A polycarboxylate surfactant and its preparation method
By optimizing the raw material combination and the dropping process, the problems of insufficient dispersion performance, complex copolymerization process and molecular weight control of existing polycarboxylate surfactants have been solved, achieving a highly efficient and uniform copolymerization reaction, obtaining high conversion rate and excellent dispersion performance, and making it suitable for coatings, detergents and water treatment and other fields.
Patent Information
- Application Number
- CN202611135489.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polycarboxylate surfactants have shortcomings in terms of dispersion performance, copolymerization process complexity, difficulty in molecular weight control, and limited dropwise addition methods, resulting in problems such as low dispersion efficiency, complex processes, uneven molecular weight, and high residual monomer levels.
Using methacrylic acid, styrene, sodium styrene sulfonate, sodium allyl sulfonate, ammonium persulfate, n-dodecyl mercaptan, benzyl triethyl ammonium chloride, and sodium hypophosphite as raw materials, a free radical copolymerization reaction was carried out. An acetone/water mixed solvent was used to control the copolymerization temperature and the dropping method. A non-synchronous dropping process of 'oil phase first, oil phase completely dropped' was adopted. Combined with the chain transfer effect of n-dodecyl mercaptan and sodium hypophosphite, the molecular weight distribution was controlled.
It achieves high conversion rate, narrow molecular weight distribution, excellent dispersion performance and low residual monomer, improves the dispersion stability and hard water resistance of hydrophobic particles, avoids gelation, and ensures the uniformity of copolymer composition and product safety.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of surfactant technology, specifically to a polycarboxylate surfactant and its preparation method, and more particularly to a polycarboxylate surfactant copolymerized from methacrylic acid, styrene, sodium styrene sulfonate and sodium allyl sulfonate, as well as the preparation method of the surfactant and its application in a dispersion system. Background Technology
[0002] Polycarboxylate surfactants (such as sodium polyacrylate and sodium methacrylate-styrene copolymer) are widely used as dispersants in coatings, detergents, ceramics, water treatment, and other fields. However, existing technologies still have the following drawbacks:
[0003] First, its dispersion performance is insufficient. Ordinary sodium polyacrylate has low dispersion efficiency for hydrophobic organic pigments such as carbon black and phthalocyanine blue, and it still easily settles even when added at levels as high as 30% of the pigment mass; In hard water with a concentration of ≥500ppm, the dispersing power decreases by more than 60%; for high specific surface area powders such as nano-silica, it may even cause agglomeration and particle size increase.
[0004] Secondly, the copolymerization process is complex. Styrene and methacrylic acid have significantly different hydrophilicities, leading to phase separation, gelation, or adhesion to the walls during the initial polymerization stages in water or alcohol-water mixed solvents. To avoid these problems, existing methods often involve continuously adding styrene dropwise over 4-6 hours, or adding it in three steps with strict control of temperature and pH, resulting in a total reaction time exceeding 12 hours. If methanol / water solvent is used, methanol forms an azeotrope with water, requiring high energy consumption for distillation recovery, and residual methanol can affect product safety.
[0005] Third, molecular weight is difficult to control. When using only dodecyl mercaptan as a chain transfer agent, its distribution in the heterogeneous system is uneven, with batch-to-batch weight-average molecular weight fluctuations exceeding ±40%, and a wide molecular weight distribution (PDI is typically greater than 2.5). A reaction temperature fluctuation of ±5℃ can cause the molecular weight to change several times. Although some literature mentions using sodium hypophosphite to assist chain transfer, improper formulation can lead to a polymerization conversion rate of less than 60% or a product molecular weight exceeding 100 kDa, resulting in gel formation.
[0006] Fourth, the dropwise addition method is singular. Existing technologies typically involve mixing all monomers and reacting them all at once, or using two processes that are added and terminated simultaneously. This leads to excessive styrene in the early stages of polymerization, causing homopolymerization side reactions, uneven copolymer sequence distribution, high residual monomer levels, and affecting product dispersion performance.
[0007] Therefore, there is an urgent need to develop a novel polycarboxylate surfactant with excellent dispersion properties, simple copolymerization process, and controllable molecular weight, as well as its preparation method. Summary of the Invention
[0008] The present invention aims to provide a polycarboxylate surfactant with excellent dispersion performance, simple copolymerization process and easy molecular weight control, and its preparation method, so as to overcome the shortcomings of the prior art.
[0009] To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution:
[0010] A polycarboxylate surfactant is prepared by free radical copolymerization from the following raw materials in parts by weight:
[0011] Methacrylic acid: 200-300 parts;
[0012] Styrene: 200-300 parts;
[0013] Sodium styrene sulfonate: 5-10 parts;
[0014] Sodium allyl sulfonate: 5-10 parts;
[0015] Ammonium persulfate: 20-35 parts;
[0016] dodecanethiol: 1-5 parts;
[0017] Benzyltriethylammonium chloride: 1-5 parts;
[0018] Sodium hypophosphite: 10-20 parts.
[0019] Furthermore, the solvent used in the preparation process is an acetone / water mixed solvent, with a volume ratio of acetone to water of 1:1 to 3:1; the total volume of the acetone / water mixed solvent is 1.0 to 2.0 times the total mass of all monomers (volume unit is mL, mass unit is g); the neutralizing agent is an aqueous solution of sodium hydroxide or potassium hydroxide.
[0020] Furthermore, the copolymerization reaction temperature is 60~80℃, and after the reaction is completed, the system is neutralized with alkali to a pH of 7~9.
[0021] The present invention also provides a method for preparing the above-mentioned polycarboxylate surfactant, comprising the following steps:
[0022] (1) Preparation of base material and two phases: Mix methacrylic acid, styrene and n-dodecyl mercaptan evenly to form an oil phase; dissolve ammonium persulfate in 2 to 4 times its mass of deionized water to form an aqueous phase; dissolve sodium styrene sulfonate, sodium allyl sulfonate, benzyl triethyl ammonium chloride and sodium hypophosphite in acetone / water mixed solvent and add it to the reactor as base material. The stirring speed is controlled at 200 to 300 r / min; before the reaction, purge the reactor with nitrogen for 10 to 40 min to replace the air in the system. The reaction is protected by a nitrogen atmosphere throughout.
[0023] (2) Non-synchronous addition: Heat to 60~80℃, start adding oil phase at a constant rate first; 5 minutes after the oil phase starts adding, start adding water phase at a constant rate; the total time t1 for adding oil phase is 10 minutes shorter than the total time t2 for adding water phase, that is, t1=t2–10.
[0024] (3) Heat preservation polymerization: After the oil phase is completely added, continue to add the aqueous phase until the aqueous phase is completely added, and maintain the temperature to continue the polymerization reaction for 0.5 to 1 hour;
[0025] (4) Neutralization treatment: Cool down to below 40°C and neutralize with alkaline solution to pH 7~9, so that the carboxylic acid groups form salts;
[0026] (5) Post-processing: Acetone is recovered by vacuum distillation at a temperature of 40~50℃ and a vacuum degree of ≥0.08MPa. Deionized water is added to adjust the solid content of the product to 25~35wt% to obtain an aqueous solution of polycarboxylate surfactant; or a solid powder is obtained by spray drying.
[0027] Preferably, the oil phase drop time t1 is 40-60 minutes, and the aqueous phase drop time t2 is 50-70 minutes.
[0028] The present invention has the following advantages over the prior art:
[0029] (1) The simultaneous introduction of two small-molecule rigid sulfonate monomers, sodium styrene sulfonate and sodium allyl sulfonate, synergistically improves the hard water resistance of the surfactant and the dispersion stability of hydrophobic particles.
[0030] (2) Using the ammonium persulfate-sodium hypophosphite redox initiation system, combined with the double chain transfer effect of n-dodecyl mercaptan and sodium hypophosphite, controllable polymerization can be achieved at a lower temperature. The weight average molecular weight of the product is controlled between 5000 and 50000, the molecular weight distribution is ≤2.0, and the total monomer conversion rate is ≥90%.
[0031] (3) Adding benzyltriethylammonium chloride as a phase transfer catalyst significantly improves the copolymerization uniformity of styrene and hydrophilic monomers and avoids layering and gelation during the polymerization process.
[0032] (4) The final product is a carboxylate / sulfonate composite structure. The surface tension of the 0.1% aqueous solution is ≤35mN / m. It has excellent dispersion effect on pigments such as carbon black and good electrolyte resistance.
[0033] (5) A unique asynchronous dropping process is adopted, in which the oil phase is added first and the oil phase is completely added first. The oil phase is added 5 minutes earlier than the aqueous phase, so that a certain amount of hydrophobic polymer seeds are formed in the reaction system first, which is conducive to the uniform copolymerization of styrene in the later stage. The oil phase is added 10 minutes earlier than the aqueous phase, which effectively avoids the side reaction of styrene homopolymerization caused by excessively high concentration of free styrene in the system in the later stage of polymerization, and ensures that the copolymer composition is uniform, the residual monomer is low, and the molecular weight distribution is narrow.
[0034] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Detailed Implementation
[0035] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0036] The present invention will be further illustrated below through specific embodiments. Experimental methods not specifically described in the embodiments are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used are commercially available industrial products.
[0037] (a) Performance testing methods
[0038] Conversion rate: The content of nonvolatile matter was determined by weighing method, and the total conversion rate of monomers was calculated.
[0039] Molecular weight and distribution: Gel permeation chromatography (GPC) was used, with polyethylene glycol as standard and 0.1 mol / L NaNO3 aqueous solution as mobile phase.
[0040] Surface tension: The surface tension of a 0.1 wt% aqueous solution was measured at 25 °C using the Wilhelmy dipstick method.
[0041] Dispersion performance: A 30wt% aqueous color paste was prepared using carbon black (DBP value 35mL / 100g) as the pigment and 20% of the carbon black mass as the dispersant. After standing for 2 hours, the supernatant was collected, and the transmittance (T%) was measured using a UV-Vis spectrophotometer. The lower the transmittance, the better the dispersibility. The Zeta potential of the color paste was also measured simultaneously.
[0042] Electrolyte resistance: Add 1000 ppm Ca to a 0.5 wt% dispersant aqueous solution. 2+ (In the form of CaCl2), the change in the transmittance of the solution was measured.
[0043] Residual styrene monomer: determined by gas chromatography.
[0044] (II) Implementation Examples
[0045] Example 1:
[0046] Raw material dosage: 240g methacrylic acid, 240g styrene, 6.25g sodium styrene sulfonate, 6.25g sodium allyl sulfonate, 28.75g ammonium persulfate, 2.5g dodecyl mercaptan, 2.5g benzyltriethylammonium chloride, 16.25g sodium hypophosphite.
[0047] Solvent: 600 mL of acetone and 300 mL of deionized water (volume ratio 2:1) are used as the solvent for the bottom material of the reactor. Separately, 80 mL of deionized water is used to dissolve ammonium persulfate to prepare an aqueous phase.
[0048] Preparation method:
[0049] (1) Preparation of oil phase: Mix 240g of methacrylic acid, 240g of styrene and 2.5g of n-dodecyl mercaptan evenly and place them in a constant pressure dropping funnel for later use.
[0050] (2) Preparation of aqueous phase: Dissolve 28.75g of ammonium persulfate in 80mL of deionized water, stir until completely dissolved, and place in another constant pressure dropping funnel for later use.
[0051] (3) Preparation of the base material: Add 6.25g of sodium styrene sulfonate, 6.25g of sodium allyl sulfonate, 2.5g of benzyl triethylammonium chloride, and 16.25g of sodium hypophosphite to the reactor, then add 600mL of acetone and 300mL of deionized water, and stir to dissolve (stirring speed 250r / min). Purge with nitrogen for 30min (nitrogen flow rate: 200ml / min), and heat to 70℃.
[0052] (4) Dropping procedure: First, start dropping the oil phase at a rate of approximately 3.6 mL / min (total dropping time approximately 50 minutes). Five minutes after the oil phase has started dropping, start dropping the aqueous phase at a rate of approximately 1.3 mL / min (total volume of the aqueous solution containing ammonium persulfate approximately 80 mL, total dropping time approximately 60 minutes). The oil phase is dropped completely after 50 minutes, and the aqueous phase is dropped continuously for another 10 minutes until it is dropped completely after 60 minutes.
[0053] (5) Post-polymerization: After the aqueous phase is added, continue stirring at 70°C for 30 minutes.
[0054] (6) Neutralization and post-treatment: Cool to 40℃ and neutralize to pH=8 with 30% sodium hydroxide solution. Recover acetone by vacuum distillation (temperature controlled at 40-45℃, vacuum degree ≥0.08MPa), add water to adjust to a solid content of 30%, and obtain a pale yellow transparent liquid product.
[0055] The resulting products underwent performance testing, and the results are listed in Table 1.
[0056] Example 2:
[0057] Except for the following differences, the contents were the same as in Example 1: 200g methacrylic acid, 280g styrene, 20g ammonium persulfate, 4g n-dodecyl mercaptan, and 20g sodium hypophosphite; the oil phase was added over 40 minutes, and the aqueous phase was added over 50 minutes. The results are shown in Table 1.
[0058] Example 3:
[0059] Except for the following differences, the process was the same as in Example 1: 20g ammonium persulfate, 4g dodecanethiol; oil phase addition time 60 minutes, aqueous phase addition time 70 minutes. Solvent: 300mL acetone and 300mL deionized water (volume ratio 1:1). Polymerization temperature 65℃. Results are shown in Table 1.
[0060] (III) Comparative Example
[0061] Comparative Example 1 (Two identical start-stop methods, mixed and added dropwise)
[0062] All monomers (methacrylic acid, styrene, sodium styrene sulfonate, sodium allyl sulfonate), n-dodecyl mercaptan, benzyltriethylammonium chloride, and sodium hypophosphite were mixed and dissolved in acetone / water to form a mixed solution, while ammonium persulfate was prepared separately as an aqueous phase. Both phases were added dropwise simultaneously and completely (each addition time was 60 minutes), and the rest was the same as in Example 1. The results are shown in Table 1.
[0063] Comparative Example 2 (two identical start-stop operations, no pre-dropping)
[0064] The oil phase and water phase were added simultaneously and completed at the same time (each addition time was 50 minutes), without a 5-minute pre-addition, and the rest was the same as in Example 1. The results are shown in Table 1.
[0065] Comparative Example 3 (Oil phase finishes later than aqueous phase)
[0066] The oil phase and water phase were added simultaneously. The oil phase was added over 60 minutes, and the water phase was added over 50 minutes (the oil phase was added 10 minutes later than the water phase). The rest was the same as in Example 1. The results are shown in Table 1.
[0067] Comparative Example 4 (using methanol instead of acetone)
[0068] The solvent was changed to 600 mL of methanol and 300 mL of deionized water, with the remaining formulation and operation the same as in Example 1. An esterification odor was generated during polymerization, the reaction solution turned yellow, and the product had a residual methanol smell. The results are shown in Table 1.
[0069] Comparative Example 5 (without phase transfer catalyst)
[0070] Benzyltriethylammonium chloride was omitted, and the rest was the same as in Example 1. During polymerization, the system exhibited obvious stratification, with styrene floating on the surface, and unreacted styrene droplets present in the post-reaction product. The results are shown in Table 1.
[0071] Comparative Example 6 (without sodium hypophosphite)
[0072] Sodium hypophosphite was omitted, and the rest was the same as in Example 1. The polymerization rate was extremely fast; after 2 hours, the system became jelly-like and could not be stirred, and the product was an insoluble gel. The results are shown in Table 1.
[0073] (iv) Performance test results and analysis
[0074]
[0075] Table 1: Performance test results of each embodiment and comparative example;
[0076] As can be seen from the data in Table 1, Examples 1-3, using the phase-separated asynchronous dropping process of the present invention, which involves "dropping the oil phase for 5 minutes first and dropping the oil phase 10 minutes earlier than the aqueous phase," achieved a conversion rate as high as 94-96%, a narrow molecular weight distribution (PDI≤1.85), a surface tension as low as 31-32 mN / m, excellent carbon black dispersion performance (transmittance≤17.8%, Zeta potential≤-48.1mV), extremely low residual styrene monomer (≤112ppm), and good electrolyte resistance (transmittance≤27.6% after calcium addition).
[0077] Comparative Examples 1-3, using different dropping methods, showed significantly inferior conversion rates, molecular weight distributions, dispersion performance, and residual monomers compared to the present invention. In particular, Comparative Example 3 (where the oil phase ended later than the aqueous phase) resulted in severe homopolymerization of styrene, with residual monomers reaching as high as 528 ppm. Comparative Example 4, using methanol instead of acetone, resulted in lower conversion rates, larger and wider molecular weight distributions, and significantly reduced dispersion performance. Comparative Example 5, without the addition of benzyltriethylammonium chloride, exhibited uneven copolymerization, a conversion rate of only 58.6%, and poor dispersion. Comparative Example 6, without the addition of sodium hypophosphite, resulted in runaway polymerization and gel formation.
[0078] The above results demonstrate that the present invention has achieved unexpected technical effects through unique raw material combinations, solvent selection, and asynchronous dropping processes of "oil phase added first and oil phase dropped completely first".
[0079] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A polycarboxylate surfactant, characterized in that, It is copolymerized from methacrylic acid, styrene, sodium styrene sulfonate and sodium allyl sulfonate as monomers; and the polymerization system contains ammonium persulfate, n-dodecyl mercaptan, benzyltriethylammonium chloride and sodium hypophosphite.
2. The polycarboxylate surfactant according to claim 1, characterized in that, The weight proportions of each raw material are as follows: 200-300 parts of methacrylic acid; 200-300 parts of styrene; 5-10 parts of sodium styrene sulfonate; 5-10 parts of sodium allyl sulfonate; 20-35 parts of ammonium persulfate; 1-5 parts of n-dodecyl mercaptan; 1-5 parts of benzyltriethylammonium chloride; 10-20 parts of sodium hypophosphite.
3. The polycarboxylate surfactant according to claim 2, characterized in that, The solvent used in its preparation is a mixture of acetone and water, with a volume ratio of acetone to water of 1:1 to 3:
1.
4. The polycarboxylate surfactant according to claim 2, characterized in that, The copolymerization reaction temperature is 60~80℃, and after the reaction is completed, the pH is neutralized with alkali to 7~9.
5. A method for preparing the polycarboxylate surfactant according to any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Mix methacrylic acid, styrene and n-dodecyl mercaptan evenly to form an oil phase; dissolve ammonium persulfate in deionized water to form an aqueous phase; dissolve sodium styrene sulfonate, sodium allyl sulfonate, benzyl triethyl ammonium chloride and sodium hypophosphite in acetone / water mixed solvent, add to the reactor as the base material, and purge with nitrogen for protection. (2) Heat the temperature to 60~80℃ and start adding the oil phase first; 5 minutes after the oil phase starts adding, start adding the water phase; the total time for adding the oil phase t1 is 10 minutes shorter than the total time for adding the water phase t2, i.e., t1=t2–10; (3) After the oil phase is completely added, continue to add the aqueous phase until the aqueous phase is completely added, and keep the temperature for polymerization for 0.5 to 1 hour; (4) After cooling, neutralize with alkali to pH 7-9; (5) The solvent is recovered by vacuum distillation, and water is added to adjust the solid content.
6. The preparation method according to claim 5, characterized in that, The oil phase drop time t1 is 40~60 minutes, and the aqueous phase drop time t2 is 50~70 minutes.
7. The use of the polycarboxylate surfactant according to any one of claims 1 to 4 or the polycarboxylate surfactant prepared by the preparation method according to claim 5 or 6 in pigment dispersion, emulsion polymerization or textile auxiliaries.