A low molecular weight, hydroxyl-terminated polyphenylene ether and its method for continuous polymerization based on submerged rotating packed bed
By employing an organic-water biphase polymerization system and a submerged rotating packed bed continuous polymerization method, the problems of low catalyst removal efficiency and poor gas-liquid mass transfer efficiency in the preparation of low molecular weight dihydroxyl-terminated polyphenylene ethers were solved, achieving an efficient and stable polymerization process that meets the performance requirements of high-frequency communication materials.
Patent Information
- Application Number
- CN202611087294.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the preparation of low molecular weight double-hydroxyl-terminated polyphenylene ethers suffers from low catalyst removal efficiency, poor gas-liquid mass transfer efficiency, difficulty in temperature control, and challenges in continuous production, making it difficult to meet the requirements of high-frequency communication materials for low dielectric loss and processing performance.
An organic-water biphase polymerization system and a submerged rotating packed bed continuous polymerization method are adopted. By separating the catalyst into liquid and liquid phases, gas-liquid mass and heat transfer are enhanced. The strong shear and turbulence effects of the rotating packed bed internal components are utilized, combined with an overflow liquid phase outlet and integrated heat exchange components, to achieve continuous and stable preparation.
It improves catalyst removal efficiency, reduces metal residue, enhances gas-liquid contact area and mixing uniformity, and enables continuous and efficient production of low molecular weight double-hydroxyl-terminated polyphenylene ether, thereby improving product quality stability and production efficiency.
Smart Images

Figure CN123107066A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer material preparation and chemical process intensification technology, and particularly to a low molecular weight double-hydroxyl-terminated polyphenylene ether and a method for continuous polymerization based on an immersed rotating packed bed. Background Technology
[0002] Polyphenylene ether (PPE) possesses excellent heat resistance, dimensional stability, and electrical insulation properties, making it widely used in high-frequency communications and electronic packaging. With the development of technologies such as 5G communications and artificial intelligence, higher demands are being placed on materials with low dielectric constants, low dielectric losses, and excellent processing performance. Low molecular weight, hydroxyl-terminated PPE, due to its good flowability and the presence of active terminal hydroxyl groups, can further react with epoxy resins, cyanate ester resins, etc., showing promising application prospects in high-frequency, high-speed electronic materials.
[0003] These polymers are typically obtained by oxidative coupling polymerization of 2,6-dimethylphenol and bisphenol monomers under copper salt / organic amine catalysis. The reaction medium is mostly organic solvents such as toluene and methanol, and the catalyst relies on subsequent complexation and water washing for removal. Copper ions have weak solubility and migration ability in organic systems, resulting in low removal efficiency, requiring multiple washings, complex processes, and high costs. Residual copper ions degrade dielectric properties and reliability, making it difficult to meet the low dielectric loss requirements of high-frequency communication materials.
[0004] Meanwhile, this polymerization is a gas-liquid multiphase reaction, and the oxygen mass transfer efficiency significantly affects the polymerization rate and product quality. Furthermore, the polymerization process has an exothermic effect, requiring high temperature control. Existing processes mostly use bubbling or stirred reactors, which suffer from low gas-liquid mass transfer efficiency, uneven bubble distribution, and limited heat transfer capacity. This easily leads to localized concentration and temperature differences, affecting polymerization stability, and also results in poor batch stability and difficulty in continuous production.
[0005] Therefore, there is an urgent need to develop a preparation technology that takes into account both the optimization of the polymerization system and the enhancement of continuous process, so as to improve the catalyst removal efficiency, reduce metal residue, enhance gas-liquid mass and heat transfer, achieve continuous and stable operation, and meet the requirements of high-performance communication materials for processability and dielectric properties while ensuring efficient polymerization. Summary of the Invention
[0006] The first technical problem to be solved by this application is to provide a low molecular weight, double-hydroxyl-terminated polyphenylene ether.
[0007] The second technical problem this application aims to solve is to provide a polymerization method for low molecular weight dihydroxyl-terminated polyphenylene ethers based on submerged rotating packed bed continuous polymerization. This polymerization method involves introducing an appropriate amount of water into an organic solvent to construct an organic-aqueous biphase polymerization system. Since the post-treatment of copper salt-catalyzed oxidative coupling polymerization typically requires catalyst removal using an aqueous chelating agent, introducing an aqueous phase into the polymerization system does not increase the complexity of the post-treatment process. After polymerization, the aqueous phase, carrying most of the copper catalyst and its complexes, can be separated from the organic phase by liquid-liquid separation. This reduces the amount of chelating agent and the number of washing cycles required in the subsequent organic phase chelation treatment, simplifies the post-treatment process, and lowers production costs, thus facilitating the production of low molecular weight dihydroxyl-terminated polyphenylene ethers with low copper ion residue. This polymerization method employs a submerged rotating packed bed polymerization reactor, which disperses and shears oxygen to form smaller, uniformly distributed bubbles, increasing the gas-liquid contact area, enhancing the mass transfer of oxygen to the liquid phase, and reducing the phenomenon of excessively high local oxygen concentrations leading to polymerization side reactions. Simultaneously, the strong shear and turbulence generated by the rotating packed bed internal components enhance the mixing of the reaction system, improving reaction uniformity. An overflow liquid phase outlet allows for continuous and stable control of the reaction residence time. Combined with a dual-tube heat exchanger integrated into the reactor, the heat transfer efficiency and temperature control capability of the polymerization process are improved, enabling the continuous, efficient, and stable preparation of low molecular weight, hydroxyl-terminated polyphenylene ethers, thus improving product quality stability and production efficiency. This solves the problems of low gas-liquid mass transfer efficiency, insufficient mixing, difficulty in temperature control, and low continuity in existing gas-liquid multiphase polymerization processes. Testing results show that the product of this invention has a molecular weight ≤3000 g / mol, a molecular weight distribution of 1.20-2.00, a polymer yield ≥75%, and a residual copper content ≤0.25 ppm.
[0008] To solve the first technical problem mentioned above, the present invention adopts the following technical solution: A low molecular weight, hydroxyl-terminated polyphenylene ether is prepared from the following raw materials: 1) monomer system, 2) catalyst system, 3) solvent system, and 4) oxidant. The monomer system includes 2,6-dimethylphenol and bisphenol monomers; The catalyst system includes a copper salt catalyst and an organic amine ligand; The solvent system includes organic solvents and water; The oxidant includes oxygen or oxygen-containing gas.
[0009] Preferably, the bisphenol monomer is one of bisphenol A, 3,3',5,5'-tetramethylbisphenol A, bisphenol F, 4,4'-dihydroxybiphenyl, 4,4'-ethylidene bisphenol and 4,4'-methylenebis(2,6-xylenol).
[0010] Preferably, the copper salt catalyst is one of copper chloride, copper bromide, copper iodide, cuprous chloride, cuprous bromide, copper sulfate, and copper acetate.
[0011] Preferably, the organic amine ligand is one or more of di-n-butylamine, pyridine, 4-dimethylaminopyridine, N,N-dimethylethylenediamine, N-methylbenzylamine, N,N,N',N'-tetramethylethylenediamine, and triethylamine; more preferably, the organic amine ligand is one or more of 4-dimethylaminopyridine, N,N-dimethylethylenediamine, and N-methylbenzylamine.
[0012] Preferably, the organic solvent is one or more of toluene, xylene, chlorobenzene, dichloromethane, chloroform, tetrahydrofuran, and acetonitrile.
[0013] To solve the second technical problem mentioned above, the present invention adopts the following technical solution: A polymerization method for low molecular weight dihydroxyl-terminated polyphenylene ethers based on submerged rotating packed bed continuous polymerization includes the following steps: 1) Check the sealing of the submerged rotating packed bed polymerization reactor and the continuous post-treatment system, and confirm that all delivery pumps, flow meters, motors and control systems are operating normally; start the heat exchange system to continuously feed the heat exchange medium into the heat exchange components of the polymerization reactor, and adjust the flow rate and temperature of the heat exchange medium to establish the temperature control conditions required for the polymerization reaction. 2) The first liquid phase feed includes 2,6-dimethylphenol, bisphenol monomer, organic amine ligand, and organic solvent; the second liquid phase feed includes copper salt catalyst and water; the two liquid phases are continuously delivered by metering pumps and heated to the set temperature by preheating devices, and then continuously enter the center of the filling internals of the submerged rotating packed bed polymerization reactor from their respective liquid phase inlets; as the liquid phases continuously enter, the reaction liquid gradually fills the reactor, keeping the filling internals submerged, and maintaining a stable liquid level through the overflow liquid phase outlet; 3) Start the motor and adjust it to the set speed to form a stable hypergravity field in the area of the filling internal components; then open the oxygen inlet pipe, adjust it to the set flow rate, and continuously introduce it into the central cavity of the filling internal components of the polymerization reactor; under the hypergravity field, the oxygen is dispersed into fine and uniform bubbles and fully contacts the liquid phase to carry out the polymerization reaction, thereby enhancing gas-liquid mass transfer and mixing; at the same time, the heat of polymerization reaction is removed in time by the heat exchange components of the polymerization reactor to maintain a stable reaction temperature; 4) After the polymerization system has stabilized, the polymerization product flows out continuously from the liquid phase outlet and enters the receiving tank; the receiving tank is used to buffer the continuous discharge and to achieve the initial separation of the microbubbles entrained in the liquid phase from the liquid phase. The separated gas is discharged through the top of the receiving tank, and the liquid phase product is continuously transported to the post-processing unit. 5) The liquid phase product undergoes a series of post-processing steps, including reaction termination, chelation, precipitation and washing, and devolatilization and drying, to obtain a low molecular weight double-hydroxyl-terminated polyphenylene ether product.
[0014] Preferably, in step 1), the submerged rotating packed bed polymerization reactor includes a shell, a motor, a liquid-phase feed assembly, a gas-phase feed assembly, a heat exchange assembly, baffles, packing internals, a guide tube, a liquid-phase outlet, a gas-phase outlet, and a material discharge port; the shell includes an elliptical head, an annular cylinder, and a lower end cover; the liquid-phase feed assembly includes a liquid inlet, a liquid inlet chamber, and a liquid inlet pipe; the liquid inlet is located at the top of the elliptical head, the liquid inlet chamber is located inside the elliptical head, and the liquid inlet pipe is located at the lower part of the liquid inlet chamber. Extending downwards to the central cavity of the filling internal component; the liquid inlet, liquid inlet chamber, and liquid inlet pipe are sequentially connected; the gas phase feeding assembly includes an air inlet, an air inlet pipe, and an air distribution head; the air inlet is located at the top of the elliptical head, the air inlet pipe extends downwards to the central cavity of the filling internal component, and the air distribution head is located at the lower end of the air inlet pipe; the air inlet, air inlet pipe, and air distribution head are sequentially connected; the heat exchange assembly includes a heat exchange medium inlet, a heat exchange cavity, a heat exchange tube bundle, and a heat exchange medium outlet; the heat exchange cavity includes a first heat exchange cavity, a second... Two heat exchange chambers and a third heat exchange chamber; the heat exchange tube bundle includes a first heat exchange tube bundle and a second heat exchange tube bundle; the first heat exchange chamber and the third heat exchange chamber are respectively disposed on the left and right sides inside the upper elliptical head of the reactor; the second heat exchange chamber is disposed below the heat exchange tube bundle inside the reactor; the heat exchange medium inlet, the first heat exchange chamber, the first heat exchange tube bundle, the second heat exchange chamber, the second heat exchange tube bundle, the third heat exchange chamber, and the heat exchange medium outlet are sequentially connected; the baffle is disposed at the lower end of the second heat exchange chamber; the filling internal structure The rotating shaft of the external motor is located below the baffle; the guide tube is axially positioned at the center of the reactor interior, and is a vertically continuous cylinder, with its lower end fixedly connected to the lower edge of the baffle, so that the interior of the guide tube is in communication with the central cavity of the filling internal component; the liquid inlet pipe and the gas inlet pipe both extend into the interior of the guide tube and extend axially along the guide tube to the central cavity of the filling internal component; the liquid phase outlet is located at the upper part of the annular cylinder; the gas phase outlet is located at the top of the elliptical head; and the material discharge port is located at the bottom of the lower end cover.
[0015] Preferably, the liquid inlet pipe includes 2-18 axially arranged distribution pipes; the distribution pipes are distributed circumferentially and extend to the central cavity region of the filling internal component; the outlet of the distribution pipe is provided with a liquid distribution structure; the liquid distribution structure is one or more of the following: circumferential opening structure, radial opening structure, axial opening structure, slit structure or nozzle structure.
[0016] More preferably, the number of the dispensing tubes is 4-8.
[0017] More preferably, the liquid distribution structure is a radially perforated structure with 4-24 perforations.
[0018] Preferably, the air distribution head is one or more of the following: a multi-hole air distribution head, a micro-hole air distribution head, a slit air distribution head, or a nozzle air distribution head.
[0019] Preferably, the heat exchange tube bundle extends along the reactor axis and is evenly distributed circumferentially within the reactor, located in the outer region of the guide tube; the number of heat exchange tube bundles is 2-24; the heat exchange tube bundle is provided with an enhanced heat exchange structure, which is one or more of the following: spiral structure, inner fin structure, outer fin structure, corrugated structure, or surface-reinforced structure.
[0020] Preferably, the heat exchange component is connected to an external temperature control system; the heat exchange medium in the heat exchange component is one of water, heat transfer oil, steam, and refrigerant.
[0021] Preferably, the number of baffles is 2-16; the baffles are flat baffle structures.
[0022] Preferably, the filling internal components include, but are not limited to, one or more combinations of structured packing, irregular packing, wire mesh packing, column packing, mesh column packing, blade structure, guide plate structure, spiral channel structure, porous media structure, and stator / rotor structure.
[0023] Preferably, in step 2), the mass concentration of 2,6-dimethylphenol is 5-20 wt%; the molar ratio of 2,6-dimethylphenol to bisphenol monomer is 4:1-20:1; the molar ratio of 2,6-dimethylphenol to copper salt is 30:1-110:1; the molar ratio of copper salt to organic amine ligand is 1:30-1:110; the volume ratio of organic solvent to water is 9:1-5:5; and the volumetric flow rate ratio of the first liquid phase feed to the second liquid phase feed is 1.5:1-20:1.
[0024] Preferably, in step 2), the set temperature is 20-70℃.
[0025] Preferably, in step 3), the polymerization reaction temperature is 20-70℃; the set rotation speed is 300-1200 rpm; and the molar ratio of oxygen to 2,6-dimethylphenol is 0.4:1-2:1.
[0026] Preferably, in step 3), the average residence time of the liquid phase material is 30-120 min.
[0027] Preferably, in step 5), a terminator is added to terminate the oxidative coupling polymerization; the terminator is one or more of hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, formic acid and their aqueous solutions.
[0028] Preferably, in step 5), a chelating agent is added to complex the residual copper catalyst in the chelation treatment process; the chelating agent is one or more of ethylenediaminetetraacetic acid and its salt, diethylenetriaminepentaacetic acid and its salt, hypozinotriacetic acid and its salt, and citric acid and its salt.
[0029] Preferably, in step 5), an antisolvent is added to the precipitation and washing process to precipitate low molecular weight double-terminated hydroxyl polyphenylene ether; the antisolvent is one or more of methanol, ethanol, isopropanol and acetone; the washing process uses one or more of water, methanol and ethanol for washing.
[0030] Preferably, in step 5), the devolatilization drying process is carried out by heating and drying under normal or reduced pressure to remove residual moisture and organic solvents.
[0031] Any range described in this invention includes the endpoint, any value between the endpoints, and any subrange consisting of the endpoint or any value between the endpoints.
[0032] Unless otherwise specified, all raw materials used in this invention can be obtained commercially, and the equipment used in this invention can be conventional equipment in the relevant field or refer to existing technology in the relevant field.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1) This invention constructs an organic-aqueous biphase polymerization system. While ensuring the stable oxidative coupling polymerization of low molecular weight, hydroxyl-terminated polyphenylene ethers, most of the copper catalyst and its complexes can be separated from the aqueous phase by liquid-liquid separation after the reaction, achieving preliminary catalyst removal. This reduces the amount of chelating agent and the number of washing cycles in the subsequent organic phase chelation treatment, simplifies the post-processing, reduces production costs, and effectively reduces residual metal ions in the product. Characterization results of the product from this invention show a molecular weight ≤3000 g / mol, a molecular weight distribution of 1.20-2.00, a polymer yield ≥75%, and a residual copper content ≤0.25 ppm.
[0035] 2) This invention uses a submerged rotating packed bed as a continuous polymerization reactor. Under the action of guiding, dispersing and shearing, oxygen forms small and uniformly distributed bubbles, which significantly increases the gas-liquid contact area and enhances the mass transfer process of oxygen to the liquid phase. At the same time, the strong shearing and turbulence generated by the rotating packed internal components enhance the mixing of the reaction system, suppress side reactions caused by excessively high local oxygen concentration, and improve the stability of the polymerization reaction and the consistency of product quality.
[0036] 3) This invention adopts a continuous feeding, continuous polymerization and continuous discharge process, uses an overflow liquid phase outlet to stably control the reaction residence time, and uses an integrated double-pass heat exchange component to enhance the heat transfer and temperature control of the polymerization reaction, thereby realizing the continuous, efficient and stable preparation of low molecular weight double-hydroxyl-terminated polyphenylene ether, improving production efficiency, product batch stability and industrial application level. Attached Figure Description
[0037] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings. Figure 1 This is a schematic diagram of the continuous polymerization process of low molecular weight dihydroxyl-terminated polyphenylene ether based on an immersed rotating packed bed polymerization reactor according to the present invention. Figure 2 This is a schematic diagram of the continuous polymerization method for low molecular weight double-hydroxyl-terminated polyphenylene ether of the present invention; Figure 3 This is a schematic diagram of the submerged rotating packed bed polymerization reactor used in this invention. Detailed Implementation
[0038] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. Those skilled in the art should understand that the specific descriptions below are illustrative rather than restrictive, and should not be construed as limiting the scope of protection of the present invention.
[0039] Various cross-sectional views of embodiments of the present invention are shown in the accompanying drawings. These drawings are not to scale, and some details have been enlarged for clarity, and some details may have been omitted. The shapes of the various regions and layers shown in the drawings, as well as their relative sizes and positional relationships, are merely exemplary and may deviate from reality due to manufacturing tolerances or technical limitations. Furthermore, those skilled in the art can design regions / layers with different shapes, sizes, and relative positions as needed.
[0040] It should be noted that when a component is said to be "fixed to" another component, it can be directly or indirectly attached to that other component. When a component is said to be "connected to" another component, it can be directly or indirectly connected to that other component.
[0041] It should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention.
[0042] As one aspect of the present invention, a low molecular weight double-hydroxyl-terminated polyphenylene ether is prepared from the following raw materials: 1) monomer system, 2) catalyst system, 3) solvent system, and 4) oxidant. The monomer system includes 2,6-dimethylphenol and bisphenol monomers; The catalyst system includes a copper salt catalyst and an organic amine ligand; The solvent system includes organic solvents and water; The oxidant includes oxygen or oxygen-containing gas.
[0043] According to certain embodiments of the present invention, the bisphenol monomer is one of bisphenol A, 3,3',5,5'-tetramethylbisphenol A, bisphenol F, 4,4'-dihydroxybiphenyl, 4,4'-ethylidene bisphenol and 4,4'-methylenebis(2,6-xylenol).
[0044] According to certain embodiments of the present invention, the copper salt catalyst is one of copper chloride, copper bromide, copper iodide, cuprous chloride, cuprous bromide, copper sulfate, and copper acetate.
[0045] According to certain embodiments of the present invention, the organic amine ligand is one or more of di-n-butylamine, pyridine, 4-dimethylaminopyridine, N,N-dimethylethylenediamine, N-methylbenzylamine, N,N,N',N'-tetramethylethylenediamine, and triethylamine; more preferably, the organic amine ligand is one or more of 4-dimethylaminopyridine, N,N-dimethylethylenediamine, and N-methylbenzylamine.
[0046] According to certain embodiments of the present invention, the organic solvent is one or more of toluene, xylene, chlorobenzene, dichloromethane, chloroform, tetrahydrofuran, and acetonitrile.
[0047] As another aspect of the invention, see Figure 1 and Figure 2 As shown, the present invention discloses a polymerization method for low molecular weight dihydroxyl-terminated polyphenylene ethers based on continuous polymerization in a submerged rotating packed bed, comprising the following steps: 1) Check the sealing of the submerged rotating packed bed polymerization reactor and the continuous post-treatment system, and confirm that all delivery pumps, flow meters, motors and control systems are operating normally; start the heat exchange system to continuously feed the heat exchange medium into the heat exchange components of the polymerization reactor, and adjust the flow rate and temperature of the heat exchange medium to establish the temperature control conditions required for the polymerization reaction. 2) The first liquid phase feed includes 2,6-dimethylphenol, bisphenol monomer, organic amine ligand, and organic solvent; the second liquid phase feed includes copper salt catalyst and water; the two liquid phases are continuously delivered by metering pumps and heated to the set temperature by preheating devices, and then continuously enter the center of the filling internals of the submerged rotating packed bed polymerization reactor from their respective liquid phase inlets; as the liquid phases continuously enter, the reaction liquid gradually fills the reactor, keeping the filling internals submerged, and maintaining a stable liquid level through the overflow liquid phase outlet; 3) Start the motor and adjust it to the set speed to form a stable hypergravity field in the area of the filling internal components; then open the oxygen inlet pipe, adjust it to the set flow rate, and continuously introduce it into the central cavity of the filling internal components of the polymerization reactor; under the hypergravity field, the oxygen is dispersed into fine and uniform bubbles and fully contacts the liquid phase to carry out the polymerization reaction, thereby enhancing gas-liquid mass transfer and mixing; at the same time, the heat of polymerization reaction is removed in time by the heat exchange components of the polymerization reactor to maintain a stable reaction temperature; 4) After the polymerization system has stabilized, the polymerization product flows out continuously from the liquid phase outlet and enters the receiving tank; the receiving tank is used to buffer the continuous discharge and to achieve the initial separation of the microbubbles entrained in the liquid phase from the liquid phase. The separated gas is discharged through the top of the receiving tank, and the liquid phase product is continuously transported to the post-processing unit. 5) The liquid phase product undergoes a series of post-processing steps, including reaction termination, chelation, precipitation and washing, and devolatilization and drying, to obtain a low molecular weight double-hydroxyl-terminated polyphenylene ether product.
[0048] According to certain embodiments of the present invention, see Figure 3As shown in step 1), the submerged rotating packed bed polymerization reactor 200 includes a shell, a motor 20, a liquid feed assembly, a gas feed assembly, a heat exchange assembly, a baffle 60, a packing internal component, a guide tube 80, a liquid outlet 91, a gas outlet 92, and a material discharge port 93; the shell includes an elliptical head 11, an annular cylinder 12, and a lower end cover 13; the liquid feed assembly includes an inlet 31, an inlet chamber 32, and an inlet pipe 33; the inlet 31 is located at the top of the elliptical head 11, the inlet chamber 32 is located inside the elliptical head 11, and the inlet pipe 33 is located at the lower part of the inlet chamber 32, extending downward to the central cavity of the packing internal component; the inlet 31, the inlet chamber 32, and the inlet... The liquid pipes 33 are connected in sequence; the liquid inlet chamber 32 is used to collect and buffer the liquid phase material; the liquid inlet pipe 33 is used to distribute and transport the liquid phase material to the filling internal component area; the gas phase feeding assembly includes an air inlet 41, an air inlet pipe 42, and an air distribution head 43; the air inlet 41 is located at the top of the elliptical head 11, the air inlet pipe 42 extends downward to the central cavity of the filling internal component, and the air distribution head 43 is located at the lower end of the air inlet pipe 42; the air inlet 41, the air inlet pipe 42, and the air distribution head 43 are connected in sequence; the air distribution head 43 is used to initially disperse the gas phase material and then introduce it into the filling internal component area; the heat exchange assembly includes a heat exchange medium inlet 51, a heat exchange cavity, a heat exchange tube bundle, and a heat exchange medium outlet 54; the heat exchange cavity includes a first heat exchange... The reactor comprises a first heat exchange chamber 521, a second heat exchange chamber 522, and a third heat exchange chamber 523; the heat exchange tube bundle includes a first heat exchange tube bundle 531 and a second heat exchange tube bundle 532; the first heat exchange chamber 521 and the third heat exchange chamber 523 are respectively located on the left and right sides inside the upper elliptical head 11 of the reactor; the second heat exchange chamber 522 is located below the heat exchange tube bundle inside the reactor; the heat exchange medium inlet 51, the first heat exchange chamber 521, the first heat exchange tube bundle 531, the second heat exchange chamber 522, the second heat exchange tube bundle 532, the third heat exchange chamber 523, and the heat exchange medium outlet 54 are sequentially connected; the heat exchange assembly is used to remove the heat released by the polymerization reaction or replenish the heat required for the reaction in a timely manner; the baffle 60 is located in the second heat exchange chamber. The lower end of body 522 is used to turbulent the reaction medium, suppress vortices caused by overall rotational flow, and promote gas-liquid mixing and uniform bubble dispersion. The rotating shaft of the motor 20 is externally connected to the filling inner component 70 and is located below the baffle. The guide tube 80 is axially arranged at the center of the reactor, and is a vertically continuous cylinder. Its lower end is fixedly connected to the lower edge of the baffle 60, so that the interior of the guide tube is in communication with the central cavity of the filling inner component 70. The liquid inlet pipe 33 and the gas inlet pipe 42 both extend into the interior of the guide tube and extend axially along the guide tube to the central cavity of the filling inner component 70. The guide tube 80 is used to guide the circulating flow of the reactants, so that the reactants circulate through the area of the filling inner component 70, thereby enhancing the mixing and mass transfer process.The liquid phase outlet 91 is located on the upper part of the annular cylinder 12; the liquid phase outlet 91 is used to continuously extract the material after the reaction and control the reactor liquid level by overflow, providing the required residence time for the reaction system; the gas phase outlet 92 is located on the top of the elliptical head 11; the material discharge port 93 is located at the bottom of the lower end cover 13; it is used to drain the liquid in the reactor during reactor cleaning and maintenance.
[0049] According to certain embodiments of the present invention, the liquid inlet pipe 33 includes 2-18 axially arranged liquid distribution pipes; the liquid distribution pipes are distributed circumferentially and extend to the central cavity region of the filling inner member 70; the outlet of the liquid distribution pipe is provided with a liquid distribution structure; the liquid distribution structure is one or more of the following: circumferential opening structure, radial opening structure, axial opening structure, slit structure or nozzle structure.
[0050] According to certain embodiments of the present invention, the number of the dispensing tubes is 4-8.
[0051] According to some embodiments of the present invention, the liquid distribution structure is a radially perforated structure with 4-24 perforations.
[0052] According to certain embodiments of the present invention, the air distribution head 43 is one or more of a porous air distribution head, a microporous air distribution head, a slit air distribution head, or a nozzle air distribution head.
[0053] According to certain embodiments of the present invention, the heat exchange tube bundle extends along the reactor axial direction and is uniformly distributed circumferentially within the reactor, and is located in the region outside the guide tube 80; the number of heat exchange tube bundles is 2-24; the heat exchange tube bundle is provided with a heat exchange enhancement structure, which is one or more of a spiral structure, an inner fin structure, an outer fin structure, a corrugated structure, or a surface strengthening structure.
[0054] According to certain embodiments of the present invention, the heat exchange component is externally connected to a temperature control system; the temperature control system is used to control the flow rate and temperature of the heat exchange medium; the heat exchange medium in the heat exchange component is one of water, heat transfer oil, steam, and refrigerant.
[0055] According to some embodiments of the present invention, the number of baffles 60 is 2-16; the baffles 60 are flat baffle structures.
[0056] According to certain embodiments of the present invention, the filling internal component 70 includes, but is not limited to, one or more combinations of structured packing, irregular packing, wire mesh packing, column packing, mesh column packing, blade structure, guide plate structure, spiral channel structure, porous media structure, and stator-rotor structure.
[0057] According to certain embodiments of the present invention, in step 2), the mass concentration of 2,6-dimethylphenol is 5-20 wt%; the molar ratio of 2,6-dimethylphenol to bisphenol monomer is 4:1-20:1; the molar ratio of 2,6-dimethylphenol to copper salt is 30:1-110:1; the molar ratio of copper salt to organic amine ligand is 1:30-1:110; the volume ratio of organic solvent to water is 9:1-5:5; and the volume flow rate ratio of the first liquid phase feed to the second liquid phase feed is 1.5:1-20:1.
[0058] According to some embodiments of the present invention, in step 2), the set temperature is 20-70°C.
[0059] According to certain embodiments of the present invention, in step 3), the temperature of the polymerization reaction is 20-70°C; the set rotation speed is 300-1200 rpm; the molar ratio of oxygen to 2,6-dimethylphenol is 0.4:1-2:1; and the set flow rate of oxygen is calculated based on the aforementioned molar ratio relationship.
[0060] According to certain embodiments of the present invention, in step 3), the average residence time of the liquid phase material is 30-120 min.
[0061] According to certain embodiments of the present invention, in step 5), a terminator is added to terminate the oxidative coupling polymerization; the terminator is one or more of hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, formic acid and their aqueous solutions.
[0062] According to certain embodiments of the present invention, in step 5), a chelating agent is added to complex the residual copper catalyst in the chelation treatment process; the chelating agent is one or more of ethylenediaminetetraacetic acid and its salt, diethylenetriaminepentaacetic acid and its salt, hypozinotriacetic acid and its salt, and citric acid and its salt.
[0063] According to certain embodiments of the present invention, in step 5), an antisolvent is added to the precipitation and washing process to precipitate low molecular weight double-terminated hydroxyl polyphenylene ether; the antisolvent is one or more of methanol, ethanol, isopropanol and acetone; the washing process uses one or more of water, methanol and ethanol for washing.
[0064] According to certain embodiments of the present invention, in step 5), the devolatilization drying process employs heating and drying under normal or reduced pressure conditions to remove residual moisture and organic solvents. Example 1
[0065] See Figure 1 and Figure 2 As shown, a method for polymerizing low molecular weight dihydroxyl-terminated polyphenylene ethers based on continuous polymerization in a submerged rotating packed bed includes the following steps: 1) Preparation of polymerization solution First liquid-phase feed: Add 2,6-dimethylphenol and 3,3',5,5'-tetramethylbisphenol A to toluene, and after complete dissolution, add N-methylbenzylamine and mix thoroughly; control the mass fraction of 2,6-dimethylphenol in the resulting solution to be 10 wt%; The second liquid phase feed: copper bromide is dissolved in water and stirred until completely dissolved to obtain an aqueous catalyst solution; Set the volumetric flow rate ratio of the two liquid feed streams to 5:1; and ensure that the molar ratio of each component entering the reactor meets the following requirements: 2,6-dimethylphenol: 3,3',5,5'-tetramethylbisphenol A: copper bromide: N-methylbenzylamine molar ratio is 50:5:1:90. 2) Start the reactor Two liquid feed streams are continuously fed into the submerged rotating packed bed reactor at a volumetric flow rate ratio of 5:1, and the total liquid flow rate is controlled to ensure that the average residence time of the liquid material is about 60 min. At the same time, the heat exchange system is turned on, and the temperature of the polymerization reactor is controlled at 40℃ through the temperature control system. The motor is started and the speed is adjusted to 600 rpm. 3) Continuous polymerization After stabilization, oxygen is introduced, and the mass flow ratio of oxygen to 2,6-dimethylphenol is controlled at 0.2:1 using a mass flow meter to carry out continuous polymerization. 4) Post-processing After continuous operation to a steady state, the polymer mother liquor drawn from the receiving tank sequentially enters each post-processing step: In the reaction termination step, acetic acid is continuously added to the polymer mother liquor at a volume flow ratio of 15:1, and the reaction is terminated by online mixing. Then, it enters a continuous phase separation device to separate the aqueous phase; In the chelation treatment step, the organic phase is continuously mixed and washed with 5 wt% EDTA-4Na aqueous solution at a volume ratio of 7:3, and the aqueous phase is separated again; In the precipitation and washing step, the obtained organic phase is continuously injected into 3-5 times its volume of methanol to precipitate the polymer, which is then separated by continuous filtration. The filter cake is further washed with an appropriate amount of methanol; In the devolatilization and drying step, the washed filter cake is sent to a devolatilization and drying device to remove volatiles under vacuum to obtain low molecular weight double-hydroxyl-terminated polystyrene.
[0066] Testing and product characterization results showed that the molecular weight was 2514 g / mol, the molecular weight distribution was 1.40, the polymer yield was 75.66%, the residual copper content was 0.16 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.96. Example 2
[0067] Repeat Example 1, except that in step 2), the two liquid feed streams are kept at a volume flow ratio of 5:1, but the total liquid flow rate is reduced, so that the average residence time of the liquid phase material in the reaction system is extended to 70 min.
[0068] The product characterization results showed that the molecular weight was 2493 g / mol, the molecular weight distribution was 1.42, the polymer yield was 81.49%, the residual copper content was 0.19 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.98.
[0069] The results show that the residence time of the reaction system can be controlled by adjusting the liquid feed flow rate; appropriately extending the residence time is beneficial to improving the polymer yield; at the same time, the obtained polymer still maintains a narrow molecular weight distribution, low residual copper content and high hydroxyl functionality, indicating that the method has good residence time control capability and process stability. Example 3
[0070] Repeat Example 1, except that in step 2), the motor speed is increased to 800 rpm.
[0071] The product characterization results showed that the molecular weight was 2484 g / mol, the molecular weight distribution was 1.38, the polymer yield was 78.84%, the residual copper content was 0.17 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.97.
[0072] The results show that appropriately increasing the rotation speed can further enhance gas-liquid mass transfer and mixing, improve polymer yield, and at the same time maintain the product molecular weight, molecular weight distribution, residual copper content and hydroxyl functionality at a better level. Example 4
[0073] Repeat Example 1, except that in step 1), the molar ratio of 2,6-dimethylphenol to copper bromide is 30:1.
[0074] The product characterization results showed that the molecular weight was 2036 g / mol, the molecular weight distribution was 1.65, the polymer yield was 78.92%, the residual copper content was 0.23 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.96.
[0075] The results show that catalyst concentration is a crucial factor affecting polymer molecular weight. Increasing the catalyst concentration can decrease the polymer molecular weight, but it also broadens the molecular weight distribution. Therefore, it is necessary to rationally control the catalyst concentration to balance molecular weight regulation and product uniformity. Example 5
[0076] Example 2 was repeated, except that in step 1), the molar ratio of 2,6-dimethylphenol to 3,3',5,5'-tetramethylbisphenol A was 8:1.
[0077] The product characterization results showed that the molecular weight was 2262 g / mol, the molecular weight distribution was 1.39, the polymer yield was 75.68%, the residual copper content was 0.19 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.99.
[0078] The results show that adjusting the molar ratio of the two monomers can control the polymer molecular weight. Decreasing the molar ratio reduces the polymer molecular weight, but also broadens the molecular weight distribution, indicating that the monomer ratio has a significant impact on the polymer molecular weight and its distribution. Comparative Example 1
[0079] Repeat Example 1, except that: in step 1), the second liquid feed is replaced with methanol instead of water, and copper bromide is dissolved in methanol to obtain a catalyst solution; in step 2), the submerged rotating packed bed polymerization reactor is replaced with a bubble stirred tank reactor, which uses mechanical stirring and bottom bubbling oxygen supply for continuous polymerization.
[0080] The product characterization results showed that the molecular weight was 2403 g / mol, the molecular weight distribution was 1.78, the polymer yield was 56.03%, the residual copper content was 68.26 ppm, and the hydroxyl functionality determined by the acetic anhydride method was 1.91.
[0081] The results showed that using methanol as the second solvent and a bubbling stirred tank reactor for continuous polymerization resulted in a lower polymer yield, a wider molecular weight distribution, and a significantly higher residual copper content. This indicates that the organic-aqueous biphase polymerization system and the submerged rotating packed bed continuous polymerization process employed in this invention have a good synergistic effect, which is beneficial for enhancing gas-liquid mass transfer and fluid mixing, promoting catalyst removal and product purification, and improving the stability of the polymerization reaction. This leads to the acquisition of low molecular weight dihydroxyl-terminated polyphenylene ethers with higher yields, narrower molecular weight distributions, and lower residual copper content.
[0082] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is impossible to exhaustively list all embodiments here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.
Claims
1. A low molecular weight, hydroxyl-terminated polyphenylene ether, characterized in that, It is prepared from the following raw materials: 1) monomer system, 2) catalyst system, 3) solvent system, and 4) oxidant; The monomer system includes 2,6-dimethylphenol and bisphenol monomers; The catalyst system includes a copper salt catalyst and an organic amine ligand; The solvent system includes organic solvents and water; The oxidant includes oxygen or oxygen-containing gas.
2. The low molecular weight, hydroxyl-terminated polyphenylene ether according to claim 1, characterized in that: The bisphenol monomer is one of bisphenol A, 3,3',5,5'-tetramethylbisphenol A, bisphenol F, 4,4'-dihydroxybiphenyl, 4,4'-ethylidene bisphenol and 4,4'-methylenebis(2,6-xylenol).
3. The low molecular weight, hydroxyl-terminated polyphenylene ether according to claim 1, characterized in that: The copper salt catalyst is one of copper chloride, copper bromide, copper iodide, cuprous chloride, cuprous bromide, copper sulfate, and copper acetate.
4. The low molecular weight, hydroxyl-terminated polyphenylene ether according to claim 1, characterized in that: The organic amine ligand is one or more of di-n-butylamine, pyridine, 4-dimethylaminopyridine, N,N-dimethylethylenediamine, N-methylbenzylamine, N,N,N',N'-tetramethylethylenediamine, and triethylamine; more preferably, the organic amine ligand is one or more of 4-dimethylaminopyridine, N,N-dimethylethylenediamine, and N-methylbenzylamine.
5. The low molecular weight, hydroxyl-terminated polyphenylene ether according to claim 1, characterized in that: The organic solvent is one or more of toluene, xylene, chlorobenzene, dichloromethane, chloroform, tetrahydrofuran, and acetonitrile.
6. A polymerization method for low molecular weight dihydroxyl-terminated polyphenylene ethers as described in any one of claims 1-5, based on submerged rotating packed bed continuous polymerization, characterized in that, Includes the following steps: 1) Check the sealing of the submerged rotating packed bed polymerization reactor and the continuous post-treatment system, and confirm that all delivery pumps, flow meters, motors and control systems are operating normally; start the heat exchange system to continuously feed the heat exchange medium into the heat exchange components of the polymerization reactor, and adjust the flow rate and temperature of the heat exchange medium to establish the temperature control conditions required for the polymerization reaction. 2) The first liquid phase feed includes 2,6-dimethylphenol, bisphenol monomer, organic amine ligand, and organic solvent; the second liquid phase feed includes copper salt catalyst and water; the two liquid phases are continuously delivered by metering pumps and heated to the set temperature by preheating devices, and then continuously enter the center of the filling internals of the submerged rotating packed bed polymerization reactor from their respective liquid phase inlets; as the liquid phases continuously enter, the reaction liquid gradually fills the reactor, keeping the filling internals submerged, and maintaining a stable liquid level through the overflow liquid phase outlet; 3) Start the motor and adjust it to the set speed to form a stable hypergravity field in the area of the filling internal components; then open the oxygen inlet pipe, adjust it to the set flow rate, and continuously introduce it into the central cavity of the filling internal components of the polymerization reactor; under the hypergravity field, the oxygen is dispersed into fine and uniform bubbles and fully contacts the liquid phase to carry out the polymerization reaction, thereby enhancing gas-liquid mass transfer and mixing; at the same time, the heat of polymerization reaction is removed in time by the heat exchange components of the polymerization reactor to maintain a stable reaction temperature; 4) After the polymerization system has stabilized, the polymerization product flows out continuously from the liquid phase outlet and enters the receiving tank; the receiving tank is used to buffer the continuous discharge and to achieve the initial separation of the microbubbles entrained in the liquid phase from the liquid phase. The separated gas is discharged through the top of the receiving tank, and the liquid phase product is continuously transported to the post-processing unit. 5) The liquid phase product undergoes a series of post-processing steps, including reaction termination, chelation, precipitation and washing, and devolatilization and drying, to obtain a low molecular weight double-hydroxyl-terminated polyphenylene ether product.
7. The polymerization method according to claim 6, characterized in that: In step 1), the submerged rotating packed bed polymerization reactor includes a shell, a motor, a liquid-phase feed assembly, a gas-phase feed assembly, a heat exchange assembly, baffles, packing internals, a guide tube, a liquid-phase outlet, a gas-phase outlet, and a material discharge port; the shell includes an elliptical head, an annular cylinder, and a lower end cover; the liquid-phase feed assembly includes a liquid inlet, a liquid inlet chamber, and a liquid inlet pipe; the liquid inlet is located at the top of the elliptical head, the liquid inlet chamber is located inside the elliptical head, and the liquid inlet pipe is located at the lower part of the liquid inlet chamber, extending downwards... The liquid inlet, liquid inlet chamber, and liquid inlet pipe extend to the central cavity of the filling internal component; the gas phase feeding assembly includes an air inlet, an air inlet pipe, and an air distribution head; the air inlet is located at the top of the elliptical head, the air inlet pipe extends downward to the central cavity of the filling internal component, and the air distribution head is located at the lower end of the air inlet pipe; the air inlet, air inlet pipe, and air distribution head are connected in sequence; the heat exchange assembly includes a heat exchange medium inlet, a heat exchange cavity, a heat exchange tube bundle, and a heat exchange medium outlet; the heat exchange cavity includes a first heat exchange cavity and a second heat exchange tube bundle. The reactor comprises a heat exchange chamber and a third heat exchange chamber; the heat exchange tube bundle includes a first heat exchange tube bundle and a second heat exchange tube bundle; the first heat exchange chamber and the third heat exchange chamber are respectively disposed on the left and right sides inside the upper elliptical head of the reactor; the second heat exchange chamber is disposed below the heat exchange tube bundle inside the reactor; the heat exchange medium inlet, the first heat exchange chamber, the first heat exchange tube bundle, the second heat exchange chamber, the second heat exchange tube bundle, the third heat exchange chamber, and the heat exchange medium outlet are sequentially connected; the baffle is disposed at the lower end of the second heat exchange chamber; the filling internal components... The rotating shaft of the external motor is located below the baffle; the guide tube is axially positioned at the center of the reactor interior, and is a vertically continuous cylinder, with its lower end fixedly connected to the lower edge of the baffle, so that the interior of the guide tube is in communication with the central cavity of the filling internal component; both the liquid inlet pipe and the gas inlet pipe extend into the interior of the guide tube and extend axially along the guide tube to the central cavity of the filling internal component; the liquid phase outlet is located at the upper part of the annular cylinder; the gas phase outlet is located at the top of the elliptical head; and the material discharge port is located at the bottom of the lower end cap. Preferably, the liquid inlet pipe includes 2-18 axially arranged distribution pipes; the distribution pipes are distributed circumferentially and extend to the central cavity area of the filling internal component; the outlet of the distribution pipe is provided with a liquid distribution structure; the liquid distribution structure is one or more of the following: circumferential opening structure, radial opening structure, axial opening structure, slit structure or nozzle structure. More preferably, the number of the dispensing tubes is 4-8; More preferably, the liquid distribution structure is a radially perforated structure with 4-24 perforations; Preferably, the air distribution head is one or more of the following: a porous air distribution head, a microporous air distribution head, a slit air distribution head, or a nozzle air distribution head. Preferably, the heat exchange tube bundle extends along the reactor axis and is evenly distributed circumferentially within the reactor, located in the outer region of the guide tube; the number of heat exchange tube bundles is 2-24; the heat exchange tube bundle is provided with an enhanced heat exchange structure, which is one or more of the following: spiral structure, inner fin structure, outer fin structure, corrugated structure, or surface-reinforced structure. Preferably, the heat exchange component is connected to an external temperature control system; the heat exchange medium inside the heat exchange component is one of water, heat transfer oil, steam, and refrigerant. Preferably, the number of baffles is 2-16; the baffles are flat baffle structures; Preferably, the filling internal components include, but are not limited to, one or more combinations of structured packing, irregular packing, wire mesh packing, column packing, mesh column packing, blade structure, guide plate structure, spiral channel structure, porous media structure, and stator / rotor structure.
8. The polymerization method according to claim 6, characterized in that: In step 2), the mass concentration of 2,6-dimethylphenol is 5-20 wt%; the molar ratio of 2,6-dimethylphenol to bisphenol monomer is 4:1-20:1; the molar ratio of 2,6-dimethylphenol to copper salt is 30:1-110:1; the molar ratio of copper salt to organic amine ligand is 1:30-1:110; the volume ratio of organic solvent to water is 9:1-5:5; and the volumetric flow rate ratio of the first liquid phase feed to the second liquid phase feed is 1.5:1-20:
1. Preferably, in step 2), the set temperature is 20-70℃.
9. The polymerization method according to claim 6, characterized in that: In step 3), the polymerization reaction temperature is 20-70℃; the set rotation speed is 300-1200 rpm; and the molar ratio of oxygen to 2,6-dimethylphenol is 0.4:1-2:
1. Preferably, in step 3), the average residence time of the liquid phase material is 30-120 min.
10. The polymerization method according to claim 6, characterized in that: In step 5), a terminator is added to terminate the oxidative coupling polymerization; the terminator is one or more of hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, formic acid, and their aqueous solutions. Preferably, in step 5), a chelating agent is added to complex the residual copper catalyst in the chelation treatment process; the chelating agent is one or more of ethylenediaminetetraacetic acid and its salt, diethylenetriaminepentaacetic acid and its salt, hypozinotriacetic acid and its salt, and citric acid and its salt. Preferably, in step 5), an antisolvent is added to the precipitation and washing process to precipitate low molecular weight double-terminated hydroxyl polyphenylene ether; the antisolvent is one or more of methanol, ethanol, isopropanol and acetone; the washing process uses one or more of water, methanol and ethanol for washing. Preferably, in step 5), the devolatilization drying process is carried out by heating and drying under normal or reduced pressure to remove residual moisture and organic solvents.