A method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag
The preparation of silicon-calcium-potassium-magnesium fertilizer by synergistic activation of molybdenum tailings and tungsten slag solves the problem of mixed storage of molybdenum tailings and tungsten slag, realizes the resource utilization of solid waste and soil improvement, reduces treatment costs and improves resource utilization rate.
Patent Information
- Application Number
- CN202611480397.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to effectively address the high environmental risks associated with the mixed storage of molybdenum tailings and tungsten slag, the high cost of treating single solid wastes, the low resource utilization rate, and the over-reliance on natural resources in traditional mineral fertilizer production.
By constructing a synergistic activation system of molybdenum tailings and tungsten slag, utilizing the silicon-aluminum richness and coarse-grained structure of molybdenum tailings as a framework support, and tungsten slag as a filler to fill the voids and provide an alkaline activator, combined with high-temperature sintering technology, silicon-calcium-potassium-magnesium fertilizer is prepared.
It achieves stable solidification of heavy metal arsenic, efficient release of nutrients, reduces raw material costs, and realizes the reduction and resource utilization of bulk solid waste. The product has excellent slow-release performance and soil improvement effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a method for the co-production of silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag. Background Technology
[0002] Tungsten (W) and molybdenum (Mo) both belong to group VIB in the periodic table and have extremely similar chemical properties. Controlled by geological mineralization patterns, they readily coexist or are associated in nature, widely existing in large-scale symbiotic deposits such as skarn and porphyry types. Based on this resource endowment, large-scale "mining-beneficiation-smelting" industrial clusters have formed in major tungsten and molybdenum producing areas in my country, such as Jiangxi, Hunan, Henan, and Fujian. In this industrial chain, the molybdenum tailings produced in the beneficiation stage and the tungsten slag produced in the subsequent smelting stage are not only highly synchronized in their formation time but also often face the situation of being mixed and stockpiled due to geographical proximity.
[0003] Although originating from the same source, the two types of solid waste differ significantly in nature. Molybdenum tailings are a large quantity of industrial solid waste discharged after molybdenum ore is crushed, ground, and flotated to extract molybdenum concentrate. Its mineral phase is rich in gangue minerals such as quartz, feldspar, and calcite; the particle size is relatively coarse, appearing as sand or silt, with a hard texture and stable chemical properties. Tungsten slag, on the other hand, is leaching residue produced during the smelting of tungsten concentrate. It is often classified as hazardous waste due to its presence of arsenic and heavy metals; its physical state is mostly extremely fine mud or micron-sized powder, with high water content and poor permeability. However, in terms of chemical composition, in addition to calcium oxide, iron oxide, and silicon dioxide, it often contains a high content of alkali.
[0004] Single governance models are no longer sufficient to meet the urgent needs of environmental protection and resource recycling in mines. Adhering to the innovative concept of "treating waste with waste," the development of technology for the co-activation of tungsten slag and molybdenum tailings to prepare mineral fertilizers can not only effectively solve the environmental risks and sorting problems caused by mixed storage of waste residues, but also represent an inevitable development trend for achieving overall reduction, harmlessness, and high-value utilization of regional bulk solid waste. Summary of the Invention
[0005] This invention aims to address at least one of the technical problems existing in the prior art. To this end, this invention provides a method for the synergistic resource utilization of molybdenum tailings and tungsten slag to prepare silicon-calcium-potassium-magnesium fertilizer. This method can solve problems such as the high environmental risk of mixed storage, high cost of treating single solid wastes, low resource utilization rate, and over-reliance on natural resources in the existing solid waste treatment process of tungsten and molybdenum mines. The method of this invention constructs a synergistic activation system of alkaline tungsten slag and siliceous-calcareous tailings, achieving stable solidification of heavy metal arsenic and efficient release of nutrients (silicon, calcium, potassium, and magnesium), thereby achieving the goals of "treating waste with waste," full utilization of bulk solid waste, and green agricultural recycling.
[0006] This invention leverages the differences in properties between molybdenum tailings and tungsten slag to achieve synergistic resource recovery, complementing each other's physicochemical properties. The silicon-aluminum richness and coarse-grained structure of molybdenum tailings serve as aggregates to provide skeletal support. Furthermore, extremely fine tungsten slag is used as filler to fill voids and optimize material gradation, while its residual alkaline components act as natural activators, promoting the dissolution and recombination of silicon and aluminum components in thermochemical reactions. This invention utilizes this combination of a silicon-aluminum skeleton and alkaline activation / filling, combined with high-temperature sintering technology, to achieve the reduction of large quantities of solid waste.
[0007] The present invention achieves its technical objective through the following technical solutions:
[0008] This invention provides a method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag, comprising the following steps:
[0009] S1. The molybdenum tailings and tungsten slag are dried, and the molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate are mixed to obtain a mixture.
[0010] S2. Roast the mixture to obtain roasted clinker, and use alkaline solution to collect the flue gas generated during the roasting process;
[0011] S3. After the roasted clinker is cooled, it is crushed and ground to obtain silicon-calcium-potassium-magnesium fertilizer.
[0012] According to some embodiments of the present invention, in step S1, the molybdenum tailings are tailings produced by the molybdenum ore flotation process, and the mineral composition includes quartz, dolomite, calcite, serpentine and mica; the molybdenum tailings have no leaching toxicity.
[0013] According to some embodiments of the present invention, in step S1, the tungsten slag is the leaching residue produced during the smelting process of tungsten concentrate; preferably, it is the tailings after recovering residual tungsten, tin and copper through a combined gravity separation-flotation process, and the mineral composition includes fluorapatite, calcite, fluorite and calcium carbonate; the tungsten slag has no leaching toxicity.
[0014] According to some embodiments of the present invention, in step S1, the moisture content of the molybdenum tailings and tungsten slag is controlled to be <2%.
[0015] According to some embodiments of the present invention, in step S1, the mass ratio of the molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate is 1:(0.2~0.6):(0.1~0.3):(0.05~0.2):(0.01~0.1).
[0016] According to some preferred embodiments of the present invention, the mass ratio of the molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate is 1:(0.4~0.5):(0.15~0.25):(0.08~0.15):(0.03~0.08).
[0017] According to some embodiments of the present invention, in step S1, the fineness of the mixture is controlled to be ≥80% of -200 mesh.
[0018] According to some embodiments of the present invention, in step S2, the calcination temperature is 1000~1200℃, the time is 30~120 min, and air is continuously introduced during the calcination process.
[0019] According to some preferred embodiments of the present invention, in step S2, the calcination temperature is 1080~1120℃ and the time is 40~100 min.
[0020] According to some embodiments of the present invention, in step S2, the alkaline solution is saturated lime water or sodium hydroxide solution.
[0021] The beneficial effects of this invention are:
[0022] 1) The method provided by the present invention utilizes the aluminosilicate minerals rich in molybdenum tailings as a framework and the residual alkaline components in tungsten slag as roasting aids, thereby achieving the synergistic utilization of components in the "waste-to-waste" approach, significantly reducing raw material costs, and realizing the simultaneous treatment and resource utilization of various industrial solid wastes.
[0023] 2) The silicon-calcium-potassium-magnesium fertilizer prepared by this invention is rich in essential medium-level elements (potassium and magnesium) and quality elements (active silicon) for crops. Because the nutrients exist in the form of stable mineral aggregates, the product has excellent slow-release properties, effectively reducing nutrient loss due to rainwater runoff. This fertilizer is weakly alkaline and has a porous structure; after being applied to the soil, it can adjust the pH value of acidic soils and improve the soil aggregate structure, achieving the dual effects of crop fertilization and soil improvement.
[0024] 3) The method provided by this invention has low requirements for the purity of raw materials and can also directly process the mixture of tungsten slag and molybdenum tailings; the process flow is short and it is particularly suitable for large-scale industrial promotion in tungsten and molybdenum industrial clusters such as Jiangxi and Henan, with significant social and economic benefits.
[0025] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Detailed Implementation
[0026] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.
[0027] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0028] Example 1
[0029] This embodiment provides a method for the co-resource utilization of tungsten slag and molybdenum tailings to prepare silicon-calcium-potassium-magnesium fertilizer. The specific steps are as follows:
[0030] 1) Dry the molybdenum tailings and tungsten slag to reduce their moisture content to below 2%;
[0031] Tables 1 and 2 show the chemical elemental analysis results of molybdenum tailings and tungsten slag, respectively. Molybdenum tailings are rich in Si, Ca, Mg, and K, while tungsten slag has relatively high Ca and Mg content. The main mineral components of molybdenum tailings include quartz, dolomite, calcite, serpentine, and mica, while the main mineral components of tungsten slag include fluorapatite, calcite, fluorite, and calcium carbonate. Both showed no leaching toxicity upon testing.
[0032] 2) Mix the dried molybdenum tailings, tungsten slag, limestone, potassium feldspar, and calcium carbonate in a mass ratio of 1:0.5:0.2:0.1:0.05. The fineness of the mixture should meet the requirement that -200 mesh accounts for ≥80% to ensure sufficient contact between the components in the subsequent reaction.
[0033] 3) The uniformly mixed material is fed into a tube furnace for high-temperature roasting at 1100℃ for 60 min. Air is continuously introduced during the roasting process to maintain an oxidizing atmosphere. The flue gas generated during roasting (mainly carbon dioxide and potassium carbonate) is treated by an absorption device, using saturated lime water as the absorbent. The precipitates generated by the reaction are collected separately and disposed of safely.
[0034] 4) After roasting, the clinker is naturally cooled to room temperature. The mixture is then crushed, ground, and sieved to obtain the silicon-calcium-potassium-magnesium fertilizer product.
[0035] Example 2
[0036] This embodiment provides a method for the co-resource utilization of tungsten slag and molybdenum tailings to prepare silicon-calcium-potassium-magnesium fertilizer. This embodiment is basically the same as embodiment 1, except that the roasting temperature in step 3) of this embodiment is 1000℃, and the other steps and processes are the same as in embodiment 1.
[0037] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0038] Example 3
[0039] This embodiment provides a method for the co-resource utilization of tungsten slag and molybdenum tailings to prepare silicon-calcium-potassium-magnesium fertilizer. This embodiment is basically the same as embodiment 1, except that the roasting temperature in step 3) of this embodiment is 1200℃, and the other steps and processes are the same as in embodiment 1.
[0040] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0041] Comparative Example 1
[0042] The difference between this comparative example and Example 1 is that in step 2), the dried molybdenum tailings, limestone, potassium feldspar, and calcium carbonate are mixed in a mass ratio of 1:0.2:0.1:0.05, and tungsten slag is not added; the other steps and processes are the same as in Example 1.
[0043] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0044] Comparative Example 2
[0045] The difference between this comparative example and Example 1 is that in step 2), the dried molybdenum tailings, tungsten slag, limestone, and potassium feldspar are mixed in a mass ratio of 1:0.5:0.2:0.1, and potassium carbonate is not added; the other steps and processes are the same as in Example 1.
[0046] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0047] Comparative Example 3
[0048] The difference between this comparative example and Example 1 is that in step 2), the dried molybdenum tailings, tungsten slag and limestone are mixed in a mass ratio of 1:0.5:0.2, and potassium feldspar and potassium carbonate are not added; the other steps and processes are the same as in Example 1.
[0049] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0050] Comparative Example 4
[0051] The difference between this comparative example and Example 1 is that in step 2), the dried molybdenum tailings and tungsten slag are mixed at a mass ratio of 1:0.5, and limestone, potassium feldspar and potassium carbonate are not added; the other steps and processes are the same as in Example 1.
[0052] Finally, a silicon-calcium-potassium-magnesium fertilizer product was obtained.
[0053] Detection and analysis:
[0054] The silicon-calcium-potassium-magnesium fertilizer products of Examples 1-3 and Comparative Examples 1-4 were measured and compared. The results are shown in Table 3.
[0055] The method for determining the content of citrate-soluble silicon, calcium, potassium and magnesium in the sample is as follows: Take an appropriate amount of the prepared sample, add 0.5 mol / L hydrochloric acid solution and extract under specified conditions. After filtration and volume adjustment, the content of each effective element in the filtrate is determined by inductively coupled plasma optical emission spectrometry (ICP-OES).
[0056] As can be seen from the above test results, the embodiments of the present invention obtain silicon-calcium-potassium-magnesium fertilizer with high effective element content by compounding molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate, and then roasting it, thus achieving efficient activation and synergistic effect of each effective component.
[0057] Comparing Example 1 and Comparative Example 1, it can be seen that the introduction of tungsten slag can significantly increase the content of effective silicon and calcium in the prepared product. Analysis suggests that the effective components in tungsten slag play a significant fluxing role at high temperatures, reducing the decomposition temperature of silicate minerals in the system and causing the insoluble, highly crystalline silicate network in molybdenum tailings to rapidly depolymerize and transform into citrate-soluble / effective silicon-calcium phases that are easily absorbed by plants. In addition, the introduction of tungsten slag can significantly reduce the consumption of limestone (exogenous calcium additive), which not only reduces raw material costs but also facilitates the synergistic disposal and resource utilization of two typical industrial solid wastes: molybdenum tailings and tungsten slag.
[0058] Comparative Examples 2-4 show that as the amount of additives (limestone, potassium feldspar, potassium carbonate) gradually decreases, the effective silicon, calcium, potassium, and magnesium contents in the products all show a significant downward trend. Comparative Example 4, using only molybdenum tailings and tungsten slag, had an effective Si content of only 1.62%, effective K₂O of 0.66%, and effective Mg of 1.03%, indicating that these two alone cannot effectively release the silicon, potassium, and magnesium nutrients. The mineral structure was not sufficiently destroyed during high-temperature roasting, resulting in poor element solubility. In Comparative Example 3, the addition of limestone significantly increased the effective Si, Ca, and Mg contents, especially effective Mg, which increased from 1.03% to 1.90%, and effective Si, which increased from 1.62% to 6.75%. This indicates that the introduction of limestone helps promote the decomposition of silicate minerals and the activation of magnesium. After adding potassium feldspar to Comparative Example 2, the effective K2O content increased slightly from 0.37% to 0.63%, but the increase was limited. This indicates that potassium elements in potassium feldspar are difficult to be effectively fixed in the solid product without additional potassium salt additives.
[0059] Compared with Example 1, no potassium carbonate was added in Comparative Example 2. Although potassium feldspar was present, the effective K2O content was only 0.63%, which was much lower than 5.55% in Example 1. This proves that the addition of potassium carbonate not only directly replenished soluble potassium, but also significantly promoted the decomposition and transformation of potassium feldspar and other potassium-containing minerals, while improving the activation efficiency of silicon and magnesium.
[0060] In summary, the synergistic resource utilization of molybdenum tailings and tungsten slag in this invention requires the use of a multi-component system of limestone, potassium feldspar, and potassium carbonate to achieve efficient synergistic release of silicon, calcium, potassium, and magnesium.
[0061] Examples 1-3 show that calcination temperature has a significant impact on the content of effective elements in the product. Increasing the calcination temperature can significantly enhance the depolymerization of the silicon-oxygen framework and greatly increase the release of effective Si and effective K2O; however, excessively high temperatures may lead to secondary crystallization and deactivation of the magnesium-containing phase, resulting in a significant decrease in effective Mg. In Example 1 (1100℃), the content of each effective element was balanced, with Si at 11.74%, Ca at 20.70%, K2O at 5.55%, and Mg at 6.95%, showing the best synergistic activation effect. Therefore, the optimal calcination temperature of this invention should be controlled at around 1100℃.
[0062] The national standard "Silicon-Calcium-Potassium-Magnesium Fertilizer" (GB / T 36207-2018) requires that the mass fractions of Si, Ca, K2O, and Mg in Type I products be greater than or equal to 9.0%, 20.0%, 3.0%, and 2.0%, respectively, and the mass fractions of Si, Ca, K2O, and Mg in Type II products be greater than or equal to 6.0%, 14.0%, 3.0%, and 2.0%, respectively. The silicon-calcium-potassium-magnesium fertilizer product obtained in Example 1 of this invention has element contents of 11.74%, 20.70%, 5.55%, and 6.95%, respectively, which are far higher than the requirements for Type I products in the standard.
[0063] Soil improvement experiment:
[0064] The silicon-calcium-potassium-magnesium fertilizer prepared in Example 1 was used in a soil improvement experiment of molybdenum tailings. The molybdenum tailings were those listed in Table 1. The amount of silicon-calcium-potassium-magnesium fertilizer added was 0.4 g / kg. Alfalfa was used as the plant, and the planting experiment lasted for 15 days. The number of germinations of each plant was recorded and the germination rate was calculated on the 5th day after sowing. The alfalfa was harvested after 15 days, and the pH, cation exchange capacity, and chlorophyll content of the improved molybdenum tailings were measured.
[0065] Soil pH was determined using the potentiometric method for determining soil pH (HJ 962-2018); cation exchange capacity was determined using the spectrophotometric method for determining cation exchange capacity (HJ 889-2017); and chlorophyll was determined using the acetone extraction method. The determination steps were as follows: 0.5 g of the leaf to be tested was weighed, chopped, and then 2.5 mL of 80% acetone and a small amount of quartz sand were added and ground. Then, 5 mL of 80% acetone was added and ground thoroughly until homogenized. The homogenate was transferred to a centrifuge tube and centrifuged at 6000 r / min for 10 min. The supernatant was then diluted to a final volume and measured using an ultraviolet spectrophotometer.
[0066] Experimental results: The germination rate of alfalfa was 95%, and the total chlorophyll content was 3.242 mg / g;
[0067] After remediation with this silicon-calcium-potassium-magnesium fertilizer, the pH of molybdenum tailings decreased from 8.33 to 7.59, and the cation exchange capacity increased from 2.27 cmol / kg to 5.23 cmol / kg.
[0068] The above soil improvement experiments show that the silicon-calcium-potassium-magnesium fertilizer prepared in this invention can effectively improve the physicochemical properties of tailings, significantly increase the exchangeable cation reserves in the soil, and create a favorable microenvironment for plant growth.
[0069] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.
Claims
1. A method for cooperatively preparing a silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag, characterized in that, Includes the following steps: S1. The molybdenum tailings and tungsten slag are dried, and the molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate are mixed to obtain a mixture. S2. Roast the mixture to obtain roasted clinker, and use alkaline solution to collect the flue gas generated during the roasting process; S3. After the roasted clinker is cooled, it is crushed and ground to obtain silicon-calcium-potassium-magnesium fertilizer.
2. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S1, the molybdenum tailings are tailings produced by the molybdenum ore flotation process, and the mineral composition includes quartz, dolomite, calcite, serpentine and mica; the molybdenum tailings have no leaching toxicity.
3. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S1, the tungsten slag is the leaching residue produced during the smelting process of tungsten concentrate; preferably, it is the tailings after recovering residual tungsten, tin, and copper through a combined gravity separation-flotation process, and its mineral composition includes fluorapatite, calcite, fluorite, and calcium carbonate; the tungsten slag has no leaching toxicity.
4. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S1, the drying process controls the moisture content of the molybdenum tailings and tungsten slag to be less than 2%.
5. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S1, the mass ratio of molybdenum tailings, tungsten slag, limestone, potassium feldspar and potassium carbonate is 1: (0.2~0.6): (0.1~0.3): (0.05~0.2): (0.01~0.1).
6. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S1, the fineness of the mixture is controlled to be ≥80% of -200 mesh.
7. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S2, the roasting temperature is 1000~1200℃ and the time is 30~120 min, with air continuously introduced during the roasting process.
8. The method for co-preparing silicon-calcium-potassium-magnesium fertilizer from molybdenum tailings and tungsten slag according to claim 1, characterized in that, In step S2, the alkaline solution is saturated lime water or sodium hydroxide solution.