A process for producing high-purity morpholine
By using Ni-Cu-Co-Mo/La-γ-Al2O3 catalyst and multi-stage distillation process, the purity and selectivity issues in morpholine production were solved, achieving the production of high-purity morpholine and long catalyst life, while reducing energy consumption and increasing the value of by-products.
Patent Information
- Application Number
- CN202611388069.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing morpholine production processes struggle to achieve high purity, suffer from low byproduct selectivity, are prone to catalyst deactivation, and have high energy consumption. Traditional processes are ill-suited to meet the requirements of high-end applications.
Using a Ni-Cu-Co-Mo/La-γ-Al2O3 multimetal catalyst, deep dehydration and dealkylation reactions were carried out by superheating diethylene glycol alone and mixing it with a high ammonia ratio, combined with medium-pressure and low-pressure pressure swing distillation, and with the assistance of a physical mixed catalyst and an amine recovery tower. Finally, high-purity morpholine was extracted in an atmospheric pressure refining distillation tower.
It achieves morpholine purity ≥99.85%, moisture ≤0.04%, color ≤10 APHA, extended catalyst life, conversion of by-products into high-value chemical raw materials, and reduced energy consumption and operating costs.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fine chemical technology, specifically relating to a process for producing high-purity morpholine. Background Technology
[0002] Morpholine (C4H9NO) is an important nitrogen-containing heterocyclic compound widely used in rubber additives, pharmaceuticals, pesticides, metal corrosion inhibitors, and surfactants. Currently, the mainstream industrial production process is the diethylene glycol hydroammoniation method: using diethylene glycol, methanol, and liquid ammonia as raw materials, a gas-phase reaction is carried out in a fixed-bed reactor under the action of Ni-Cu and Al2O3 catalysts to generate morpholine and N-methylmorpholine. Inevitably, byproducts such as N-ethylmorpholine, ethylene glycol monomethyl ether, and bismorpholino diethyl ether are also produced.
[0003] The existing process has the following prominent problems: (1) After the reaction product is separated by ordinary distillation, the purity of morpholine is usually 98.5~99.5%, which is difficult to meet the requirements of high-end rubber additives and pharmaceutical raw materials; (2) Morpholine forms an azeotrope with water, and conventional distillation cannot reduce the water content to below 0.04%; (3) In the traditional process, the diethylene glycol is not completely vaporized and easily enters the reactor in the form of droplets, which leads to catalyst flooding and carbon deposition; the main catalyst has poor hydrothermal stability and is easy to deactivate; the by-product is converted at high temperature, resulting in serious carbon deposition and short lifespan; the distillation dehydration has high energy consumption and is easy to cause thermal decomposition of morpholine; (4) The total selectivity of diethylene glycol is only about 80%, and a large amount of raw materials are converted into by-products such as N-methylmorpholine and N-ethylmorpholine, and these by-products are usually discharged as low-value front fractions.
[0004] Therefore, developing a high-purity morpholine production process that can operate stably for a long period of time has significant industrial value. Summary of the Invention
[0005] The purpose of this invention is to address the existing problems by providing a process for producing high-purity morpholine.
[0006] This invention is achieved through the following technical solution:
[0007] A process for producing high-purity morpholine includes the following steps:
[0008] (1) Diethylene glycol is heated to 270~290℃ and vaporized, and then mixed with vaporized methanol and liquid ammonia (methanol and liquid ammonia are vaporized to 80~120℃ respectively), and then introduced into a fixed-bed reactor packed with Ni-Cu-Co-Mo / La-γ-Al2O3 main reaction catalyst to carry out catalytic reaction, generating reaction products containing morpholine, N-methylmorpholine, water and by-products;
[0009] (2) After the reaction product is cooled to 40~60℃, gas-liquid separation is performed. The gas phase is separated by membrane separation to remove light hydrocarbons and buffered before being recycled to the reactor. The crude liquid product is sequentially fed into the methanol recovery tower and the azeotropic distillation tower. The lowest azeotrope of N-methylmorpholine, N-ethylmorpholine and water is collected from the top of the tower, and the crude morpholine solution is obtained from the bottom of the tower.
[0010] (3) The crude morpholine solution from step (2) is sequentially fed into a medium-pressure dehydration tower and a low-pressure dehydration tower for deep dehydration by pressure swing distillation to obtain dehydrated morpholine;
[0011] (4) The azeotrope collected from the top of the column in step (2) is mixed with liquid ammonia and hydrogen is added. The mixture is then introduced into a by-product conversion reactor filled with a physical mixing catalyst to carry out a dealkylation reaction. The reaction product is then returned to the condensation separation system in step (2) after methylamine and ethylamine are removed by the amine recovery tower.
[0012] (5) The dehydrated morpholine obtained in step (3) is fed into a refining distillation column. Under normal pressure and nitrogen protection, the morpholine product is collected from the side stream at the 30th to 40th theoretical plate from the top of the column.
[0013] Further, the molar ratio of diethylene glycol, methanol and liquid ammonia in step (1) is 1:(1.2~2.0):(6.0~8.0).
[0014] Further, the composition of the main reaction catalyst in step (1) is: Ni 18~22wt%, Cu 6~8wt%, Co 3~5wt%, Mo 1~2wt%, the support is La-modified γ-Al2O3, the La2O3 content is 3~5wt%, and the support pore volume is 0.5~0.7cm. 3 / g, specific surface area 180~220m² 2 / g, average pore size 12~15nm.
[0015] Furthermore, the preparation method of the main reaction catalyst is as follows: Ni, Cu, Co, and Mo nitrate or ammonium salt solutions are impregnated onto the La-γ-Al2O3 support using an equal-volume impregnation method, oxalic acid is added to the impregnation solution as a complexing agent, and the solution is then dried, air-calcined, and activated by H2 / N2 reduction.
[0016] Furthermore, the preparation of the main reaction catalyst includes the following steps:
[0017] (a) Carrier molding:
[0018] Boehmite was mixed with lanthanum nitrate solution, extruded into strips, and calcined at 550℃ for 4 h to obtain La-γ-Al2O3.
[0019] (b) Preparation of impregnation solution:
[0020] Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Co(NO3)2·6H2O, (NH4)6Mo7O 24 Dissolve 4H2O in deionized water according to the target ratio, add oxalic acid equal to the total molar amount of metal ions, and stir until clear;
[0021] (c) Isostatic impregnation:
[0022] The above solution was added dropwise to the carrier, allowed to stand at room temperature for 12 hours, and then dried at 110°C for 12 hours.
[0023] (d) Calcination and reduction:
[0024] The catalyst was calcined at 550°C for 4 hours in air and then reduced at 450°C for 4 hours in a mixed atmosphere of H2 / N2 (volume ratio 1:4) to obtain the main reaction catalyst.
[0025] Furthermore, the conditions for the catalytic reaction are: temperature 220~240℃, pressure 1.6~2.0MPa, and liquid hourly space velocity 0.6~1.2h. -1 (Calculated as diethylene glycol).
[0026] Further, the operating conditions of the methanol recovery tower in step (2) are: atmospheric pressure, theoretical plate 15~20, reflux ratio 1.5~2.0; the operating conditions of the azeotropic distillation tower are: atmospheric pressure, theoretical plate 40~50, reflux ratio 2.5~3.5.
[0027] Further, the theoretical plate size of the medium-pressure dehydration tower in step (3) is 35~40, the reflux ratio is 2.0~2.5, the operating pressure is 0.25~0.35MPa, and the tower bottom temperature is ≤175℃;
[0028] The theoretical plate size of the low-pressure dehydration tower is 30~35 mm, the reflux ratio is 1.5~2.0, and the tower bottom is equipped with an online moisture meter and interlocked control with the bottom sampling. The operating pressure is 0.02~0.04 MPa, the tower bottom temperature is ≤120℃, and the tower bottom yields dehydrated morpholine with a water content of ≤0.04%.
[0029] Furthermore, the mass ratio of the azeotrope to liquid ammonia in step (4) is 1:(0.8~1.2);
[0030] The physically mixed catalyst is mechanically mixed from 60% P-ZSM-5 (P loading 1~3wt%) and 40% Ni-Mo / Al2O3 (Ni 8~12wt%, Mo 1~3wt%).
[0031] Furthermore, the preparation method of the P-ZSM-5 is as follows: commercially available H-ZSM-5 (Si / Al=50) is ion-exchanged with 0.1M (NH4)2HPO4 solution at 80℃ for 4h, filtered, washed, dried, and calcined at 550℃ for 4h;
[0032] The preparation method of Ni-Mo / Al2O3 is as follows: using γ-Al2O3 as a support, Ni(NO3)2 and (NH4)6Mo7O are co-impregnated in equal volumes. 24 Dry and reduce with H2 at 450℃.
[0033] The dealkylation conditions are: temperature 240~270℃, pressure 1.2~1.6MPa, and mass hourly space velocity 1.5~2.5h. -1 ;
[0034] The amount of hydrogen added is 3 to 6% of the reactor inlet gas volume.
[0035] Furthermore, the operating conditions of the amine recovery tower in step (4) are: atmospheric pressure, theoretical plate size 20~30, reflux ratio 1.5~2.5, methylamine and ethylamine mixture is collected from the top of the tower, and the bottom material is returned to the condensation separation system in step (2).
[0036] Furthermore, the theoretical number of plates in the refining distillation column described in step (5) is 55~65, the reflux ratio is 3.5~5.0, a trace amount of nitrogen is introduced into the top of the column for protection, and heavy components are intermittently discharged from the bottom of the column.
[0037] The present invention has the following advantages over the prior art:
[0038] 1. This invention eliminates the impact of liquid-phase feed on the catalyst and the occurrence of side reactions by using diethylene glycol as a single superheated gas-phase feed and a high ammonia ratio synergistically. A Ni-Cu-Co-Mo / La-γ-Al₂O₃ multi-metal catalyst is employed, utilizing the electronic modulation of Co and the stabilizing effect of Mo to improve the overall selectivity of diethylene glycol to 92-94%. Based on this, deep dehydration is achieved through medium- and low-pressure swing distillation to reduce the product moisture content to below 0.04%, followed by side stream collection from the refining tower, ultimately yielding high-quality morpholine with a purity ≥99.85% and a color ≤10 APHA, meeting the application requirements of pharmaceutical-grade high-end rubber additives.
[0039] 2. The diethylene glycol superheated vaporization feed of this invention eliminates the risks of catalyst bed flooding and carbon deposition. The La-modified γ-Al₂O₃ support significantly suppresses the hydrothermal phase transition, thereby improving catalyst lifespan. The byproduct conversion unit uses a physically mixed catalyst in conjunction with an amine recovery tower, avoiding the problems of easy core-shell structure detachment and light amine accumulation, resulting in a long service life. Simultaneously, the simplified dual-tower pressure swing distillation avoids the thermal decomposition of morpholine in the high-temperature range above 180℃, and combined with gas-phase circulating membrane separation for impurity removal and atmospheric pressure nitrogen-protected purification, the overall energy consumption is low.
[0040] 3. This invention selectively converts N-methylmorpholine and N-ethylmorpholine, which are discharged as low-value fore-distillates in traditional processes, into morpholine under mild conditions via a dealkylation reaction, and recovers byproducts methylamine and ethylamine for use as chemical feedstocks or fuels. This invention achieves significant improvements in product quality, raw material efficiency, and operating costs, and has excellent industrial application value. Detailed Implementation
[0041] To further explain the present invention, the following specific embodiments are described.
[0042] Example 1
[0043] A process for producing high-purity morpholine includes the following steps:
[0044] (1) Diethylene glycol was separately superheated to 270°C and vaporized, while methanol and liquid ammonia were vaporized to 80°C respectively. The mixture was then introduced into a fixed-bed reactor packed with Ni-Cu-Co-Mo / La-γ-Al2O3 main catalyst at a temperature of 220°C, a pressure of 1.6 MPa, and a liquid hourly space velocity of 0.6 h⁻¹. -1 Under certain conditions, a catalytic reaction is carried out to produce reaction products containing morpholine, N-methylmorpholine, water, and byproducts;
[0045] The main reaction catalyst has the following composition: Ni 18wt%, Cu 6wt%, Co 3wt%, Mo 1wt%, with La-modified γ-Al₂O₃ as the support, La₂O₃ content 3wt%, and support pore volume 0.5 cm⁻¹. 3 / g, specific surface area 180m² 2 / g, average pore size 12nm;
[0046] The preparation of the main reaction catalyst includes the following steps:
[0047] (a) Carrier molding:
[0048] Boehmite was mixed with lanthanum nitrate solution, extruded into strips, and calcined at 550℃ for 4 h to obtain La-γ-Al2O3.
[0049] (b) Preparation of impregnation solution:
[0050] Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Co(NO3)2·6H2O, (NH4)6Mo7O 24 Dissolve 4H2O in deionized water according to the target ratio, add oxalic acid equal to the total molar amount of metal ions, and stir until clear;
[0051] (c) Isostatic impregnation:
[0052] The above solution was added dropwise to the carrier, allowed to stand at room temperature for 12 hours, and then dried at 110°C for 12 hours.
[0053] (d) Calcination and reduction:
[0054] The catalyst was calcined at 550°C for 4 hours in air and then reduced at 450°C for 4 hours in a mixed atmosphere of H2 / N2 (volume ratio 1:4) to obtain the main reaction catalyst.
[0055] (2) After the reaction product is cooled to 40°C, gas-liquid separation is performed. The gas phase is separated by membrane separation to remove light hydrocarbons and buffered before being recycled to the reactor. The crude liquid product is sequentially fed into the methanol recovery tower and the azeotropic distillation tower. The lowest azeotrope of N-methylmorpholine, N-ethylmorpholine and water is collected from the top of the tower, and the crude morpholine solution is obtained from the bottom of the tower.
[0056] The operating conditions for the methanol recovery tower are: atmospheric pressure, 15 theoretical plates, and a reflux ratio of 1.5; the operating conditions for the azeotropic distillation tower are: atmospheric pressure, 40 theoretical plates, and a reflux ratio of 2.5.
[0057] (3) The crude morpholine solution from step (2) is sequentially fed into a medium-pressure dehydration tower and a low-pressure dehydration tower for deep dehydration by pressure swing distillation to obtain dehydrated morpholine;
[0058] The medium-pressure dehydration tower has a theoretical plate size of 35, a reflux ratio of 2.0, an operating pressure of 0.25 MPa, and a bottom temperature of ≤175℃.
[0059] The low-pressure dehydration tower has a theoretical plate size of 30 mm, a reflux ratio of 1.5, and is equipped with an online moisture meter in the tower bottom and interlocked with the bottom sampling control. The operating pressure is 0.02 MPa, the tower bottom temperature is ≤120℃, and the tower bottom yields dehydrated morpholine with a water content of ≤0.04%.
[0060] (4) The azeotrope collected from the top of the column in step (2) is mixed with liquid ammonia at a mass ratio of 1:0.8, and hydrogen is added. The amount of hydrogen added is 3% of the gas volume at the reactor inlet. The mixture is then introduced into a by-product conversion reactor packed with a physically mixed catalyst at a temperature of 240℃, a pressure of 1.2MPa, and a mass hourly space velocity of 1.5h. -1Under the conditions of dealkylation reaction, the reaction product is returned to the condensation separation system of step (2) after methylamine and ethylamine are removed by amine recovery tower;
[0061] The physically mixed catalyst is mechanically mixed from 60% P-ZSM-5 (P loading 1wt%) and 40% Ni-Mo / Al2O3 (Ni 8wt%, Mo 1wt%).
[0062] The preparation method of P-ZSM-5 is as follows: commercially available H-ZSM-5 (Si / Al=50) is ion exchanged with 0.1M (NH4)2HPO4 solution at 80℃ for 4 hours, filtered, washed, dried, and calcined at 550℃ for 4 hours.
[0063] The preparation method of Ni-Mo / Al2O3 is as follows: using γ-Al2O3 as a support, Ni(NO3)2 and (NH4)6Mo7O are co-impregnated in equal volumes. 24 Drying and reduction with H2 at 450℃;
[0064] The operating conditions of the amine recovery tower are: atmospheric pressure, theoretical plate 20, reflux ratio 1.5, methylamine and ethylamine mixture is collected from the top of the tower, and the bottom material is returned to the condensation and separation system of step (2);
[0065] (5) The dehydrated morpholine obtained in step (3) is fed into a refining distillation column. Under normal pressure and nitrogen protection, the morpholine product is collected from the side stream at the 30th theoretical plate from the top of the column.
[0066] The refining distillation column has a theoretical plate number of 55, a reflux ratio of 3.5, a trace amount of nitrogen gas is introduced at the top of the column for protection, and heavy components are intermittently discharged from the bottom of the column.
[0067] Example 2
[0068] A process for producing high-purity morpholine includes the following steps:
[0069] (1) Diethylene glycol was separately superheated to 280°C and vaporized, while methanol and liquid ammonia were vaporized to 100°C respectively. The mixture was then introduced into a fixed-bed reactor packed with Ni-Cu-Co-Mo / La-γ-Al2O3 main reaction catalyst at a temperature of 230°C, a pressure of 1.8 MPa, and a liquid hourly space velocity of 0.9 h⁻¹. -1 Under certain conditions, a catalytic reaction is carried out to produce reaction products containing morpholine, N-methylmorpholine, water, and byproducts;
[0070] The main reaction catalyst has the following composition: Ni 20wt%, Cu 7wt%, Co 4wt%, Mo 1.5wt%, and the support is La-modified γ-Al₂O₃ with a La₂O₃ content of 4wt% and a support pore volume of 0.6 cm⁻¹. 3 / g, specific surface area 200m² 2 / g, average pore size 13.5nm;
[0071] The preparation method is the same as in Example 1.
[0072] (2) After the reaction product is cooled to 50°C, gas-liquid separation is performed. The gas phase is separated by membrane separation to remove light hydrocarbons and buffered before being recycled to the reactor. The crude liquid product is successively fed into the methanol recovery tower and the azeotropic distillation tower. The lowest azeotrope of N-methylmorpholine, N-ethylmorpholine and water is collected from the top of the tower, and the crude morpholine solution is obtained from the bottom of the tower.
[0073] The operating conditions for the methanol recovery tower are: atmospheric pressure, 18 theoretical plates, and a reflux ratio of 1.8; the operating conditions for the azeotropic distillation tower are: atmospheric pressure, 45 theoretical plates, and a reflux ratio of 3.0.
[0074] (3) The crude morpholine solution from step (2) is sequentially fed into a medium-pressure dehydration tower and a low-pressure dehydration tower for deep dehydration by pressure swing distillation to obtain dehydrated morpholine;
[0075] The medium-pressure dehydration tower has a theoretical plate size of 38, a reflux ratio of 2.3, an operating pressure of 0.30 MPa, and a bottom temperature of ≤175℃.
[0076] The low-pressure dehydration tower has a theoretical plate size of 33, a reflux ratio of 1.8, and is equipped with an online moisture meter in the tower bottom and interlocked with the bottom sampling control. The operating pressure is 0.03 MPa, the tower bottom temperature is ≤120℃, and the tower bottom yields dehydrated morpholine with a water content of ≤0.04%.
[0077] (4) The azeotrope collected from the top of the column in step (2) is mixed with liquid ammonia at a mass ratio of 1:1.0, and hydrogen is added. The amount of hydrogen added is 4.5% of the gas volume at the reactor inlet. The mixture is then introduced into a by-product conversion reactor packed with a physically mixed catalyst at a temperature of 255℃, a pressure of 1.4MPa, and a mass hourly space velocity of 2.0h. -1 Under the conditions of dealkylation reaction, the reaction product is returned to the condensation separation system of step (2) after methylamine and ethylamine are removed by amine recovery tower;
[0078] The physically mixed catalyst is composed of 60% P-ZSM-5 (P loading 2wt%) and 40% Ni-Mo / Al2O3 (Ni 10wt%, Mo 2wt%) mechanically mixed.
[0079] The preparation methods of P-ZSM-5 and Ni-Mo / Al2O3 are the same as in Example 1;
[0080] The operating conditions of the amine recovery tower are: atmospheric pressure, theoretical plate 25, reflux ratio 2.0, methylamine and ethylamine mixture is collected from the top of the tower, and the bottom material is returned to the condensation and separation system of step (2);
[0081] (5) The dehydrated morpholine obtained in step (3) is fed into a refining distillation column. Under normal pressure and nitrogen protection, the morpholine product is collected from the side stream at the 35th theoretical plate from the top of the column.
[0082] The refining distillation column has a theoretical plate number of 60, a reflux ratio of 4.2, a trace amount of nitrogen gas is introduced at the top of the column for protection, and heavy components are intermittently discharged at the bottom of the column.
[0083] Example 3
[0084] A process for producing high-purity morpholine includes the following steps:
[0085] (1) Diethylene glycol was separately superheated to 290°C and vaporized, while methanol and liquid ammonia were vaporized to 120°C respectively. The mixture was then introduced into a fixed-bed reactor packed with Ni-Cu-Co-Mo / La-γ-Al2O3 main catalyst at a temperature of 240°C, a pressure of 2.0 MPa, and a liquid hourly space velocity of 1.2 h⁻¹. -1 Under certain conditions, a catalytic reaction is carried out to produce reaction products containing morpholine, N-methylmorpholine, water, and byproducts;
[0086] The main reaction catalyst has the following composition: Ni 22wt%, Cu 8wt%, Co 5wt%, Mo 2wt%, with La-modified γ-Al₂O₃ as the support, La₂O₃ content 5wt%, and support pore volume 0.7 cm⁻¹. 3 / g, specific surface area 220m² 2 / g, average pore size 15nm;
[0087] The preparation method is the same as in Example 1;
[0088] (2) After the reaction product is cooled to 60°C, gas-liquid separation is performed. The gas phase is separated by membrane separation to remove light hydrocarbons and buffered before being recycled to the reactor. The crude liquid product is sequentially fed into the methanol recovery tower and the azeotropic distillation tower. The lowest azeotrope of N-methylmorpholine, N-ethylmorpholine and water is collected from the top of the tower, and the crude morpholine solution is obtained from the bottom of the tower.
[0089] The operating conditions for the methanol recovery tower are: atmospheric pressure, 20 theoretical plates, and a reflux ratio of 2.0; the operating conditions for the azeotropic distillation tower are: atmospheric pressure, 50 theoretical plates, and a reflux ratio of 3.5.
[0090] (3) The crude morpholine solution from step (2) is sequentially fed into a medium-pressure dehydration tower and a low-pressure dehydration tower for deep dehydration by pressure swing distillation to obtain dehydrated morpholine;
[0091] The medium-pressure dehydration tower has a theoretical plate size of 40 mm, a reflux ratio of 2.5, an operating pressure of 0.35 MPa, and a bottom temperature of ≤175°C.
[0092] The low-pressure dehydration tower has a theoretical plate size of 35 mm, a reflux ratio of 2.0, and is equipped with an online moisture meter in the tower bottom and interlocked with the bottom sampling control. The operating pressure is 0.04 MPa, the tower bottom temperature is ≤120℃, and the tower bottom yields dehydrated morpholine with a water content of ≤0.04%.
[0093] (4) The azeotrope collected from the top of the column in step (2) is mixed with liquid ammonia at a mass ratio of 1:1.2, and hydrogen is added. The amount of hydrogen added is 6% of the gas volume at the reactor inlet. The mixture is then introduced into a by-product conversion reactor packed with a physically mixed catalyst at a temperature of 270°C, a pressure of 1.6 MPa, and a mass hourly space velocity of 2.5 h⁻¹. -1 Under the conditions of dealkylation reaction, the reaction product is returned to the condensation separation system of step (2) after methylamine and ethylamine are removed by amine recovery tower;
[0094] The physically mixed catalyst is composed of 60% P-ZSM-5 (P loading 3wt%) and 40% Ni-Mo / Al2O3 (Ni 12wt%, Mo 3wt%) mechanically mixed.
[0095] The preparation methods of P-ZSM-5 and Ni-Mo / Al2O3 are the same as in Example 1;
[0096] The operating conditions of the amine recovery tower are: atmospheric pressure, theoretical plate size 30, reflux ratio 2.5, methylamine and ethylamine mixture is collected from the top of the tower, and the bottom material is returned to the condensation and separation system of step (2);
[0097] (5) The dehydrated morpholine obtained in step (3) is fed into a refining distillation column. Under normal pressure and nitrogen protection, the morpholine product is collected from the side stream at the 40th theoretical plate from the top of the column.
[0098] The refining distillation column has a theoretical plate number of 65, a reflux ratio of 5.0, a trace amount of nitrogen gas is introduced at the top of the column for protection, and heavy components are intermittently discharged from the bottom of the column.
[0099] Comparative Example 1
[0100] Compared with Example 2, in Comparative Example 1, diethylene glycol was not superheated and vaporized separately. Instead, diethylene glycol, methanol, and liquid ammonia were mixed and heated together to 230°C using conventional methods, reducing the ammonia / diethylene glycol molar ratio to 3.5. The remaining parameters were the same as in Example 2.
[0101] Comparative Example 2
[0102] Compared with Example 2, the main reaction catalyst in Comparative Example 2 was replaced with conventional Ni-Cu / γ-Al2O3 (Ni 20wt%, Cu 8wt%), which does not contain Co and Mo, and the support was unmodified γ-Al2O3 (without La stabilization). The other parameters were the same as in Example 2.
[0103] Comparative Example 3
[0104] Compared with Example 2, in Comparative Example 3, the crude morpholine solution was dehydrated by single-tower atmospheric pressure azeotropic distillation, without passing through medium-pressure and low-pressure variable pressure distillation towers, and the other parameters were the same as in Example 2.
[0105] Comparative Example 4
[0106] Compared with Example 2, Comparative Example 4 uses a core-shell structured catalyst P-ZSM-5@NiO (prepared according to the original method) in the byproduct conversion unit, without an amine recovery tower, and the other parameters are the same as in Example 2.
[0107] Morpholine was prepared using the methods described in Examples 1-3 and Comparative Examples 1-4, respectively, and its performance was then tested under the same conditions.
[0108] 1. Testing Methods
[0109] (1) Purity of Morpholine product
[0110] According to the standard GB / T 28608-2012, gas chromatography was used for detection.
[0111] (2) Moisture content
[0112] The Karl Fischer method was used for testing, in accordance with the standard GB / T 6283-2008.
[0113] (3) Chromaticity
[0114] According to the standard GB / T 3143, the platinum-cobalt colorimetric method was used for detection.
[0115] (4) Diethylene glycol conversion rate
[0116] According to the standard GB / T 28608-2012, the residual diethylene glycol in the product was analyzed by gas chromatography.
[0117] 2. Test Results
[0118] Each experiment was run continuously for 720 hours under the same conditions, and the average value of the stable operation period (240~720h) was taken. The results are summarized in Table 1 below.
[0119] Table 1
[0120] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Morpholine purity (%) 99.85 99.87 99.86 99.12 99.35 99.05 99.42 Moisture (%) 0.03 0.03 0.04 0.06 0.05 0.18 0.04 Chromaticity (APHA) 8 ≤10 ≤10 15 12 14 11 Total selectivity of diethylene glycol (%) 92.3 92.8 93.1 83.7 85.2 90.1 89.5 N-methylmorpholine conversion rate (%) 96.2 96.8 96.5 95.8 96.2 96.0 93.5 Main catalyst lifetime (h) >2000 >2000 >2000 450 800 >2000 >2000 Byproduct conversion catalyst lifetime (h) >1000 >1200 >1200 >1000 >1000 >1000 650
[0121] As shown in Table 1 above, the performance of Examples 1-3 is significantly better than that of the Comparative Example. Comparative Example 1 used mixed heating to introduce diethylene glycol into the reactor as droplets, leading to catalyst coking, increased pressure drop, and a lifespan of only 450 hours. The low ammonia ratio exacerbated side reactions, reducing the overall selectivity to 83.7%, and the product purity, moisture content, and color were all inferior to those of Example 2. This invention uses superheated gas-phase feed and a high ammonia ratio, eliminating liquid film and carbon, and increasing the overall selectivity to 92.8%.
[0122] Comparative Example 2 used conventional Ni-Cu / γ-Al2O3, achieving a total selectivity of 85.2%, product purity of 99.35%, moisture content of 0.05%, and catalyst lifetime of 800 hours. This demonstrates that the Co introduced in this invention regulates the electronic structure to suppress cracking side reactions, Mo improves resistance to carbon deposition, and La-modified support inhibits hydration phase transition, resulting in a total selectivity of 92.8% and a catalyst lifetime >2000 hours.
[0123] Comparative Example 3 used single-tower atmospheric pressure azeotropic distillation, but due to the azeotropic limitation, the moisture content was only reduced to 0.18%, and the product color was 14 APHA. This invention removes most of the water first in a medium-pressure tower, followed by deep dehydration in a low-pressure tower. The tower bottom temperature is ≤175℃ to avoid thermal decomposition of morpholine, resulting in a moisture content ≤0.04% and a color ≤10 APHA.
[0124] Comparative Example 4 used a core-shell structure P-ZSM-5@NiO without amine recovery. After 800 hours, the shell detached, NiO agglomerated, and the catalyst lifetime was only 650 hours. Due to the accumulation of methylamine and ethylamine in the system, the main reaction atmosphere was disturbed, and the overall selectivity dropped to 89.5%. This invention uses a physically mixed catalyst without interface detachment problems, and the conversion rate is stable at over 96.8%. Combined with an amine recovery tower to separate low-boiling substances, the overall selectivity is maintained at 92.8%, and the catalyst lifetime is >1200 hours.
[0125] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A production process for high-purity morpholine, characterized in that, Includes the following steps: (1) Diethylene glycol is heated and vaporized separately, mixed with vaporized methanol and liquid ammonia, and then introduced into a fixed-bed reactor packed with Ni-Cu-Co-Mo / La-γ-Al2O3 main reaction catalyst to carry out catalytic reaction, generating reaction products containing morpholine, N-methylmorpholine, water and by-products; (2) After the reaction product is cooled, the gas and liquid are separated. The gas phase is separated by membrane separation to remove light hydrocarbons and then buffered and recycled to the reactor. The crude liquid product enters the methanol recovery tower and the azeotropic distillation tower in sequence. The lowest azeotrope of N-methylmorpholine, N-ethylmorpholine and water is collected from the top of the tower, and the crude morpholine solution is obtained from the bottom of the tower. (3) The crude morpholine solution was sequentially fed into a medium-pressure dehydration tower and a low-pressure dehydration tower for deep dehydration by pressure swing distillation to obtain dehydrated morpholine; (4) The azeotrope collected from the top of the column in step (2) is mixed with liquid ammonia and hydrogen is added. The mixture is then introduced into a byproduct conversion reactor filled with a physical mixing catalyst to carry out a dealkylation reaction. The reaction product is returned to the condensation separation system in step (2) after methylamine and ethylamine are removed by the amine recovery tower. (5) The dehydrated morpholine is fed into a refining distillation column. Under normal pressure and nitrogen protection, the morpholine product is collected from the side stream at the 30th to 40th theoretical plate from the top of the column.
2. The method according to claim 1, characterized in that, The molar ratio of diethylene glycol, methanol and liquid ammonia in step (1) is 1:(1.2~2.0):(6.0~8.0).
3. The method according to claim 1, characterized in that, The main reaction catalyst in step (1) has the following composition: Ni 18~22wt%, Cu 6~8wt%, Co 3~5wt%, Mo 1~2wt%, and the support is La-modified γ-Al2O3 with a La2O3 content of 3~5wt% and a support pore volume of 0.5~0.7cm. 3 / g, specific surface area 180~220m² 2 / g, average pore size 12~15nm.
4. The method according to claim 3, characterized in that, The preparation method of the main reaction catalyst is as follows: Ni, Cu, Co and Mo nitrate or ammonium salt solutions are impregnated into the La-γ-Al2O3 support by equal volume impregnation method, oxalic acid is added to the impregnation solution as a complexing agent, and then the solution is dried, air-calcined and H2 / N2 reduced and activated.
5. The method according to claim 1, characterized in that, The conditions for the catalytic reaction are: temperature 220~240℃, pressure 1.6~2.0MPa, and liquid hourly space velocity 0.6~1.2h. -1 .
6. The method according to claim 1, characterized in that, The operating conditions of the methanol recovery tower in step (2) are: atmospheric pressure, theoretical plate 15~20, reflux ratio 1.5~2.0; the operating conditions of the azeotropic distillation tower are: atmospheric pressure, theoretical plate 40~50, reflux ratio 2.5~3.
5.
7. The method according to claim 1, characterized in that, The theoretical plate size of the medium-pressure dehydration tower mentioned in step (3) is 35~40, the reflux ratio is 2.0~2.5, the operating pressure is 0.25~0.35MPa, and the tower bottom temperature is ≤175℃; The theoretical plate size of the low-pressure dehydration tower is 30~35 mm, the reflux ratio is 1.5~2.0, and the tower bottom is equipped with an online moisture meter and interlocked control with the bottom sampling. The operating pressure is 0.02~0.04 MPa, and the tower bottom temperature is ≤120℃.
8. The method according to claim 1, characterized in that, The mass ratio of the azeotrope to liquid ammonia in step (4) is 1:(0.8~1.2); The physically mixed catalyst is mechanically mixed from 60% P-ZSM-5 (P loading 1~3wt%) and 40% Ni-Mo / Al2O3 (Ni 8~12wt%, Mo 1~3wt%). The dealkylation conditions are: temperature 240~270℃, pressure 1.2~1.6MPa, and mass hourly space velocity 1.5~2.5h. -1 ; The amount of hydrogen added is 3 to 6% of the reactor inlet gas volume.
9. The method according to claim 1, characterized in that, The operating conditions of the amine recovery tower in step (4) are: atmospheric pressure, theoretical plate size 20~30, reflux ratio 1.5~2.5, methylamine and ethylamine mixture is collected from the top of the tower, and the bottom material is returned to the condensation and separation system in step (2).
10. The method according to claim 1, characterized in that, The theoretical number of plates in the refining distillation column described in step (5) is 55~65, the reflux ratio is 3.5~5.0, a small amount of nitrogen is introduced into the top of the column for protection, and heavy components are intermittently discharged from the bottom of the column.