A method for catalytic degradation of polyethylene terephthalate in supercritical ammonia and its application
By using a high-entropy metal-organic framework catalyst (HE-MOF) in supercritical ammonia, PET can be directly converted into p-phenylenediamine, solving the problem of low added value of PET degradation products and achieving efficient and environmentally friendly deep value-added conversion.
Patent Information
- Application Number
- CN202611620103.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have low added value of PET degradation products and require harsh conversion conditions, making it difficult to effectively convert waste PET into the high-value chemical p-phenylenediamine.
High-entropy metal-organic framework (HE-MOF) catalysts were used to catalyze the degradation of PET in supercritical ammonia. Through a series of ammonolysis and reductive decarbonylation reactions, PET was directly converted into p-phenylenediamine, taking advantage of the high diffusivity of supercritical ammonia and the synergistic catalytic effect of the multiple metal sites of HE-MOF.
It achieves deep value-added conversion of PET, the product p-phenylenediamine has high added value, the catalyst can be reused, the reaction conditions are mild, green and environmentally friendly, the process is simplified, and the shortcomings of existing technologies are avoided.
Smart Images

Figure CN123106439A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste plastic resource utilization technology, specifically relating to a method for catalytic degradation of polyethylene terephthalate in supercritical ammonia and its application. Background Technology
[0002] Polyethylene terephthalate (PET) is a thermoplastic polyester formed by the condensation polymerization of terephthalic acid and ethylene glycol. Due to its excellent mechanical properties and chemical stability, PET is widely used in beverage bottles, textile fibers, and packaging films. Waste PET is difficult to degrade rapidly in the natural environment; therefore, depolymerizing and recycling it using chemical or biological methods is an important approach to PET waste management. Existing PET depolymerization methods mainly include alcoholysis, hydrolysis, and enzymatic hydrolysis, with different methods employing different reaction media, catalytic systems, and yielding different products.
[0003] Patent application CN122541727A discloses a method for preparing bimetallic MOF catalysts based on a soft template method and its application in the ethylene glycololysis of PET. This method uses polystyrene-block-polyethylene oxide as a soft template to prepare a mesoporous bimetallic MOF catalyst, and uses Zn / Co-MOF to catalyze the alcoholysis reaction of PET with ethylene glycol, recovering bis(hydroxyethyl) terephthalate (BHET) through post-processing. Patent application CN121895183A discloses an amino acid-zinc complex catalyst and its application in PET degradation. This method also uses ethylene glycol as a depolymerization solvent, catalyzing the alcoholysis of PET at 150–200 °C, and recovering BHET through crystallization. Both methods target BHET as the product to be recovered.
[0004] Patent application CN122213495A discloses a method for preparing porous PET materials based on solution crystallization and a method for PET degradation. This method first dissolves PET in a good solvent, then proceeds with solvent evaporation and solution crystallization to obtain a porous PET material with a continuous through-pore structure. Subsequently, PET is degraded using a PET hydrolase to improve the enzymatic hydrolysis performance of the crystalline PET material. This method requires dissolution and porosification treatment before enzymatic hydrolysis; in the examples, the solvent evaporation time is 48–72 hours.
[0005] The aforementioned patent documents utilize either ethylene glycol hydrolysis or enzymatic hydrolysis routes to recover PET, but none disclose a specific method for converting PET into p-phenylenediamine using ammonia as the reaction medium. p-phenylenediamine is an important raw material for the preparation of materials such as para-aramid fibers. Therefore, developing a catalytic conversion method for preparing p-phenylenediamine from waste PET is a direction for expanding PET recycling pathways. Summary of the Invention
[0006] To overcome the problems of low added value of PET degradation products and harsh conversion conditions in existing technologies, this invention provides a method for catalytic degradation of polyethylene terephthalate (PET) in supercritical ammonia. Using a high-entropy metal-organic framework (HE-MOF) as a catalyst, PET is directly degraded into p-phenylenediamine (PPD) and ethylene glycol, achieving deep value-added conversion of waste PET.
[0007] The specific technical solution adopted is as follows: A method for catalytic degradation of polyethylene terephthalate in supercritical ammonia includes the following steps: The polyethylene terephthalate (PET) to be degraded and the high-entropy metal-organic framework catalyst HE-MOF were added to a high-pressure reactor. The high-pressure reactor was purged with nitrogen to remove air. Then, liquid ammonia was introduced into the high-pressure reactor, stirred and mixed, and heated to convert the liquid ammonia to a supercritical state. The reaction was maintained at a temperature of 133~200 ℃ and a pressure of 11.3~20 MPa for 1~24 h. After the reaction was completed, the products p-phenylenediamine and ethylene glycol were obtained through post-treatment. High-entropy metal-organic framework catalysts (HE-MOFs) were prepared by the following method: a mixed solution comprising five metal salts, an organic ligand, and a regulator was subjected to a solvothermal reaction at 120–160 °C for 12–24 h to obtain the high-entropy metal-organic framework catalyst HE-MOF; the metal ions in the metal salts were Zn and... 2+ Cu 2+ Co 2+ Ni 2+ Mn 2+ The organic ligand is terephthalic acid (H2BDC), and the modifier is acetic acid or formic acid.
[0008] This invention constructs a tandem reaction method for the catalytic conversion of PET to p-phenylenediamine and ethylene glycol using an HE-MOF catalyst in a supercritical ammonia medium. This method first utilizes the high diffusivity and strong solubility of supercritical ammonia to achieve efficient ammonolysis of PET. Supercritical ammonia serves as both the reaction medium and reactant, generating a terephthalamide intermediate. Then, leveraging the synergistic catalytic effect of multiple metal sites in the HE-MOF (especially transition metals with redox activity such as Co, Ni, and Cu), the amide group (-CONH2) of terephthalamide is catalytically converted to an amino group (-NH2), ultimately yielding p-phenylenediamine (PPD). This invention features mild reaction conditions, extremely high added value of the product (PPD is widely used in aramid fibers, rubber antioxidants, etc., with an added value approximately 2-3 times that of terephthalamide), and the catalyst is recyclable, providing a novel pathway for the resource utilization of waste plastics.
[0009] Preferably, the amount of high-entropy metal-organic framework catalyst HE-MOF added is 1wt%-10wt% of the polyethylene terephthalate to be degraded, and most preferably 5wt%.
[0010] Preferably, the mass ratio of liquid ammonia added to the high-pressure reactor to polyethylene terephthalate to be degraded is 5-50:1, more preferably 15-25:1.
[0011] Furthermore, the reaction temperature for catalytic degradation of polyethylene terephthalate is 150~190 ℃, preferably 160~180 ℃, the reaction pressure is preferably 12~18 MPa, and the reaction time is 3~12 h, preferably 6~8 h.
[0012] Specifically, the post-processing method is as follows: cooling and depressurization, filtering and separating the reaction mixture, recovering ethylene glycol from the liquid product by vacuum distillation, separating p-phenylenediamine from the solid product by organic solvent extraction or cooling crystallization, and recovering the high-entropy metal-organic framework catalyst from the remaining solid phase for reuse (the high-entropy metal-organic framework catalyst can be reused after washing and drying).
[0013] Preferably, the high-entropy metal-organic framework catalyst is a porous nanoparticle with amorphous characteristics and a BET specific surface area of 200~800 m². 2 / g.
[0014] Furthermore, in the preparation of high-entropy metal-organic framework catalysts, the molar concentrations of each metal salt in the mixed solution are equal, the configurational entropy is >1.5R (R is the gas constant), the total metal ion concentration is 0.05~0.2 mol / L, and the ratio of the total molar amount of metal ions to the molar amount of organic ligands is 2~4:1.
[0015] The metal ions in the metal salts include Zn 2+ Cu 2+ Co 2+ Ni 2+ Mn 2+ Among them, Zn 2+ and Cu 2+ Provides strong Lewis acid sites for activating carbonyl groups, Co 2+ Ni 2+ Mn provides redox activity for the reductive decarbonylation of amides. 2+ Adjusting the electronic structure enhances catalytic activity.
[0016] Preferably, the solvent of the mixed solution is N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide or N-methyl-2-pyrrolidone, and the volume ratio of the regulator to the solvent is 1:5~20.
[0017] Specifically, in the preparation of high-entropy metal-organic framework catalysts, after the solvothermal reaction is completed, the product is naturally cooled to room temperature, centrifuged to separate the solid product, washed sequentially with DMF and anhydrous ethanol, and then vacuum dried at 60~100 ℃ for 12~24 h to obtain the high-entropy metal-organic framework catalyst.
[0018] The present invention also provides the application of the method for catalytic degradation of polyethylene terephthalate in supercritical ammonia in the treatment of waste polyethylene terephthalate products.
[0019] Waste polyethylene terephthalate (PET) products include, but are not limited to, PET packaging bottles, PET fiber products, PET films, PET sheets, and PET engineering plastic parts.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention utilizes HE-MOF catalyst to directly convert waste PET into p-phenylenediamine in supercritical ammonia, realizing a series of ammonolysis-reduction decarbonylation reactions. p-phenylenediamine is a key intermediate for dye synthesis and a key monomer for para-aramid polymerization, with high economic value. Compared with the prior art, this invention avoids the product residue problem of alcoholysis, overcomes the defects of cumbersome process and slow rate of enzyme degradation, and upgrades the product from low-value depolymerization monomer to high-value fine chemicals, realizing the deep value-added transformation of waste PET products.
[0021] (2) In the reaction process of this invention, supercritical ammonia is used as the reaction medium and reactant. The high diffusivity and strong solubility of supercritical ammonia enable the PET ammonolysis step to proceed efficiently. In addition, the multi-metal Lewis acid sites and redox active sites of the HE-MOF catalyst synergistically catalyze the subsequent amide reduction decarbonylation reaction. The two steps are completed in series in the same reactor, which is simple to operate.
[0022] (3) The high entropy effect (entropy stabilization effect > 1.5R) of HE-MOF catalyst endows the catalyst with excellent structural stability in the supercritical ammonia high temperature and high pressure environment, which solves the technical problem of easy decomposition of traditional MOF under corresponding conditions. The catalyst can be recycled more than 6 times.
[0023] (4) Compared with the existing p-phenylenediamine production method (p-dichlorobenzene ammonolysis process), the method of the present invention has mild conditions, faster reaction speed, and the reaction medium ammonia can be recycled and reused. It does not involve strong acids or strong bases throughout the process, making it green and environmentally friendly. Attached Figure Description
[0024] Figure 1 These are comparison photos of PET before and after the catalytic degradation reaction.
[0025] Figure 2This is a graph showing the trend of PET conversion rate and p-phenylenediamine PPD yield under different temperature conditions.
[0026] Figure 3 The graph shows the relationship between the number of HE-MOF catalyst cycles and PET conversion and p-phenylenediamine PPD yield. Detailed Implementation
[0027] To make the objectives, features, and advantages of this invention more apparent and understandable, a detailed description is provided below through specific embodiments. Many specific details are set forth in the following description to provide a thorough understanding of the invention. However, the invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below. Technical features in various embodiments of the invention can be combined appropriately without mutual conflict.
[0028] Unless otherwise specified, the operating methods in the following examples are generally performed under conventional conditions or as recommended by the manufacturer. Contents not described in detail in this specification are prior art known to those skilled in the art. Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.
[0029] In the following embodiments: PET conversion rate (%) = (mass of PET before reaction - mass of remaining PET) / mass of PET before reaction × 100%; p-Phenylenediamine yield (%) = (Amount of actual PPD / Amount of theoretical PPD) × 100%; Ethylene glycol yield (%) = (Amount of actual EG / Amount of theoretical EG) × 100%; The high-entropy metal-organic framework catalyst used is represented by ZnCuCoNiMn-HE-MOF. Its specific preparation process is as follows: Weigh 0.002 mol of Zn(NO3)2·6H2O, 0.002 mol of Cu(NO3)2·3H2O, 0.002 mol of Co(NO3)2·6H2O, 0.002 mol of Ni(NO3)2·6H2O, and 0.002 mol of Mn(NO3)2·4H2O, and dissolve them in 60 mL of DMF. Stir until dissolved. Add 0.003 mol of H2BDC (metal ion:ligand ≈ 3.3:1), add 6 mL of acetic acid, and react solvothermically at 140 °C for 18 h. After cooling, centrifuge, and wash the obtained solid product three times each with DMF and ethanol. Dry under vacuum at 100 °C for 18 h to obtain ZnCuCoNiMn-HE-MOF (BET ~ 480 m). 2 / g, average pore size ~4.5 nm, configurational entropy ≈1.609R).
[0030] Example 1 In this embodiment, the method for catalytic degradation of polyethylene terephthalate in supercritical ammonia is carried out according to the following steps: (1) Weigh 2.0 g of PET powder (particle size <0.5 mm, derived from commercially available mineral water bottle crushed material) and 0.1 g of ZnCuCoNiMn-HE-MOF catalyst (catalyst amount is 5 wt% of PET mass), add them to 100 mL of high pressure reactor, seal it, and then use high-purity nitrogen to replace the gas in the reactor 3 times to remove air.
[0031] (2) Charge 30 g of liquid ammonia (the mass ratio of liquid ammonia to PET is 15:1) into the high-pressure reactor. Turn on the mechanical stirrer (300 rpm) to ensure that the liquid ammonia and PET are in full contact. Heat to 160 °C at a heating rate of 2 °C / min. At this point, the pressure inside the reactor is about 15 MPa (the ammonia has entered the supercritical state). At the same time, maintain the temperature at 160 °C and 15 MPa and stir for 6 h.
[0032] (3) After the reaction is complete, stop heating and allow it to cool naturally to room temperature before slowly depressurizing (ammonia can be recovered and recycled through condensation). Open the high-pressure reactor and vacuum filter the reaction mixture. After removing a small amount of low-boiling-point impurities by vacuum distillation, the resulting liquid is the recovered ethylene glycol (EG). Extract the filter residue with hot ethanol to obtain p-phenylenediamine (PPD). Cool the extract to crystallize and obtain white to light pink needle-like crystals—p-phenylenediamine (PPD). The remaining solid phase can be recovered using the ZnCuCoNiMn-HE-MOF catalyst.
[0033] In this embodiment, the PET conversion rate was 93.5%, the PPD yield was 85.2%, and the EG yield was 91.0%. The PPD purity (HPLC) was ≥99.0%, and the ethylene glycol purity (GC-FID, internal standard method) was ≥98.0%, with a moisture content of <0.5% and the remainder being trace organic residues. The product melting point was 139~142 ℃, consistent with the PPD standard (140~143 ℃). Comparison photos of PET before and after the catalytic degradation reaction are shown below. Figure 1 As shown (scNH3 represents supercritical ammonia).
[0034] The p-phenylenediamine product obtained in Example 1 was subjected to the following tests: (a) Melting point: 139~142 ℃, consistent with PPD standard (140~143 ℃). Compared with terephthalamide (310~312 ℃), the melting point is significantly lower, proving that the amide → amine conversion is complete.
[0035] (b) FTIR (KBr): 3410, 3320 cm -1 (-NH2 stretching vibration), 1625 cm -1 (NH bending), 1515 cm -1 (Benzene ring C=C), 1265 cm -1 (CN telescopic), 830 cm -1 (Para disubstitution). It has no 1655 cm. -1 The C=O peak of the amide confirms that the amide has been completely reduced to an amine.
[0036] (c) 1 ¹H NMR (DMSO-d6, 400 MHz): δ 6.30 (s, 4H, Ar-H), δ 4.35 (br s, 4H, -NH₂). Compared with terephthalamide (δ 8.00, Ar-H; δ 7.57, -CONH₂), Ar-H is significantly shifted to δ 6.30 at a higher field due to the strong electron-donating effect of -NH₂.
[0037] (d) HPLC purity: ≥99.0%.
[0038] Examples 2-6 The reaction conditions in Examples 2-6 differ from those in Example 1 only in the reaction temperature. To investigate the effect of reaction temperature alone, the pressure inside the reactor was kept constant at 15 MPa by adjusting the amount of liquid ammonia added. Different reaction temperatures and corresponding amounts of liquid ammonia added are shown in Table 1. Catalyst dosage, reaction time, and other operating conditions were the same as in Example 1. Specific process parameters and reaction results are shown in Table 1 and... Figure 2 .
[0039] Table 1. PET degradation results at different reaction temperatures
[0040] From Table 1 and Figure 2 It can be seen that the PPD yield is only 38.2% at 140 ℃, and the product is mainly terephthalamide (incomplete reduction and decarbonylation); the PPD yield reaches 85-87% at 160~170 ℃, with the best selectivity; the PPD yield decreases at >180 ℃, possibly due to PPD polymerization or deep decomposition at high temperature.
[0041] Example 7 The filter residue (residual solid phase, containing HE-MOF catalyst and a small amount of unreacted PET) after the reaction in Example 1 was washed with DMF to dissolve the residual PET and oligomers, then washed three times with anhydrous ethanol, and dried under vacuum at 100 °C for 12 h before being reused for the catalytic degradation reaction under the conditions of Example 1. This was repeated for 6 cycles; the results are shown in Table 2 and [Table data would be inserted here]. Figure 3 .
[0042] Table 2 Results of HE-MOF catalyst recycling
[0043] From Table 2 and Figure 3 As can be seen, this batch of catalyst was used 6 times. The PPD yield was 74.1% in the 6th cycle. After 6 cycles, the PET conversion rate of the HE-MOF catalyst remained at 84.6%, and the PPD yield remained at 74.1%. The slow decline in catalytic activity may be attributed to mechanical mass loss during multiple recovery operations, the covering of some active sites by insoluble oligomers, and trace dissolution of metal sites under long-term high temperature and high pressure. Overall, the HE-MOF catalyst exhibits excellent cycling stability in the supercritical ammonia environment, which is mainly attributed to the entropy stabilizing effect of the high entropy effect on the catalyst framework structure (configurational entropy > 1.5R).
[0044] Examples 8-9 The difference between this embodiment and Example 1 is that the amount of ZnCuCoNiMn-HE-MOF catalyst added is different, with 0.020 g and 0.2 g added respectively, accounting for 1 wt% and 10 wt% of the PET mass. The remaining experimental conditions, operations, product separation and analysis methods are the same as in Example 1, and the results are shown in Table 3.
[0045] Table 3. PET degradation results under different catalyst feed conditions
[0046] The results showed that when the high-entropy metal-organic framework catalyst HE-MOF was added at 1 wt% of the polyethylene terephthalate (PET) to be degraded, the PET conversion rate was 85.4%, the terephthalamide yield was 43.4%, and the p-phenylenediamine yield was 40.1%. When the addition amount was 10 wt% of the PET to be degraded, the PET conversion rate was 94.8%, the terephthalamide yield was 5.5%, and the p-phenylenediamine yield was 86.4%. The molar yields of both products were calculated based on the amount of PET repeating units in the initial feed.
[0047] Comparative Example 1 The only difference between this comparative example and Example 1 is that no catalyst was added, and the other operating conditions were the same as in Example 1 (160 °C, 6 h, scNH3:PET = 15:1).
[0048] In this comparative example, the PET conversion rate was 88.3%, but the terephthalamide yield was 82.5%, and the PPD yield was only 2.1%. The above results indicate that (1) supercritical ammonia itself can efficiently catalyze the ammonolysis of PET to terephthalamide; (2) however, supercritical ammonia alone cannot achieve the reductive decarbonylation of amide to amine, and the HE-MOF catalyst is a necessary condition for significantly improving the PPD yield.
[0049] Comparative Example 2 The only difference between this comparative example and Example 1 is that the HE-MOF catalyst in Example 1 is replaced with an equal mass (0.1 g) of a single-metal MOF catalyst Zn-BDC (prepared in the same way as the HE-MOF catalyst but without the addition of Cu, Co, Ni, and Mn salts), while other conditions remain unchanged.
[0050] In this comparative example, the PET conversion rate was 91.5%, the terephthalamide yield was 76.3%, and the p-phenylenediamine yield was only 11.6%. These results indicate that the single-metal MOF exhibits only Lewis acidity without multi-metal redox synergy, resulting in extremely weak amide decarbonylation activity. This verifies the crucial contribution of the multi-metal high-entropy synergistic effect to catalytic activity.
[0051] Comparative Example 3 The only difference between this comparative example and Example 1 is that the HE-MOF catalyst in Example 1 is replaced with a ternary medium-entropy MOF catalyst ZnCuCo-MOF (prepared using the same method as the HE-MOF catalyst, but containing only Zn, Cu, and Co metals), with the catalysts fed in a molar ratio of 1:1:1, the configurational entropy ≈ 1.1R, and other conditions remaining unchanged.
[0052] In this comparative example, the PET conversion rate was 89.1%, and the PPD yield was 42.6%. These results indicate that the catalytic activity of this ternary medium-entropy MOF catalyst lies between that of a single-metal MOF and a pentagonal HE-MOF. The pentagonal HE-MOF catalyst exhibits significantly improved catalytic performance compared to the ternary medium-entropy MOF catalyst.
[0053] Comparative Example 4 The only difference between this comparative example and Example 1 is that the ammonia did not reach the supercritical state (125 ℃, 15 MPa; 125 ℃ is below the critical temperature of ammonia, and ammonia was not in a supercritical state under the corresponding pressure), while other conditions remained the same.
[0054] In this comparative example, the PET conversion rate was only 9.3%, and the product contained almost no PPD; the main product was terephthalamide. These results indicate that the supercritical state is crucial for improving the diffusion coefficient of ammonia molecules and enhancing their ability to penetrate into the PET polymer matrix, and is a prerequisite for efficient degradation.
[0055] Comparative Example 5 The only difference between this comparative example and Example 1 is that HE-MOF is replaced by a commercial 5% Ru / C catalyst of equal mass, while other conditions remain unchanged.
[0056] In this comparative example, the PET conversion rate was 90.2%, the PPD yield was 55.6%, and the terephthalamide yield was 32.1%; the PPD yield in the second cycle was 28.1%. After use, the Ru particle size increased from 2–3 nm to 8–15 nm, and the Ru loss was approximately 18.6%. Under the stated conditions, the product yield and cycling performance of Ru / C and HE-MOF differed.
[0057] Product characterization The above examples and comparative examples fully demonstrate that this invention utilizes the synergistic effect of supercritical ammonia and HE-MOF to achieve a direct tandem conversion of waste PET into high-value p-phenylenediamine. Under optimal conditions (160 ℃, 15 MPa, 6 h, 5 wt% catalyst), the PET conversion rate is >93%, the PPD yield is >85%, and the catalyst can be recycled more than 6 times. This method features mild reaction conditions, extremely high added value of the product, and is entirely green and environmentally friendly, opening up a new avenue for the high-value utilization of waste plastics.
[0058] The embodiments described above provide a detailed explanation of the technical solutions of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, additions, or similar substitutions made within the scope of the principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for the catalytic degradation of polyethylene terephthalate in supercritical ammonia, characterized in that, Includes the following steps: The polyethylene terephthalate to be degraded and the high-entropy metal-organic framework catalyst were added to a high-pressure reactor. The high-pressure reactor was purged with nitrogen, and then liquid ammonia was introduced into it. The mixture was stirred and heated to convert the liquid ammonia to a supercritical state. The reaction was maintained at a temperature of 133~200 ℃ and a pressure of 11.3~20 MPa for 1~24 h. After the reaction was completed, the products p-phenylenediamine and ethylene glycol were obtained through post-treatment. High-entropy metal-organic framework catalysts were prepared by the following method: a mixed solution comprising five metal salts, an organic ligand, and a modifier was subjected to a solvothermal reaction at 120–160 °C for 12–24 h to obtain the high-entropy metal-organic framework catalyst; the metal ions in the metal salts were Zn and Zn, respectively. 2+ Cu 2+ Co 2+ Ni 2+ Mn 2+ The organic ligand is terephthalic acid, and the regulator is acetic acid or formic acid.
2. The method according to claim 1, characterized in that, The amount of high-entropy metal-organic framework catalyst added is 1wt%-10wt% of the polyethylene terephthalate to be degraded.
3. The method according to claim 1, characterized in that, The mass ratio of liquid ammonia added to the high-pressure reactor to the polyethylene terephthalate to be degraded is 5-50:
1.
4. The method according to claim 1, characterized in that, The reaction temperature for catalytic degradation of polyethylene terephthalate is 150~190 ℃, the reaction pressure is 12~18 MPa, and the reaction time is 3~12 h.
5. The method according to claim 1, characterized in that, The post-processing method is as follows: cooling and depressurization, filtering and separating the reaction mixture, recovering ethylene glycol from the liquid product by vacuum distillation, separating p-phenylenediamine from the solid product by organic solvent extraction or cooling crystallization, and recovering the high-entropy metal-organic framework catalyst from the remaining solid phase for reuse.
6. The method according to claim 1, characterized in that, When preparing high-entropy metal-organic framework catalysts, the molar concentrations of each metal salt in the mixed solution are equal, the total metal ion concentration is 0.05~0.2 mol / L, and the ratio of the total molar amount of metal ions to the molar amount of organic ligands is 2~4:
1.
7. The method according to claim 1, characterized in that, The solvent for the mixed solution is N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, or N-methyl-2-pyrrolidone, and the volume ratio of the regulator to the solvent is 1:5~20.
8. The application of the method according to any one of claims 1-7 in the treatment of waste polyethylene terephthalate products.
Citation Information
Patent Citations
Amino acid-zinc complex catalyst, preparation thereof and application of amino acid-zinc complex catalyst in PET degradation
CN121895183A
Preparation method of PET porous material based on solution crystallization and PET degradation method
CN122213495A
Bimetal-MOF catalyst synthesized based on soft template method, preparation method of bimetallic-MOF catalyst and application of bimetallic-MOF catalyst in PET glycolysis
CN122541727A