si, SiC, SiO2 and Fe2O3.
[0040] 2) Weigh the raw materials according to the following proportions: fused magnesia particles (5~3mm, 3~1mm, 1~0mm, with contents of 40%, 20%, and 40% respectively), crushed porous magnesia aggregate, 200-mesh fused magnesia fine powder, natural graphite, and pretreated silicon cutting waste; first, dry mix the fine powder, graphite, and additives for 15 minutes; then add 2% phenolic resin and continue mixing for 10 minutes; finally, crush the prepared porous magnesia sample, sieve it to obtain 3~1mm or 5~3mm aggregate, and use it at a mass ratio of 0~50% to replace the fused magnesia particles of the same size and mix them evenly.
[0041] 3) Compression molding: Pressed at 250MPa into a cylindrical sample of Φ50mm×50mm.
[0042] 4) Heat treatment: First, dry at 200℃ for 8 hours; place the dried sample in a graphite crucible, then place an outer corundum crucible inside, and fill the gap between the two crucibles with graphite powder to form a protective atmosphere. Keep at 1600℃ for 3 hours, and after furnace cooling, obtain a lightweight ultra-low carbon magnesium-carbon refractory material.
[0043] Antioxidant test method
[0044] A cylindrical specimen with a diameter of 50 mm × 50 mm was pressed under 200 MPa and dried and cured at 200 °C for 8 hours. It was then oxidized at 1400 °C in air for 3 hours. The oxidized specimen was then cut transversely along the center and the thickness of the oxide layer was measured.
[0045] All comparative examples and embodiments used the above process steps to prepare ultra-low carbon magnesium-carbon brick samples.
[0046] Example 1
[0047] The raw materials and formulations in this embodiment are as follows:
[0048] Fused magnesia particles: 80%
[0049] Fused magnesia fine powder: 16%
[0050] Graphite: 2%
[0051] Pre-processing of silicon wire cutting waste: 2%
[0052] Phenolic resin: 2% (added externally)
[0053] Performance characteristics: The apparent porosity of the ultra-low carbon magnesia-carbon brick is 20.26%, and the bulk density is 2.74 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 85.64MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 1.13mm. After three water-cooling cycles of thermal shock at 1100℃, the strength retention rate is 72.88%, and the antioxidant performance is improved.
[0054] Example 2
[0055] The raw materials and formulations in this embodiment are as follows:
[0056] Fused magnesia particles: 80%
[0057] Fused magnesia fine powder: 14%
[0058] Graphite: 2%
[0059] Pre-processing of silicon wire cutting waste: 4%
[0060] Phenolic resin: 4% (added externally)
[0061] Performance characteristics: The apparent porosity of the ultra-low carbon magnesia-carbon brick is 10.25%, and the bulk density is 3.24 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 88.72MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 812.87μm. After three water-cooling cycles at 1100℃, the strength retention rate is 75.51%. The thermal shock resistance and oxidation resistance are both better than those of Comparative Example 1.
[0062] Example 3
[0063] The raw materials and formulations in this embodiment are as follows:
[0064] Fused magnesia particles: 80%
[0065] Fused magnesia fine powder: 12%
[0066] Graphite: 2%
[0067] Pre-processing of silicon wire cutting waste: 6%
[0068] Phenolic resin: 2% (added externally).
[0069] Performance characteristics: The apparent porosity of the ultra-low carbon magnesia-carbon brick is 8.64%, and the bulk density is 3.37 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 91.23MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 660.17μm. After three water-cooling cycles at 1100℃, the strength retention rate is 77.87%. The thermal shock resistance and oxidation resistance are both better than those of Comparative Example 1.
[0070] Example 4
[0071] The raw materials and formulations in this embodiment are as follows:
[0072] Fused magnesia particles + porous magnesia aggregate (replacement rate): 84%
[0073] Fused magnesia fine powder: 8%
[0074] Graphite: 2%
[0075] Pre-processing of silicon wire cutting waste: 6%
[0076] Phenolic resin: 2% (added externally);
[0077] Of which, porous magnesium oxide aggregate (replacing 3~1mm fused magnesia particles): 21.25%;
[0078] Preparation of porous magnesium oxide: 200 mesh magnesia + 8% SiC, 1550℃×3h.
[0079] Performance and effects: Ultra-low carbon magnesia-carbon bricks achieve a certain degree of lightweighting, with an apparent porosity of 15.18%, a closed porosity of 5.32%, and a bulk density of 2.76 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 90.83MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 648.33μm. After three water-cooling cycles at 1100℃, the strength retention rate is 81.34%, and the thermal shock resistance is significantly improved.
[0080] Example 5
[0081] The raw materials and formulations in this embodiment are as follows:
[0082] Fused magnesia particles + porous magnesia aggregate (replacement rate): 84%
[0083] Fused magnesia fine powder: 8%
[0084] Graphite: 2%
[0085] Pre-processing of silicon wire cutting waste: 6%
[0086] Phenolic resin: 2% (added externally);
[0087] Of which, porous magnesium oxide aggregate (replacing 3~1mm fused magnesia particles): 27.00%;
[0088] Preparation of porous magnesium oxide aggregate: 200 mesh magnesia + 8% SiC, 1550℃×3h.
[0089] Performance characteristics: The ultra-low carbon magnesia-carbon brick has an apparent porosity of 21.91%, a closed porosity of 11.47%, and a bulk density of 2.45 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 88.41MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 625.54μm. After three water-cooling cycles at 1100℃, the strength retention rate is 84.92%. The silicon wire cutting waste exhibits superior synergistic improvement in elemental silicon oxidation resistance, direct introduction or in-situ formation of silicon carbide reinforcement, intermetallic compound Fe-Si reinforcement, and thermal shock resistance.
[0090] Example 6
[0091] The raw materials and formulations in this embodiment are as follows:
[0092] Fused magnesia particles + porous magnesia aggregate (replacement rate): 84%
[0093] Fused magnesia fine powder: 8%
[0094] Graphite: 2%
[0095] Pre-processing of silicon wire cutting waste: 6%
[0096] Phenolic resin: 2% (added externally);
[0097] Of which, porous magnesium oxide aggregate (replacing 5~3mm fused magnesia particles): 15.5%;
[0098] Porous magnesium oxide aggregate (replacing 3~1mm fused magnesia particles): 42.50%;
[0099] Preparation of porous magnesium oxide aggregate: 200 mesh magnesia + 16% SiC, 1550℃×3h.
[0100] Comparative Example 1
[0101] The raw materials and proportions for this comparative example are as follows:
[0102] Fused magnesia particles: 85%
[0103] Fused magnesia fine powder: 13%
[0104] Graphite: 2%
[0105] Phenolic resin: 2% (added externally)
[0106] Performance characteristics: The apparent porosity of the ultra-low carbon magnesia-carbon brick is 18.2%, and the bulk density is 2.82 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 72.31MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 1.73mm. After three water-cooling cycles of thermal shock at 1100℃, the strength retention rate is 64.23%, indicating good oxidation resistance.
[0107] Performance characteristics: The ultra-low carbon magnesia-carbon brick has an apparent porosity of 28.76%, a closed porosity of 19.83%, and a bulk density of 1.86 g / cm³. 3 After heat treatment at 1600℃, the room temperature compressive strength is 84.26MPa. After holding at 1400℃ for 3 hours, the oxide layer thickness is 585.12mm. After three water-cooling cycles of thermal shock at 1100℃, the strength retention rate is 87.25%. The optimal effect is achieved by synergistic improvement of elemental silicon anti-oxidation, direct introduction or in-situ formation of silicon carbide reinforcement, and in-situ formation of Fe-Si intermetallic compounds in silicon wire cutting waste, while also achieving the goal of lightweighting.
[0108] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention is limited to these examples; within the framework of the invention, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of the different aspects of the invention as described above, which are not provided in detail for the sake of brevity. Any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the scope of protection of the invention.
Claims
1. A lightweight ultra-low carbon magnesia-carbon brick, comprising raw material component A and a binder, characterized in that, By mass percentage, raw material component A comprises the following components: 89-96% fused magnesia particles and / or porous magnesia aggregate, 1-3% graphite, and 1-8% pretreated silicon wire cutting waste; the amount of binder added is 2-4% of raw material component A, and the pretreated silicon wire cutting waste is composed of four main components: elemental silicon, silicon carbide, silicon dioxide and ferric oxide, with other impurities content ≤2%.
2. The lightweight ultra-low carbon magnesia-carbon brick according to claim 1, characterized in that, The pretreated silicon wire cutting waste is obtained by heat treatment of silicon wire cutting waste. By mass percentage, the pretreated silicon wire cutting waste contains 30-40% elemental silicon, 25-35% silicon carbide, 15-20% silicon dioxide, and 5-13% ferric oxide.
3. The lightweight ultra-low carbon magnesia-carbon brick according to claim 1, characterized in that, The binder includes phenolic resin.
4. The lightweight ultra-low carbon magnesia-carbon brick according to claim 1, characterized in that, The purity of the fused magnesia particles is ≥97%, and the particle size distribution consists of three grades: 5~3mm, 3~1mm, and 1~0mm.
5. The lightweight ultra-low carbon magnesia-carbon brick according to claim 1, characterized in that, The porous magnesium oxide aggregate is made by using fused magnesia B as raw material, adding 8-16% foaming agent, pressing it into shape under a pressure of 180-220MPa, and then holding it at 1500-1700℃ for 2-4 hours.
6. The lightweight ultra-low carbon magnesia-carbon brick according to claim 5, characterized in that, The fused magnesia B is selected from 200-mesh fused magnesia, and the foaming agent includes industrial SiC.
7. The lightweight ultra-low carbon magnesia-carbon brick according to claim 1, characterized in that, When fused magnesia particles and porous magnesia aggregate are used together in raw material component A, the porous magnesia aggregate replaces 25-60% of the 3-1 mm and / or 5-3 mm fused magnesia particles.
8. The method for preparing lightweight ultra-low carbon magnesia-carbon bricks according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Raw material pretreatment: Heat-treat the silicon wire cutting waste to remove impurities; S2. Batching and mixing: Weigh out the fused magnesia particles of each grade according to the proportion, add the binder and mix for 10-15 minutes; then add graphite and pretreated silicon wire cutting waste, and continue mixing until uniform to obtain the mixture; S3. Compression molding: The mixture is pressed into shape at 180~250MPa; S4. Drying and heat treatment: First, dry at 200℃ for 8~10h; then, under a carbon-protected atmosphere, keep at 1600℃ for 1~3h to obtain ultra-low carbon magnesia-carbon bricks.
9. The method for preparing lightweight ultra-low carbon magnesia-carbon bricks according to claim 8, characterized in that, The carbon embedding protection is as follows: the sample is placed in a graphite crucible, and then the graphite crucible containing the sample is placed in a corundum crucible. The gap between the corundum crucible and the graphite crucible is filled with graphite powder. Both crucibles are sealed with lids and then placed in a furnace for heat treatment.
10. The application of the lightweight ultra-low carbon magnesia-carbon bricks according to any one of claims 1-7 in smelting furnaces and refining furnaces.