Preparation and application of a quinone-pyrazine-based MOF photocatalytic material
The selective oxidative coupling of benzylamine under visible light driven by quinone-pyrazine-based MOF photocatalysts solves the problems of low efficiency and poor environmental friendliness in traditional methods, and provides a highly efficient and stable catalyst for the synthesis of green fine chemicals and pharmaceutical intermediates.
Patent Information
- Application Number
- CN202611535889.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for the selective oxidative coupling reaction of benzylamine suffer from problems such as harsh reaction conditions, numerous byproducts, and difficulty in catalyst recovery and reuse. Traditional methods are inefficient and environmentally unfriendly.
A quinone-pyrazine-based MOF photocatalyst was prepared by a solvothermal reaction of ligand 2,7-bis(1H-pyrazol-4-yl)tribenzophenazine-10,15-dione with a nickel source in a mixed solvent, forming a catalytic material with a well-defined framework and uniformly distributed functional sites. Visible light was used to drive molecular oxygen to activate the selective oxidative dehydrogenation coupling of benzylamine.
The catalyst achieved a benzylamine oxidation reaction with high selectivity and high conversion rate at room temperature and pressure, with 100% imine selectivity. The catalyst can be recycled 5 times and still maintains a product yield of more than 90%, demonstrating excellent catalytic activity and stability.
Smart Images

Figure CN123107110A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic materials technology, specifically relating to the preparation and application of a quinone-pyrazine-based MOF photocatalytic material. Background Technology
[0002] With the continuous advancement of global industrialization, the consumption of fossil fuels has been increasing year by year. The resulting energy shortages and environmental pollution have become core issues restricting the sustainable development of human society. Developing clean and renewable alternative energy sources and green synthesis technologies is an important scientific proposition facing the fields of materials and catalysis. Solar energy, with its natural advantages such as huge reserves, wide distribution, and environmental friendliness, is recognized as one of the clean energy sources with the greatest application potential. According to statistics, the total energy radiated to the Earth by the sun every hour exceeds the total energy consumption of mankind throughout the year. How to efficiently convert low-density solar energy into storable and usable chemical energy has been a long-term research hotspot in the field of energy catalysis.
[0003] Selective oxidative coupling of benzylamine is a core reaction for constructing C=N double bonds and preparing imine-based fine chemicals, with products widely used in pharmaceuticals, pesticides, fragrances, and functional materials. Traditional preparation processes often rely on stoichiometric oxidants or homogeneous noble metal catalysts, which generally suffer from harsh reaction conditions, numerous byproducts, low atom economy, and difficulty in catalyst recovery. The photocatalytic oxidation strategy of benzylamine, driven by visible light and using molecular oxygen as a clean oxidant, can achieve highly selective dehydrogenation coupling at room temperature and pressure, offering advantages such as low energy consumption and environmental friendliness, making it an important research direction in the field of green organic catalysis.
[0004] Metal-organic frameworks (MOFs) with well-defined crystalline structures exhibit remarkable application potential in visible light-driven organic conversion due to their unique advantages of tunable pore size and precise ligand functionalization. Through covalent modification strategies of the ligand skeleton, functional groups can be introduced directionally to achieve precise control of electronic structure and band levels. Single-variable research designs based on isomorphic skeletons can eliminate interference from irrelevant factors such as topological structure, clearly establishing the structure-performance relationship and effectively solving the common problems of ambiguous active sites and inadequate elucidation of reaction mechanisms in traditional heterogeneous catalytic systems. Integrating quinone-pyrazine groups into the MOF organic ligand skeleton can, on the one hand, enhance intramolecular charge transfer effects, suppress photogenerated carrier recombination, and improve visible light utilization efficiency; on the other hand, it can activate molecular oxygen through quinone structural active sites, efficiently mediating the selective oxidative dehydrogenation of benzylamine, generating imine products with high selectivity, while also possessing excellent catalytic cycle stability. This quinone-pyrazine MOF catalytic system provides a novel approach for constructing a highly efficient visible light-driven amine oxidation conversion platform and has broad application prospects in the field of green and fine organic synthesis. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a preparation and application of a quinone-pyrazine-based MOF photocatalytic material with high catalytic reaction efficiency.
[0006] The first objective of this invention is to provide a quinone-pyrazine-based MOF photocatalytic material, which is prepared by a solvothermal reaction of ligand 2,7-bis(1H-pyrazol-4-yl)tribenzophenazine-10,15-dione (H2DPNq) with a nickel source in a mixed solvent; wherein the mixed solvent is a mixed solution of N,N-dimethylformamide and water.
[0007] The aforementioned quinone-pyrazine-based MOF photocatalyst is a deep purple powder. Specifically, the nickel source is nickel acetate tetrahydrate (Ni(OAc)₂·4H₂O); the volume ratio of N,N-dimethylformamide to water in the mixed solvent is 1~8:1, preferably 3~5:1. The reaction can be carried out in two ways: either the ligand H₂DPNq and the nickel source can be directly dissolved in the mixed solvent before reaction, or they can be dissolved separately in N,N-dimethylformamide and water, and then mixed for a solvothermal reaction. In both methods, the preferred mass ratio of nickel source to water in the mixed solvent is 7.00~10.00 mg:1.0 mL, and the preferred mass ratio of ligand H₂DPNq to N,N-dimethylformamide in the mixed solvent is 1.00~3.00 mg:1.00 mL; the ligand H₂DPNq and nickel source are added in a stoichiometric ratio, and in one specific embodiment, the molar ratio is 3:4. The solvothermal reaction temperature is not lower than 100 ℃, preferably 120~140 ℃; when the reaction temperature is controlled at 120~140 ℃, the reaction time is preferably 12~72h.
[0008] The second objective of this invention is to provide a method for preparing the above-mentioned quinone-pyrazine-based MOF photocatalytic material, specifically comprising: dissolving the ligand H2DPNq and the nickel source in N,N-dimethylformamide and water, respectively; mixing the two solutions evenly and then carrying out a solvothermal reaction to obtain the target material.
[0009] The selection of nickel source, solvent ratio, feed ratio, solvothermal reaction parameters, etc. involved in this preparation method are all consistent with the limitations in the aforementioned quinone-pyrazine-based MOF photocatalytic material system.
[0010] A third objective of this invention is to provide the application of the above-mentioned quinone-pyrazine-based MOF photocatalytic material in the photocatalytic self-coupling reaction of benzylamine to prepare imine compounds.
[0011] Compared with existing technologies, this invention constructs a quinone-pyrazine MOF photocatalytic material with a well-defined framework and uniformly distributed functional sites through the coordination assembly of Ni8 metal clusters and 2,7-bis(pyrazol-4-yl)tribenzo[a,c,i]phenazine-10,15-dione ligands. The applicant's experimental results show that this material has excellent light-harvesting ability in the visible light region, along with a matched band structure and high charge separation efficiency, effectively driving the coupling process of molecular oxygen activation and selective oxidative dehydrogenation of benzylamine. When applied to the photocatalytic oxidation of benzylamine to imine, the benzylamine conversion rate reaches 99.90%, and the target imine product selectivity is 100%, exhibiting excellent catalytic activity and product selectivity; moreover, it is recyclable, with a product yield still exceeding 90.00% after 5 cycles.
[0012] This provides a highly efficient and stable non-precious metal heterogeneous catalytic material for visible light-driven green selective oxidation of amines, with broad application prospects in green fine chemicals, pharmaceutical intermediate synthesis, and clean energy conversion. Attached Figure Description
[0013] Figure 1 The ligand H2DPNq prepared in Example 1 1 H NMR spectrum.
[0014] Figure 2 For the ligand H2DPN prepared in Comparative Example 1 1 H NMR spectrum.
[0015] Figure 3 For the ligand H2DPB prepared in Comparative Example 2 1 H NMR spectrum.
[0016] Figure 4 The infrared spectra of the ligands and MOF photocatalysts GXMZU137, GXMZU136 and GXMZU135 prepared in Examples 1, 1 and 2 respectively are shown. (a) is the infrared spectrum of ligand H2DPNq and MOF photocatalyst GXMZU137 prepared in Example 1, (b) is the infrared spectrum of ligand H2DPN and MOF photocatalyst GXMZU136 prepared in Comparative Example 1, and (c) is the infrared spectrum of ligand H2DPB and MOF photocatalyst GXMZU135 prepared in Comparative Example 1.
[0017] Figure 5 The PXRD patterns are of GXMZU137, GXMZU136 and GXMZU135 prepared in Example 1, Comparative Examples 1 and 2, respectively.
[0018] Figure 6The solid-state UV-Vis diffuse reflectance spectra of GXMZU137, GXMZU136, and GXMZU135 prepared in Example 1, Comparative Examples 1 and 2, respectively.
[0019] Figure 7 The fluorescence spectra of GXMZU137, GXMZU136 and GXMZU135 prepared in Example 1, Comparative Examples 1 and 2 are shown.
[0020] Figure 8 The images shown are SEM and EDS images of GXMZU137 obtained in Example 1.
[0021] Figure 9 The graph shows the yield and selectivity results of five cycles of the photocatalytic benzylamine self-coupling reaction using GXMZU137 in Example 1. Detailed Implementation
[0022] To better explain the technical solution of the present invention, the present invention will be further described in detail below with reference to embodiments, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical features used in the embodiments can be replaced with other technical features known in the art that have equivalent or similar functions or effects without departing from the inventive concept.
[0023] Example 1: Preparation of GXMZU137 photocatalytic material
[0024] (1) Preparation of functional ligand intermediates:
[0025]
[0026] Weigh 1.00 g of 2,7-dibromo-9,10-phenanthrenequinone and 3.0072 g of 1-tetrahydropyrano-4-pyrazoloborate pinacol ester, and add them to a round-bottom flask containing 45.00 mL of 1,4-dioxane and 12.00 mL of deionized water. Then add 1.5104 g of anhydrous potassium carbonate and 0.3157 g of tetra(triphenylphosphine)palladium. After thorough mixing, nitrogen gas is continuously purged to purge air from the system. Under nitrogen protection, the temperature is raised to 110 °C and the reaction is carried out with stirring for 48 h. After the reaction is complete, the reaction solution is allowed to cool naturally to room temperature. 50.00 mL of saturated sodium chloride aqueous solution is added to promote the full precipitation of the product. After the reaction is complete, the reaction mixture is cooled to room temperature and extracted three times with CH2Cl2. The combined organic layers are dried over anhydrous Na2SO4. After solvent evaporation, the crude product was purified by silica gel column chromatography. The eluent was a 1:1 volume ratio of petroleum ether to ethyl acetate mixture. After collecting the target component, it was dried by rotary evaporation, and a purple-red solid was collected to obtain the tetrahydropyran-protected intermediate.
[0027] (2) Preparation of functional ligands:
[0028]
[0029] Weigh 0.30 g of the above intermediate product and 0.145 g of 2,3-diaminonaphthalene-1,4-dione into a round-bottom flask containing 30.00 mL of anhydrous ethanol and 10.00 mL of acetic acid. After stirring thoroughly at room temperature, heat to 90 °C and stir for 24 h. After the reaction is complete, allow the reaction solution to cool naturally to room temperature, collect the brown product by vacuum filtration under reduced pressure, and wash with anhydrous ethanol and methanol to obtain the target product protected by tetrahydropyran. The reaction yield is 95%.
[0030] The target product protected by tetrahydropyran was deprotected as follows: The intermediate product was dispersed in 50.00 mL of anhydrous ethanol, and 25.00 mL of 1.00 mol / L hydrochloric acid solution was added. After stirring, the mixture was heated to 80 °C and stirred at a constant temperature for 8 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the precipitate was collected by filtration. After washing with ethanol, the precipitate was transferred to a beaker containing 100.00 mL of distilled water for dispersion. The pH of the system was adjusted to 5.0-7.0 using 0.50 mol / L sodium bicarbonate aqueous solution (precisely adjusted to pH=7.0 in this example). After filtration again, the filter cake was repeatedly washed with deionized water until the filtrate was neutral. Then, it was washed successively with a small amount of anhydrous ethanol and anhydrous diethyl ether. After drying, the brown target ligand was obtained and named H2DPNq. The reaction yield was 80%.
[0031] (3) Preparation of GXMZU137 photocatalytic material: 48.00 mg of ligand H2DPNq was accurately weighed and dissolved in 16.00 mL of N,N-dimethylformamide by ultrasonication; 31.80 mg of nickel acetate tetrahydrate was weighed and completely dissolved in 4.00 mL of deionized water. The two solutions were mixed and stirred evenly, transferred to a stainless steel reactor lined with polytetrafluoroethylene and sealed. The mixture was heated to 120 °C for a solvothermal reaction, which lasted for about 72 h until the system was completely reacted. After the reaction was completed, the mixture was naturally cooled to room temperature, and a solid product precipitated in the system. The product was collected and washed repeatedly with N,N-dimethylformamide, anhydrous ethanol, and anhydrous diethyl ether to remove unreacted raw materials and residual solvent. The product was then dried thoroughly under vacuum to obtain a dark purple powdery quinone-pyrazine MOF photocatalytic material, named GXMZU137 (GXMZU is the abbreviation for Guangxi University for Nationalities), with a product yield of 70%.
[0032] Comparative Example 1: Preparation of GXMZU136 photocatalytic material
[0033] (1) Preparation of functional ligands:
[0034]
[0035] Weigh 0.3 g of the intermediate product from Example 1 above and 0.122 g of 2,3-diaminonaphthalene, and add them to a round-bottom flask containing 30.00 mL of anhydrous ethanol and 10.00 mL of acetic acid. After stirring thoroughly at room temperature, heat to 90 °C and stir for 24 h. After the reaction is complete, allow the reaction solution to cool naturally to room temperature, collect the bright orange product by vacuum filtration under reduced pressure, and wash with anhydrous ethanol and methanol to obtain the target product protected by tetrahydropyran. The reaction yield is 94%.
[0036] The target product protected by tetrahydropyran was deprotected as follows: The intermediate product was dispersed in 50.00 mL of anhydrous ethanol, and 25.00 mL of 1.00 mol / L hydrochloric acid solution was added. After stirring, the mixture was heated to 80 °C and stirred at a constant temperature for 8 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the precipitate was collected by filtration. After washing with ethanol, the precipitate was transferred to a beaker containing 100.00 mL of distilled water for dispersion. The pH of the system was adjusted to 5.0-7.0 using 0.50 mol / L sodium bicarbonate aqueous solution (precisely adjusted to pH=7.0 in this example). After filtration again, the filter cake was repeatedly washed with deionized water until the filtrate was neutral. Then, it was washed successively with a small amount of anhydrous ethanol and anhydrous diethyl ether. After drying, the orange target ligand was obtained and named H2DPN. The reaction yield was 80%.
[0037] (2) Preparation of GXMZU136 photocatalytic material: 45.00 mg of ligand H2DPN was dissolved in 16.00 mL of N,N-dimethylformamide, and 31.80 mg of Ni(OAc)2·4H2O was dissolved in 4.00 mL of water. The two solutions were then mixed and subjected to a solvothermal reaction at 120 °C in a reaction vessel until complete (about 72 h). After the reaction was completed, the mixture was cooled to room temperature. After the reaction was completed, the mixture was cooled to room temperature, and a solid precipitated. The solid was collected, washed with solvents N,N-dimethylformamide, ethanol and diethyl ether, and dried under vacuum to obtain nickel-based MOF photocatalytic material (reddish-brown powder, denoted as GXMZU136, GXMZU = Guangxi University for Nationalities), with a yield of 70%.
[0038] Comparative Example 2: Preparation of GXMZU135 photocatalytic material
[0039] (1) Preparation of functional ligands:
[0040]
[0041] Weigh 0.30 g of the intermediate obtained in Example 1 and 0.122 g of o-phenylenediamine, and add them to a round-bottom flask containing 30.00 mL of anhydrous ethanol and 10.00 mL of acetic acid. After stirring evenly at room temperature, the mixture is heated to 90 °C and stirred for 24 h. After the reaction is complete, allow it to cool naturally to room temperature, collect the bright orange solid by vacuum filtration, and wash it successively with anhydrous ethanol and methanol to obtain a tetrahydropyran-protected ligand intermediate with a reaction yield of 90%.
[0042] The tetrahydropyran-protected intermediate was deprotected as follows: the intermediate was dispersed in 50.00 mL of anhydrous ethanol, and 25.00 mL of 1.0 mol / L hydrochloric acid solution was added. After stirring, the mixture was heated to 80 °C and stirred at a constant temperature for 8 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the precipitate was collected by filtration. After washing with ethanol, the solid was transferred to a beaker containing 100.00 mL of distilled water and dispersed thoroughly. The pH of the system was adjusted to 5.0-7.0 with 0.50 mol / L sodium bicarbonate aqueous solution (in this example, the pH was precisely adjusted to 7.0). After filtration again, the filter cake was repeatedly washed with deionized water until the filtrate was neutral. Then, it was washed successively with a small amount of anhydrous ethanol and anhydrous diethyl ether. After vacuum drying, the yellow target ligand was obtained and named H2DPB, with a reaction yield of 80%.
[0043] (2) Weigh 40.00 mg of ligand H2DPB and dissolve it in 16.00 mL of N,N-dimethylformamide. Separately, dissolve 31.80 mg of nickel acetate tetrahydrate (Ni(OAc)2·4H2O) in 4.00 mL of deionized water. Mix the two solutions thoroughly and transfer them to a reaction vessel. Heat the mixture to 120 °C and carry out a solvothermal reaction for 72 h. After the reaction is completed, allow it to cool naturally to room temperature. A solid product precipitates. Collect the solid and wash it sequentially with N,N-dimethylformamide, anhydrous ethanol, and anhydrous diethyl ether. After vacuum drying, a yellow-brown powdered nickel-based MOF photocatalyst material is obtained, denoted as GXMZU135 (GXMZU is the abbreviation for Guangxi University for Nationalities), with a yield of 70%.
[0044] The ligands and MOF photocatalytic materials prepared in Example 1, Comparative Examples 1 and 2 were characterized and analyzed, and the results are as follows:
[0045] 1. Proton NMR spectrum
[0046] The ligands prepared in Example 1 and Comparative Examples 1-2 were characterized by NMR, respectively:
[0047] The 1H NMR spectrum of the ligand prepared in Example 1 is shown below. Figure 1 As shown. By Figure 1 It can be determined that the ligand H2DPAq obtained in Example 1 is 2,7-bis(1H-pyrazol-4-yl)tribenzo[a,c,i]phenazine-10,15-dione.
[0048] The 1H NMR spectrum of the ligand prepared in Comparative Example 1 is shown below. Figure 2 As shown. By Figure 2 It can be determined that the ligand H2DPN prepared in Comparative Example 1 is 2,7-bis(1H-pyrazol-4-yl)tribenzo[a,c,i]phenazine.
[0049] The 1H NMR spectrum of the ligand prepared in Comparative Example 2 is shown below. Figure 3 As shown. By Figure 3 It can be determined that the ligand H2DPB prepared in Comparative Example 2 is 2,7-bis(1H-pyrazol-4-yl)dibenzo[a,c]phenazine.
[0050] 2. Infrared spectroscopy analysis
[0051] The ligands and photocatalysts GXMZU137, GXMZU136, and GXMZU135 prepared in Example 1 and Comparative Examples 1-2 were characterized and analyzed using infrared spectroscopy. The characterization results are as follows: Figure 4 As shown. By Figure 4 (a) It can be seen that GXMZU137 is located at 1670~1678 cm. -1 The presence of characteristic stretching vibration peaks attributable to the C=O double bond of the quinone-pyrazinyl ligand within the range indicates that the quinone-pyrazinyl group is stably retained during MOF synthesis. Compared to the corresponding ligands, the three Ni8-MOF materials exhibit characteristic stretching vibration peaks at 3000–3300 cm⁻¹. -1 The characteristic peaks of the pyrazole NH stretching vibration at the site were all weakened, which preliminarily proved that the pyrazole site was coordinated with the metal cluster, and the MOF photocatalytic material was successfully synthesized.
[0052] 3. PXRD Analysis
[0053] X-ray powder diffraction was used to characterize the crystal phase and structure of GXMZU137, GXMZU136, and GXMZU135 prepared in Example 1 and Comparative Examples 1-2. The results are as follows: Figure 5 As shown in the figure. The test results show that the measured PXRD diffraction peaks of GXMZU137 completely match the simulated diffraction peaks, indicating that the material phase is pure and the synthesis was successful. The PXRD diffraction peak positions of GXMZU136 and GXMZU135 are completely consistent with those of GXMZU137, indicating that the three have the same crystal coordination structure and are isomorphic Ni8-MOF materials. The diffraction peaks of the three materials are sharp, all of which have high crystallinity and good structural integrity.
[0054] 4. Ultraviolet-Visible Diffuse Reflectance Analysis
[0055] Solid-state UV-Vis diffuse reflectance spectroscopy was performed on GXMZU137, GXMZU136, and GXMZU135 prepared in Example 1 and Comparative Examples 1-2. The results are as follows: Figure 6 As shown. By Figure 6 It is known that the optical absorption edge of GXMZU137 exceeds 700 nm, indicating that the material has a wide range of visible light trapping capabilities; the synergistic effect of the conjugated framework and quinone-pyrazine units endows the material with strong electron acceptance and transport capabilities.
[0056] 5. Fluorescence spectroscopy analysis
[0057] The fluorescence emission spectra of GXMZU137, GXMZU136, and GXMZU135 prepared in Example 1 and Comparative Examples 1-2 were characterized using a fluorescence spectrophotometer. The results are as follows: Figure 7 As shown. By Figure 7 It can be seen that the fluorescence emission intensity of GXMZU137 is significantly lower than that of GXMZU135 and GXMZU136, indicating that the recombination rate of photogenerated electron-hole pairs in GXMZU137 is the lowest, which is more conducive to photocatalytic aerobic oxidation.
[0058] 6. SEM and EDS analysis
[0059] The GXMZU137 prepared in Example 1 was characterized by scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS). The characterization results are as follows: Figure 8 As shown. By Figure 8 It is known that the quinone-pyrazine-based MOF photocatalytic material crystal of the present invention is an octahedral crystal, with C, O, Ni and N uniformly distributed in the sample.
[0060] Application Example 1
[0061] 5.00 mg of the GXMZU137 photocatalyst material prepared in Example 1 and 10.92 μL (0.1 mmol) of benzylamine (C7H9N) were placed in a quartz reaction tube. 4.00 mL of acetonitrile was added as the reaction solvent. After sealing the quartz tube, oxygen was bubbled into the system for 20 min to fully replace the air inside the tube. A 50 W, 400-800 nm LED lamp was used as the visible light source, and the reaction was irradiated at room temperature for 3 h. After the reaction, the catalyst was recovered by centrifugation, and the reaction supernatant was collected. The product yield was quantitatively determined by gas chromatography (GC), and the product structure was qualitatively confirmed by nuclear magnetic resonance spectroscopy (NMR). The main product was N-benzyl-1-phenylmethylimine (C7H9N). 14 H 13 N). Calculations showed that the yield of N-benzyl-1-phenylmethylimine was 99.90%, and the product selectivity was 100%. Figure 8 As shown.
[0062] Material Application Analysis: After the complete photocatalytic reaction of GXMZU137 in Application Example 1, the catalyst GXMZU137 was centrifuged, washed with solvent, and dried before being added back into a fresh benzylamine reaction system. The catalytic experiment was repeated under identical reaction conditions, for a total of four cycles. The product yields for the five reactions were 99.90%, 98%, 96%, 95%, and 92%, respectively, with a product selectivity of 100% throughout the entire process. The test results are as follows: Figure 9 As shown in the figure, after five cycles, the activity of GXMZU137 in catalyzing the self-coupling of benzylamine showed no significant decline, and the catalytic performance remained stable. This cyclic experiment demonstrates that the quinone-pyrazine-based MOF photocatalytic material described in this invention possesses excellent structural stability and reusability, and the catalyst can be recycled, exhibiting good practical application value and economic benefits.
[0063] Application Comparative Example 1
[0064] The only difference between this example and Application Example 1 is that GXMZU136 prepared in Comparative Example 1 is used instead of GXMZU137 as the catalyst.
[0065] The results showed that the product N-benzyl-1-phenylmethyleneimine (C) was obtained. 14 H 13 N). Calculations showed that the yield of N-benzyl-1-phenylmethylimine was 28%, with a selectivity of 100%.
[0066] Application Comparative Example 2
[0067] The only difference between this example and Application Example 1 is that GXMZU135 prepared in step (1) of Example 1 is used instead of GXMZU137 as the catalyst.
[0068] The results showed that the product N-benzyl-1-phenylmethyleneimine (C) was obtained. 14 H 13 N). Calculations showed that the yield of N-benzyl-1-phenylmethylimine was 11%, with a selectivity of 100%.
[0069] Application Example 2
[0070] The only difference between this example and Application Example 1 is that 4-fluorobenzylamine (C7H8FN) is used instead of benzylamine (C7H9N).
[0071] The results showed that the product N-(4-fluorobenzyl)-1-(4-fluorophenyl)methylimine (C) was obtained. 14 H 11 F2N). Calculations showed that the yield of N-(4-fluorobenzyl)-1-(4-fluorophenyl)methylimine was 70%, with a selectivity of 100%.
[0072] Application Example 3
[0073] The only difference between this example and Application Example 1 is that 4-bromobenzylamine (C7H8BrN) is used instead of benzylamine (C7H9N).
[0074] The results showed that the product N-(4-bromobenzyl)-1-(4-bromophenyl)methylimine (C) was obtained. 14 H 11 (Br2N). Calculations showed that the yield of N-(4-bromobenzyl)-1-(4-bromophenyl)methylimine was 99%, with a selectivity of 100%.
[0075] Application Example 4
[0076] The only difference between this example and Application Example 1 is that 4-trifluoromethylbenzylamine (C8H8FN) is used instead of benzylamine (C7H9N).
[0077] The results showed that the product N-(4-trifluoromethylbenzyl)-1-(4-trifluoromethylphenyl)methylimine (C) was obtained. 16 H 11 F6N). Calculations showed that the yield of N-(4-trifluoromethylbenzyl)-1-(4-trifluoromethylphenyl)methylimine was 56%, with a selectivity of 100%.
[0078] Application Example 5
[0079] The only difference between this example and Application Example 1 is that 4-methylbenzylamine (C8H) is used. 11 N) replaces benzylamine (C7H9N).
[0080] The results showed that the product N-(4-methylbenzyl)-1-(4-methylphenyl)methylimine (C) was obtained. 16 H 17 N). Calculations showed that the yield of N-(4-methylbenzyl)-1-(4-methylphenyl)methylimine was 67%, with a selectivity of 100%.
[0081] Application Example 6
[0082] The only difference between this example and Application Example 1 is that 4-methoxybenzylamine (C8H) is used. 11 ON) replaces benzylamine (C7H9N).
[0083] The results showed that the product N-(4-methoxybenzyl)-1-(4-methoxyphenyl)methylimine (C) was obtained. 16 H 17 O2N). Calculations showed that the yield of N-(4-methoxybenzyl)-1-(4-methoxyphenyl)methylimine was 99%, with a selectivity of 100%.
[0084] Application Example 7
[0085] The only difference between this example and Application Example 1 is that 3-methoxybenzylamine (C8H) is used. 11 ON) replaces benzylamine (C7H9N).
[0086] The results showed that the product N-(3-methoxybenzyl)-1-(3-methoxyphenyl)methylimine (C) was obtained. 16 H 17 O2N). Calculations showed that the yield of N-(3-methoxybenzyl)-1-(3-methoxyphenyl)methylimine was 90%, with a selectivity of 100%.
Claims
1. A quinone-pyrazinyl MOF photocatalytic material, characterized in that, The material is prepared by a solvothermal reaction of ligand H2DPNq with a nickel source in a mixed solvent; the ligand H2DPNq is 2,7-bis(1H-pyrazol-4-yl)tribenzo[a,c,i]phenazine-10,15-dione, and the mixed solvent is a mixed solution of N,N-dimethylformamide and water.
2. The quinone-pyrazinyl MOF photocatalytic material of claim 1, wherein The nickel source is nickel acetate tetrahydrate (Ni(OAc)2·4H2O).
3. A method of preparing the quinone-pyrazinyl MOF photocatalytic material of claim 1, comprising: The ligand H2DPNq and the nickel source were dissolved in N,N-dimethylformamide and deionized water, respectively. The two solutions were combined and mixed, and then subjected to a solvothermal reaction to obtain the target material.
4. The production method according to claim 3, characterized by, The nickel source is nickel acetate tetrahydrate (Ni(OAc)2·4H2O).
5. The preparation method according to claim 3, characterized in that, The reaction temperature of the solvothermal reaction is not lower than 100 ℃.
6. The application of the quinone-pyrazine-based MOF photocatalyst material according to claim 1 in the photocatalytic self-coupling reaction of benzylamine to prepare imine compounds.