A polyesteramide with a rigid micro-crosslinked network, its preparation method and application
By introducing trimesic acid into polyesteramide to construct a rigid micro-crosslinked network, the problem of modulus reduction in linear polyesteramide at high temperatures is solved, thereby improving the high-temperature performance of the material while maintaining its processing performance. This makes it suitable for electronic and electrical appliances and automotive interior structural parts.
Patent Information
- Application Number
- CN202611475531.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing linear polyesteramides have low glass transition temperatures under high-temperature conditions, their molecular chains are prone to slippage, and their modulus decreases, making it difficult to meet the requirements for high-temperature interior parts in electronic appliances and automobiles. Existing modification methods tend to sacrifice toughness and processing performance.
Tristyrene was used as a rigid micro-crosslinking node monomer to construct a rigid micro-crosslinking network with aliphatic dicarboxylic acids, aliphatic diols and cyclic lactam compounds. Local crosslinking at the molecular scale was formed through melt polycondensation, which maintained the thermoplasticity of the material and significantly improved the glass transition temperature and high temperature modulus.
It significantly improves the glass transition temperature and high temperature modulus at low addition levels, while maintaining the thermoplasticity and toughness of the material, making it suitable for the processing and application of electronic and electrical appliances and automotive interior structural parts.
Smart Images

Figure CN123107073A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature resistant engineering plastics technology, specifically including a polyesteramide with a rigid micro-crosslinked network, its preparation method and application. Background Technology
[0002] Polyesteramides combine the processing properties of polyesters with the mechanical and chemical resistance properties of polyamides, making them promising for applications in engineering plastics and synthetic fibers. However, linear polyesteramides generally have low glass transition temperatures, and under high-temperature conditions, the molecular chains are prone to segment slippage, resulting in a significant decrease in material modulus and dimensional deformation of products, making it difficult to meet the requirements for high-temperature resistant interior parts in electronics, electrical appliances, and automobiles.
[0003] Existing methods for improving the heat resistance of polyesteramides have significant shortcomings: inorganic filler modification leads to decreased material toughness and increased surface defects in products; the introduction of large amounts of aromatic diacid monomers causes a sharp increase in melt viscosity, significantly increasing the difficulty of processing and molding; common aliphatic polyol crosslinking agents require high addition amounts to achieve improved heat resistance, but high addition amounts can easily lead to excessive crosslinking, causing the material to lose its thermoplasticity and making injection molding and extrusion impossible. Therefore, developing a polyesteramide that improves both modulus and heat resistance without sacrificing melt processability has practical engineering value. Summary of the Invention
[0004] In view of the technical defects of existing linear polyesteramides, such as insufficient heat resistance, significant decrease in high-temperature modulus, and easy sacrifice of toughness and processing performance by existing modification methods, the first objective of this invention is to provide a polyesteramide with a rigid micro-crosslinked network.
[0005] A second objective of this invention is to provide a method for preparing the polyesteramide as described above.
[0006] The third objective of this invention is to provide an application of the polyesteramide described above in the preparation of electronic and electrical structural parts, high-temperature resistant automotive interior parts, and industrial fibers.
[0007] To achieve the first objective mentioned above, the technical solution adopted by the present invention includes: This invention discloses a polyester amide with a rigid micro-crosslinked network, wherein the polyester amide is constructed by melt polycondensation of pyromellitic acid as a rigid micro-crosslinked node monomer with aliphatic dicarboxylic acid, aliphatic diol and cyclic lactam compound to form a rigid micro-crosslinked network; The total effective monomer mass is calculated as the sum of the masses of aliphatic dicarboxylic acid and cyclic lactam compounds, and the amount of pyromellitic tricarboxylic acid added is 0.1 to 3.0 wt% of the total effective monomer mass.
[0008] This invention selects pyromellitic acid as a rigid micro-crosslinking node monomer. Its three carboxyl groups are located at the 1,3,5-para positions on the benzene ring, exhibiting high spatial symmetry and uniform esterification reactivity. Under extremely low pyromellitic acid addition levels (0.1-3.0 wt%), molecular-scale localized rigid micro-crosslinking nodes can be formed within the copolymer. Only microscopic localized crosslinking is formed, and the material bulk remains thermoplastic, allowing for melt injection molding and extrusion processing without macroscopic gelation. The micro-crosslinking nodes restrict the thermal movement of molecular chain segments, significantly improving the glass transition temperature, heat distortion temperature, and high-temperature modulus; simultaneously, due to the low addition level, it does not cause embrittlement resulting from overall high crosslinking.
[0009] Furthermore, the aliphatic dicarboxylic acid is selected from one or more of octanoic acid, adipic acid, sebacic acid, and dodecanoic acid.
[0010] Furthermore, the aliphatic diol is selected from one or more of ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.
[0011] Furthermore, the cyclic lactam compound is selected from autolactam and / or dodecalactam.
[0012] Furthermore, the molar ratio of the cyclic lactam compound to the aliphatic dicarboxylic acid is (7:3) to (8.5:1.5).
[0013] Furthermore, the molar ratio of the aliphatic diol to the aliphatic dicarboxylic acid is (1.3~2.0):1.
[0014] Furthermore, the initial decomposition temperature of the polyesteramide is ≥390℃, the heat distortion temperature is ≥100℃, and the elongation at break is ≥100%.
[0015] To achieve the second objective mentioned above, the technical solution adopted by the present invention includes: This invention discloses a method for preparing the polyesteramide as described above, comprising the following steps: S1. Add the cyclic lactam compound and water to the reactor and carry out a prepolymerization reaction under an inert atmosphere to obtain a polyamide prepolymer; S2. After depressurization, add aliphatic dicarboxylic acid, aliphatic diol, pyromellitic acid and catalyst, heat up to carry out esterification reaction, after the esterification reaction is completed, carry out staged vacuum polycondensation reaction, control the reaction endpoint by melt torque, and discharge to obtain the product.
[0016] Furthermore, the prepolymerization reaction conditions in step S1 are: prepolymerization temperature 180~210℃, prepolymerization pressure 0.8~1.5 MPa, and prepolymerization reaction time 0.5~2 h.
[0017] Furthermore, in step S1, the mass ratio of the cyclic lactam compound to water is (9~11):2.
[0018] Furthermore, the temperature of the esterification reaction in step S2 is 200~240℃, and the time of the esterification reaction is 2.5-4.5h.
[0019] Furthermore, the staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The polymerization temperature of the staged vacuum polycondensation reaction is 250~280℃, the vacuum degree of the pre-polymerization stage is 500~2000 Pa, the duration of the pre-polymerization stage is 1.5~3 h, the vacuum degree of the final polymerization stage is 50~300 Pa, and the final polymerization time is 1.5~4 h.
[0020] Furthermore, the catalyst is a titanium-based catalyst and / or an antimony-based catalyst, such as tetrabutyl titanate, tetraethyl titanate, antimony trioxide, etc.
[0021] Furthermore, the amount of catalyst added is 0.05 to 0.5 wt% of the sum of the mass of the aliphatic dicarboxylic acid and the cyclic lactam compound.
[0022] Furthermore, the reaction endpoint is defined as the controlled torque reaching 20-25 N·cm or higher.
[0023] In this invention, a rigid micro-crosslinked network with aromatic rings as crosslinking nodes is constructed based on the symmetrical rigid benzene ring structure of trimesic acid. This network significantly improves the glass transition temperature, high-temperature modulus, and dimensional stability of the material even with low addition amounts, while avoiding embrittlement and loss of processability caused by high crosslinking. This material is suitable for high-end applications such as electronic and electrical components, automotive interior structural parts, and high-temperature resistant fibers.
[0024] Beneficial effects of this invention: This invention provides a polyesteramide with a rigid micro-crosslinked network. By introducing a very low amount of trimesic acid, the heat resistance and modulus of the product can be significantly improved. Compared with the prior art, it has the following advantages: 1) Significant improvement in heat resistance: With extremely low addition of pyromellitic acid, the glass transition temperature of the product can be increased by 10~18℃, the heat distortion temperature by 20~35℃, and the high-temperature mechanical retention rate can be increased by more than 30%, which is significantly better than traditional aliphatic crosslinking agents.
[0025] 2) Excellent modulus and dimensional stability: The tensile modulus of the product is increased by 30%~50%, the molding shrinkage rate is reduced, and the dimensional stability at high temperature is outstanding, making it suitable for structural component application requirements.
[0026] 3) Regular and controllable cross-linking structure: The three carboxyl groups of pyromellitic acid have symmetrical and uniform reactivity, and the cross-linking points are evenly distributed, resulting in a regular cross-linking structure. This is the key to forming an effective cross-linking network at low addition levels. Furthermore, the system is gel-free and can be processed through conventional processes such as injection molding, extrusion, and spinning.
[0027] 4) High cost performance: The crosslinking agent triphenyl benzoic acid is used in small amounts, which significantly improves the effect and has a low overall cost. The process is compatible with existing high-pressure melt polycondensation equipment in the polyester amide industry, does not require special equipment, and is easy to promote industrially. Attached Figure Description
[0028] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.
[0029] Figure 1 The NMR spectrum of the polyesteramide prepared in Example 1 is shown. Detailed Implementation
[0030] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0031] Performance testing methods 1) Thermal stability: Thermogravimetric analysis was used to test the initial decomposition temperature at a nitrogen atmosphere and a heating rate of 20℃ / min. The initial decomposition temperature at which the weight loss was 5wt% was recorded.
[0032] 2) Thermal properties: Differential scanning calorimeter test, nitrogen atmosphere, heating rate 10℃ / min, and melting point recorded.
[0033] 3) Mechanical properties: Tensile strength and modulus were determined in accordance with GB / T 1040.1-2006.
[0034] 4) Heat distortion temperature: determined according to GB / T 1634.2-2019, with a load of 0.45MPa.
[0035] Example 1 1 mol of caprolactam and 12 g of deionized water were added to a high-pressure reactor and reacted at 1.2 MPa and 190 °C for 1 h under nitrogen protection to obtain a polyamide prepolymer. After depressurization, 0.3 mol of sebacic acid, 0.6 mol of 1,4-butanediol, 1.8 g of trimesic acid, and 0.40 g of tetrabutyl titanate catalyst were added, and the temperature was raised to 220 °C for esterification for 3.5 h. The temperature was further raised to 230 °C, and pre-condensation and final condensation were carried out sequentially. Pre-condensation was performed at 2000 Pa for 1.5 h, followed by final condensation at 200 Pa to a torque of 25 N·cm. The product was then discharged and pelletized. (NMR spectrum is shown below.) Figure 1 .
[0036] The prepared polyesteramide has the following properties after testing: melting point 171℃, initial decomposition temperature 390℃, tensile strength 58.8MPa, heat distortion temperature 115℃, and elongation at break 189%.
[0037] Example 2 1 mol of caprolactam and 12 g of deionized water were added to a high-pressure reactor and reacted at 1.2 MPa and 190 °C for 1 h under nitrogen protection to obtain a polyamide prepolymer. After depressurization, 0.25 mol of sebacic acid, 0.45 mol of 1,4-butanediol, 2 g of trimesic acid, and 0.35 g of tetrabutyl titanate catalyst were added, and the temperature was raised to 220 °C for esterification reaction for 3.5 h. The temperature was further raised to 230 °C, and pre-condensation and final condensation were carried out sequentially. After pre-condensation at 2000 Pa for 1.5 h and final condensation at 200 Pa to a torque of 25 N·cm, the material was discharged and pelletized to obtain the product.
[0038] The prepared polyesteramide has the following properties after testing: melting point 193℃, initial decomposition temperature 397℃, tensile strength 64.2MPa, heat distortion temperature 128℃, and elongation at break 165%.
[0039] Example 3 1 mol caprolactam and 14 g deionized water were added to a high-pressure reactor and reacted at 1.2 MPa and 190 °C for 1 h under nitrogen protection to obtain a polyamide prepolymer. The pressure was released, and 0.3 mol sebacic acid, 0.6 mol 1,3-propanediol, 1.2 g trimesic acid, and 0.4 g tetrabutyl titanate were added. The temperature was raised to 220 °C, and the esterification reaction was carried out for 3.5 h. Subsequently, the temperature was raised to 260 °C; pre-condensation and final condensation were carried out sequentially. Pre-condensation was carried out under a vacuum of 1800 Pa for 1.5 h; final condensation was carried out under a vacuum of 200 Pa. The reaction was stopped when the melt torque reached 23 N·cm, and the product was discharged and pelletized.
[0040] The prepared polyesteramide was tested and found to have the following properties: melting point 175℃; initial thermal decomposition temperature 394℃; tensile strength 62.1MPa; heat distortion temperature 112℃; and elongation at break 182%.
[0041] Example 4 1 mol caprolactam and 13 g deionized water were added to a high-pressure reactor; under nitrogen protection, the reaction was carried out at 1.2 MPa and 190 °C for 1 h to obtain a polyamide prepolymer. The pressure was released, and 0.2 mol adipic acid, 0.4 mol g 1,4-butanediol, 1.3 g trimesic acid, and 0.3 g tetrabutyl titanate were added. The temperature was raised to 220 °C, and the esterification reaction was carried out for 3.5 h. Then the temperature was raised to 230 °C; pre-condensation and final condensation were carried out sequentially. Pre-condensation was carried out under a vacuum of 1800 Pa for 1.5 h; final condensation was carried out under a vacuum of 200 Pa. The reaction was stopped when the melt torque reached 24 N·cm, and the product was discharged and pelletized.
[0042] The prepared polyesteramide has the following properties after testing: melting point 191℃; initial thermal decomposition temperature 396℃; tensile strength 61.5MPa; heat distortion temperature 114℃; elongation at break 207%.
[0043] Example 5 1 mol caprolactam and 12 g deionized water were added to a high-pressure reactor; under nitrogen protection, the reaction was carried out at 1.2 MPa and 190 °C for 1 h to obtain a polyamide prepolymer. The pressure was released, and 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 1.0 g trimesic acid, and 0.20 g tetrabutyl titanate were added. The temperature was raised to 220 °C, and the esterification reaction was carried out for 3.5 h. Then the temperature was raised to 240 °C; pre-condensation and final condensation were carried out sequentially. Pre-condensation was carried out under a vacuum of 1800 Pa for 1.5 h; final condensation was carried out under a vacuum of 200 Pa. The reaction was stopped when the melt torque reached 23 N·cm, and the product was discharged and pelletized.
[0044] The prepared polyesteramide was tested and found to have the following properties: melting point 164℃; initial thermal decomposition temperature 393℃; tensile strength 53.8MPa; heat distortion temperature 106℃; and elongation at break 215%.
[0045] Example 6 0.7 mol caprolactam, 0.3 mol dodelactam, and 13 g deionized water were added to a high-pressure reactor. Under nitrogen protection, the reaction was carried out at 1.2 MPa and 190 °C for 1 h to obtain a polyamide prepolymer. The pressure was released, and 0.25 mol sebacic acid, 0.5 mol 1,4-butanediol, 1 g trimesic acid, and 0.40 g tetrabutyl titanate were added. The temperature was raised to 220 °C, and the esterification reaction was carried out for 3.5 h. Subsequently, the temperature was raised to 235 °C; pre-condensation and final condensation were carried out sequentially. Pre-condensation was carried out under a vacuum of 2000 Pa for 1.5 h; final condensation was carried out under a vacuum of 200 Pa. The reaction was stopped when the melt torque reached 25 N·cm, and the product was discharged and pelletized.
[0046] The prepared polyesteramide has the following properties after testing: melting point 184℃; initial thermal decomposition temperature 391℃; tensile strength 60.4MPa; heat distortion temperature 109℃; and elongation at break 287%.
[0047] Comparative Example 1 1 mol of caprolactam and 12 g of deionized water were added to a high-pressure reactor and reacted at 1.2 MPa and 190 °C for 1 h under nitrogen protection to obtain a polyamide prepolymer. After depressurization, 0.3 mol of sebacic acid, 0.6 mol of 1,4-butanediol, and 0.4 g of tetrabutyl titanate catalyst were added, and the temperature was raised to 220 °C for esterification reaction for 3.5 h. The temperature was further raised to 230 °C, and pre-condensation and final condensation were carried out sequentially. After pre-condensation at 2000 Pa for 1.5 h and final condensation at 200 Pa to a torque of 25 N·cm, the material was discharged and pelletized to obtain the product.
[0048] The prepared polyesteramide has the following properties after testing: melting point 162℃, initial decomposition temperature 347℃, tensile strength 51.3MPa, heat distortion temperature 81℃, and elongation at break 218%.
[0049] Comparative Example 2 1 mol of caprolactam and 1 / 3 mol of deionized water were added to a high-pressure reactor and reacted at 1.2 MPa and 190 °C for 1 h under nitrogen protection to obtain a polyamide prepolymer. After depressurization, 0.5 mol of sebacic acid, 0.8 mol of 1,4-butanediol, 2.2 g of glycerol, and 0.40 g of tetrabutyl titanate catalyst were added, and the temperature was raised to 220 °C for esterification for 3.5 h. The temperature was further raised to 235 °C, and pre-condensation and final condensation were carried out sequentially. After pre-condensation at 2000 Pa for 1.5 h and final condensation at 200 Pa to a torque of 25 N·cm, the product was discharged and pelletized.
[0050] The prepared polyesteramide has the following properties after testing: melting point 168℃, initial decomposition temperature 392℃, tensile strength 46.5MPa, heat distortion temperature 67℃, and elongation at break 361%.
[0051] Comparative Example 3 1 mol caprolactam and 12 g deionized water were added to a high-pressure reactor; under nitrogen protection, the reaction was carried out at 1.2 MPa and 190 °C for 1 h to obtain a polyamide prepolymer. The pressure was released, and 0.3 mol sebacic acid, 0.6 mol 1,4-butanediol, 3.3 g trimesic acid, and 0.40 g tetrabutyl titanate were added. The temperature was raised to 220 °C, and the esterification reaction was carried out for 3.5 h. Then the temperature was raised to 235 °C; pre-condensation and final condensation were carried out sequentially. Pre-condensation was carried out under a vacuum of 2000 Pa for 1.5 h; final condensation was carried out under a vacuum of 200 Pa; the reaction was stopped when the melt torque reached 25 N·cm; the material was then discharged and pelletized.
[0052] The prepared polyesteramide was tested and found to have the following properties: melting point 186℃; initial thermal decomposition temperature 403℃; tensile strength 70.1MPa; heat distortion temperature 131℃; elongation at break 18%, and the material became significantly brittle.
[0053] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.
Claims
1. A polyesteramide having a rigid micro-crosslinked network, characterized in that, The polyesteramide is constructed by melt polycondensation of pyromellitic acid as a rigid micro-crosslinking node monomer with aliphatic dicarboxylic acid, aliphatic diol and cyclic lactam compound to form a rigid micro-crosslinking network. The amount of pyromellitic acid added is 0.1 to 3.0 wt% of the sum of the mass of the aliphatic dicarboxylic acid and the cyclic lactam compound.
2. The polyesteramide according to claim 1, characterized in that, The aliphatic dicarboxylic acid is selected from one or more of octanoic acid, adipic acid, sebacic acid, and dodecanoic acid; The aliphatic diol is selected from one or more of ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol; The cyclic lactam compound is selected from autolactam and / or dodecalactam.
3. The polyesteramide according to claim 1, characterized in that, The molar ratio of the cyclic lactam compound to the aliphatic dicarboxylic acid is (7:3) to (8.5:1.5); The molar ratio of the aliphatic diol to the aliphatic dicarboxylic acid is (1.3~2.0):
1.
4. The polyesteramide according to claim 1, characterized in that, The initial decomposition temperature of the polyesteramide is ≥390℃, the heat distortion temperature is ≥100℃, and the elongation at break is ≥100%.
5. A method for preparing polyesteramide as described in any one of claims 1-4, characterized in that, Includes the following steps: S1. Add the cyclic lactam compound and water to the reactor and carry out a prepolymerization reaction under an inert atmosphere to obtain the polyamide prepolymer; S2. After depressurization, add aliphatic dicarboxylic acid, aliphatic diol, pyromellitic acid and catalyst, heat up to carry out esterification reaction, after the esterification reaction is completed, carry out staged vacuum polycondensation reaction, control the reaction endpoint by melt torque, and discharge to obtain the product.
6. The preparation method according to claim 5, characterized in that, The prepolymerization reaction conditions in step S1 are: prepolymerization temperature 180~210℃, prepolymerization pressure 0.8~1.5 MPa, and prepolymerization reaction time 0.5~2 h; Preferably, the mass ratio of the cyclic lactam compound to water is (9~11):
2.
7. The preparation method according to claim 5, characterized in that, The esterification reaction in step S2 is carried out at a temperature of 200~240℃ for 2.5~4.5h. The staged vacuum polycondensation reaction includes two stages: pre-polymerization and final polymerization. The polymerization temperature of the staged vacuum polycondensation reaction is 250~280℃, the vacuum degree of the pre-polymerization stage is 500~2000 Pa, the duration of the pre-polymerization stage is 1.5~3 h, and the vacuum degree of the final polymerization stage is 50~300 Pa.
8. The preparation method according to claim 5, characterized in that, The catalyst is a titanium-based catalyst and / or an antimony-based catalyst; preferably, it is one or more of tetrabutyl titanate, tetraethyl titanate, and antimony trioxide. Preferably, the amount of catalyst added is 0.05 to 0.5 wt% of the sum of the mass of the aliphatic dicarboxylic acid and the cyclic lactam compound.
9. The preparation method according to claim 5, characterized in that, The reaction endpoint is reached when the controlled torque reaches 20~25 N·cm.
10. The application of the polyesteramide as described in any one of claims 1-4 in the preparation of electronic and electrical structural parts, high-temperature resistant automotive interior parts, and industrial fibers.