A novel through-hole ceramic and its preparation method

By preparing through-hole ceramics with a multi-level porous structure, and utilizing the foaming mechanism of silicon carbide and iron oxide to form interconnected channels, the problem of existing through-hole ceramics being unable to simultaneously achieve lightweight, high water absorption and high sound absorption performance is solved, realizing a high-efficiency sound absorption effect with low cost and simple process.

CN123106243APending Publication Date: 2026-11-17SHANDONG JUAN INORGANIC THERMAL INSULATION DECORATION MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611259999.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing porous ceramics struggle to achieve a balance between lightweight, high water absorption, and high sound absorption performance, and their complex manufacturing processes limit their application in fields such as high-efficiency sound absorption and liquid absorption.

Method used

Using raw materials such as diatomaceous earth, kaolin, blast furnace slag, calcite, iron oxide powder and foaming agent, a multi-level porous ceramic is prepared through a firing process. The foaming mechanism of silicon carbide and iron oxide is used to form interconnected channels. Combined with the stable structure of the anorthite-quartz crystal phase, it achieves lightweight, high water absorption and high sound absorption performance.

Benefits of technology

The prepared porous ceramics have low specific gravity, excellent sound absorption performance, good mechanical properties and simple process, and are highly adaptable to meet the needs of different application scenarios.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a novel through-porous ceramic and its preparation method, belonging to the field of through-porous ceramic technology. The ceramic has a specific gravity of 140-350 kg / m³, a volumetric water absorption rate of 60-90%, a mass water absorption rate of 180-400%, a compressive strength ≥1.5 MPa, and a sound absorption coefficient nrc ≥0.4. The pore size of the mesopores is 10 μm ≤ d ≤ 50 μm; the pore size of the macropores is d ≥ 50 μm. It possesses lightweight, high water absorption, high sound absorption, and good mechanical properties. The ceramic's internal structure forms a multi-level pore structure of mesopores (10 μm ≤ d ≤ 50 μm) and macropores (d ≥ 50 μm), which is beneficial for improving the absorption and transport efficiency of liquids, while simultaneously enhancing sound absorption performance. The raw materials are widely available and low-cost: using industrial byproducts such as diatomaceous earth and blast furnace slag as the main raw materials reduces production costs and achieves comprehensive resource utilization, conforming to the concept of green environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a novel perforated ceramic and its preparation method, belonging to the field of perforated ceramic technology. Background Technology

[0002] Through-porous ceramics are widely used in filtration, sound absorption, heat insulation, biomedicine, and chemical catalysis due to their excellent permeability, low density, high specific surface area, and superior sound absorption and liquid absorption properties. Traditional through-porous ceramics are mostly prepared using organic foam impregnation, pore-forming agent addition, or foaming methods. While these methods can achieve a certain pore structure, they generally suffer from uneven pore size distribution, poor pore connectivity, low mechanical strength, and complex manufacturing processes. Furthermore, existing through-porous ceramics struggle to simultaneously achieve lightweight, high water absorption, and high sound absorption coefficient, limiting their application in high-efficiency sound absorption and liquid absorption. Therefore, developing a novel through-porous ceramic with low specific gravity, high water absorption, excellent sound absorption performance, and a simple manufacturing process is of significant practical importance. Summary of the Invention

[0003] Based on the problems described in the background, the problem that this invention aims to solve is:

[0004] How to develop a new type of through-hole ceramic with low specific gravity, high water absorption, excellent sound absorption performance and simple preparation process.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] A novel method for preparing through-hole ceramics, with the following raw material formula:

[0007] Diatomaceous earth 40-60%;

[0008] Kaolin content 8-15%;

[0009] Blast furnace slag 20-30%;

[0010] Calcite 5-10%;

[0011] 1-5% ferric oxide powder;

[0012] Foaming agent 0.2-0.8%;

[0013] Water-reducing agent 0.7-1.5%;

[0014] The chemical composition range of the mixture is as follows:

[0015] SiO2: Al2O3: CaO: MgO: Fe2O3: Na2O: K2O: IL=57-65: 10-15: 12-17: 1.5-3.5: 1.8-4: 0.5-1.5: 0.5-1.5: 6-8.

[0016] The preparation method is as follows:

[0017] (1) Weigh the raw materials according to the formula, grind them into a slurry, and make them into powder for later use;

[0018] (2) The powder is placed in a refractory mold and fired in a kiln to obtain perforated ceramics;

[0019] (3) Cut the thick through-hole ceramic to obtain products with different requirements.

[0020] Preferably, the grinding fineness in step 1 is: 0.1-0.5% residue on a 325-mesh sieve and 1.4-1.45 specific gravity of the slurry.

[0021] Preferably, the powder produced in step 1 is produced by spray drying tower, and the moisture content of the powder produced by spray drying tower is 8-20%.

[0022] Preferably, the highest firing temperature in step 2 is 1130-1170℃, and the firing cycle is 3-12 hours.

[0023] Preferably, the sintered crystalline phases in step 2 are mainly anorthite-quartz, pseudowollastonite, and enstatite. Among them, anorthite-quartz is the main phase, with a small amount of pseudowollastonite and enstatite phases present.

[0024] A novel perforated ceramic, prepared according to the above-described method, has a specific gravity of 140-350 kg / m³, a volumetric water absorption rate of 60-90%, a mass water absorption rate of 180-400%, a compressive strength ≥1.5 MPa, and a sound absorption coefficient nrc ≥0.4. The pore size of the mesopores is 10 μm ≤ d ≤ 50 μm; the pore size of the macropores is d ≥ 50 μm. This perforated ceramic meets the national industry standard for sound-absorbing panels with a sound absorption coefficient nrc ≥ 0.4; the sound-absorbing panel obtained according to the preparation method of this invention has a sound absorption coefficient nrc ≥ 0.7, making it an excellent ceramic for sound-absorbing panels.

[0025] When the porous ceramic powder enters the firing stage (starting from 1050℃), the calcium oxide provided by the calcite in the raw materials reacts with the silica and alumina provided by the diatomaceous earth, kaolin and other raw materials to generate a liquid phase with calcium feldspar as the main crystalline phase. At this time, the foaming agent silicon carbide plays a role, causing the product to start to produce relatively large bubbles. The reaction formula of the silicon carbide foaming mechanism is SiC + O2 → SiO2 + CO / CO2. These bubbles are generally larger than 50 micrometers in diameter, each bubble is a separate chamber, and there are no channels connecting the bubbles.

[0026] Subsequently, as the temperature rises, ferric oxide begins to play a role on the bubble walls initiated by silicon carbide, initiating new bubbles. The reaction at this point is SiC + 4Fe₂O₃ → SiO₂ + 8FeO + CO₂, with ferric oxide acting as both a bubble promoter and stabilizer. These bubbles typically have diameters between 10 and 50 micrometers, essentially creating smaller bubbles on top of the original large bubble walls. The channels formed by these smaller bubbles connect the original large bubbles, creating well-defined, interconnected channels.

[0027] The beneficial effects of this invention are:

[0028] The porous ceramic prepared by this invention has a sound absorption coefficient NRC≥0.4, and combines lightweight, high water absorption, high sound absorption and good mechanical properties.

[0029] The ceramic interior forms a multi-level pore structure consisting of intermediate pores (10μm ≤ d ≤ 50μm) and macropores (d ≥ 50μm), which is beneficial for improving the absorption and transport efficiency of liquids, while also enhancing sound absorption performance.

[0030] The raw materials are widely available and low in cost: using industrial by-products such as diatomaceous earth and blast furnace slag as the main raw materials not only reduces production costs but also achieves comprehensive utilization of resources, which is in line with the concept of green environmental protection.

[0031] The preparation process is simple and highly controllable, with low firing temperature, short cycle, and significant energy-saving effect.

[0032] The main crystalline phase after firing in this invention is an anorthite-quartz crystalline phase, which has a stable structure and good durability and safety in use.

[0033] This invention is highly adaptable and widely used. The formula and process parameters can be adjusted according to needs to prepare through-hole ceramics with different pore sizes, densities and properties to meet the requirements of different application scenarios. It is an excellent material for the production of sound-absorbing panels and artificial islands and reefs. Detailed Implementation

[0034] Example 1

[0035] A novel perforated ceramic plate, the mass percentage of its formulation is as follows:

[0036] 45% diatomaceous earth;

[0037] Blast furnace slag 26%;

[0038] 10% calcite;

[0039] 15% kaolin;

[0040] Iron oxide red 4.2%;

[0041] Foaming agent 0.5%;

[0042] Water-reducing agent 1.3%;

[0043] (1) The raw materials weighed according to the proportion are put into the ball mill and ground into slurry. The fineness of the slurry is 325 mesh with a residue of 0.2 g and a specific gravity of 1.41.

[0044] (2) The ground mud is pulverized by spray drying tower; the moisture content of the powder prepared by spray drying tower is 9%;

[0045] (3) The powder produced by the spray drying tower is placed into a refractory sagger;

[0046] (4) The refractory sagger is fired in the kiln at a maximum temperature of 1130℃ for 12 hours.

[0047] (5) The fired finished products are cut and packaged according to customer requirements.

[0048] The cut product was tested, and the following data were obtained: specific gravity 280kg / m³, volumetric water absorption rate: 75%, mass water absorption rate: 320%, compressive strength 1.62mp, and sound absorption coefficient nrc 0.78.

[0049] Example 2

[0050] A novel perforated ceramic plate, the mass percentage of its formulation is as follows:

[0051] 55% diatomaceous earth;

[0052] 25% blast furnace slag;

[0053] 5% calcite;

[0054] Kaolin 11%;

[0055] Iron oxide red 1.7%;

[0056] Foaming agent 0.8%;

[0057] Water-reducing agent 1.5%;

[0058] (1) The raw materials weighed according to the proportion are put into the ball mill and ground into slurry. The fineness of the slurry is 325 mesh with a residue of 0.35 g and a specific gravity of 1.45.

[0059] (2) The ground mud is pulverized by spray drying tower; the moisture content of the powder prepared by spray drying tower is 20%;

[0060] (3) The powder produced by the spray drying tower is placed into a refractory sagger;

[0061] (4) The refractory sagger is fired in the kiln at a maximum temperature of 1170℃ for 3 hours.

[0062] (5) The fired finished products are cut and packaged according to customer requirements.

[0063] The cut product was tested, and the following data were obtained: specific gravity 320kg / m³, volumetric water absorption rate: 65%, mass water absorption rate: 210%, compressive strength 1.66mp, and sound absorption coefficient nrc 0.73.

[0064] Example 3

[0065] A novel porous ceramic plate, the mass percentage of its formulation is as follows:

[0066] Diatomaceous earth 60%;

[0067] 20% blast furnace slag;

[0068] Calcite 9.5%;

[0069] 8% kaolin;

[0070] 1% iron oxide red;

[0071] Foaming agent 0.2%;

[0072] Water-reducing agent 1.3%;

[0073] (1) The raw materials weighed according to the proportion are put into the ball mill and ground into slurry. The fineness of the slurry is 325 mesh with a residue of 0.48 g and a specific gravity of 1.44.

[0074] (2) The ground mud is pulverized by spray drying tower; the moisture content of the powder prepared by spray drying tower is 15%;

[0075] (3) The powder produced by the spray drying tower is placed into a refractory sagger;

[0076] (4) The refractory sagger is fired in the kiln at a maximum temperature of 1160℃ for 8 hours.

[0077] (5) The fired finished products are cut and packaged according to customer requirements.

[0078] The cut product was tested, and the following data were obtained: specific gravity 350kg / m³, volumetric water absorption rate: 60%, mass water absorption rate: 180%, compressive strength 1.71mp, and sound absorption coefficient nrc 0.7.

[0079] Example 4

[0080] A novel perforated ceramic plate, the mass percentage of its formulation is as follows:

[0081] 40% diatomaceous earth;

[0082] 30% blast furnace slag;

[0083] Calcite 8.8%;

[0084] 15% kaolin;

[0085] Iron oxide red 5%;

[0086] Foaming agent 0.5%;

[0087] Water-reducing agent 0.7%;

[0088] (1) The raw materials weighed according to the proportion are put into the ball mill and ground into slurry. The fineness of the slurry is 325 mesh with a residue of 0.12 g and a specific gravity of 1.4.

[0089] (2) The ground mud is pulverized by spray drying tower; the moisture content of the powder prepared by spray drying tower is 8%;

[0090] (3) The powder produced by the spray drying tower is placed into a refractory sagger;

[0091] (4) The refractory sagger is fired in the kiln at a maximum temperature of 1150℃ for 10 hours.

[0092] (5) The fired finished products are cut and packaged according to customer requirements.

[0093] The cut product was tested, and the following data were obtained: specific gravity 180kg / m³, volumetric water absorption rate: 90%, mass water absorption rate: 400%, compressive strength 1.5mp, and sound absorption coefficient nrc 0.86.

Claims

1. A novel method for preparing through-hole ceramics, characterized in that, The raw material formula is as follows: Diatomaceous earth 40-60%; Kaolin content 8-15%; Blast furnace slag 20-30%; Calcite 5-10%; 1-5% ferric oxide powder; Foaming agent 0.2-0.8%; Water-reducing agent 0.7-1.5%; The chemical composition range of the mixture is as follows: SiO2: Al2O3: CaO: MgO: Fe2O3: Na2O: K2O: IL=57-65: 10-15: 12-17: 1.5-3.5: 1.8-4: 0.5-1.5: 0.5-1.5: 6-8.

2. The preparation method is as follows: (1) Weigh the raw materials according to the formula, grind them into a slurry, and make them into powder for later use; (2) The powder is put into the refractory mold and fired in the kiln to obtain perforated ceramics; (3) Cut the thick through-hole ceramic to obtain products with different requirements.

3. The novel method for preparing through-hole ceramics according to claim 1, characterized in that, The grinding fineness in step 1 is: 0.1-0.5% residue on a 325-mesh sieve, and a slurry specific gravity of 1.4-1.

45.

4. The novel method for preparing through-hole ceramics according to claim 1, characterized in that, In step 1, the powder is produced by spray drying tower, and the moisture content of the powder produced by spray drying tower is 8-20%.

5. The novel method for preparing through-hole ceramics according to claim 1, characterized in that, The highest firing temperature in step 2 is 1130-1170℃, and the firing cycle is 3-12 hours.

6. The novel method for preparing through-hole ceramics according to claim 1, characterized in that, In step 2, the sintered crystal phases are anorthite-quartz, pseudowollastonite, and enstatite.

7. A novel through-hole ceramic, prepared according to any one of claims 1-5, characterized in that, The ceramic has a specific gravity of 140-350 kg / m³, a volume water absorption rate of 60-90%, a mass water absorption rate of 180-400%, a compressive strength of ≥1.5 MPa, and a sound absorption coefficient of nrc ≥0.

4. The pore size of the mesopores is 10 μm ≤ d ≤ 50 μm, and the pore size of the macropores is d ≥ 50 μm.

8. A novel through-hole ceramic according to claim 6, characterized in that, The sound absorption coefficient nrc ≥ 0.7.