Fibers for 3D printing and their preparation methods, 3D printed products

By optimizing composite materials and processes, 3D printing filaments with island structures were prepared, solving the problem of poor gloss effect in existing 3D printed products and achieving a soft, silk-like luster and low roughness.

CN123107323APending Publication Date: 2026-11-17JF POLYMERS (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611624374.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing 3D printed products lack the soft diffuse reflection and sense of layering unique to silk. Their high surface roughness makes them appear dull and unable to simulate the luster of real silk.

Method used

The wire is prepared by combining two polymer materials with independent glass transition temperatures and refractive index differences to form an island structure. By combining masterbatch pre-dispersion and secondary dilution extrusion processes, the particle size and distribution of the dispersed phase are controlled to achieve multiple interfacial reflections and refractions of light.

Benefits of technology

It achieves a soft, silk-like luster in 3D printed products, reduces surface roughness, enhances specular reflection capabilities, and creates a uniform and stable light scattering effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107323A_ABST
    Figure CN123107323A_ABST
Patent Text Reader

Abstract

This application discloses filaments for 3D printing, their preparation methods, and 3D printed articles. The filaments for 3D printing include a continuous matrix phase and a dispersed phase distributed within the matrix phase. The matrix phase includes a first polymer material, and the dispersed phase includes a second polymer material. The filaments have independent first and second glass transition temperatures. The refractive index of the first polymer material is n1, and the refractive index of the second polymer material is n2, where |n1-n2|≥0.05. The average equivalent diameter of the dispersed phase particles is not less than 90nm. This significantly enhances the scattering intensity of the filaments, allowing light to undergo multiple interfacial reflections and refractions upon entering the filament, resulting in a soft, silky luster.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of 3D printing, specifically to filaments for 3D printing and methods for their preparation, and 3D printed articles. Background Technology

[0002] With the popularization of 3D printing technology, users' aesthetic requirements for the appearance of printed products are increasing. In addition to basic mechanical properties, special visual effects, such as the silk-like luster of 3D printed products, have become a hot topic in market research. However, 3D printed products provided by existing technologies only have surface luster and lack the soft diffuse reflection and sense of layering unique to silk; or although there is scattering, the surface roughness is high, resulting in an overall dull appearance that does not resemble real silk.

[0003] It should be noted that the above statements are only used to provide background information related to this application and do not necessarily constitute prior art. Summary of the Invention

[0004] In a first aspect of this application, a filament for 3D printing is provided, characterized in that it comprises a continuous matrix phase and a dispersed phase distributed in the matrix phase, the matrix phase comprising a first polymeric material, the dispersed phase comprising a second polymeric material, the filament having an independent first glass transition temperature and a second glass transition temperature; the refractive index of the first polymeric material is n1, the refractive index of the second polymeric material is n2, and |n1-n2|≥0.05; the average equivalent diameter of the dispersed phase particles is not less than 90 nm.

[0005] Therefore, the dispersed phase and the matrix phase in the wire of this application have their own independent glass transition temperatures, indicating that the dispersed phase and the matrix phase are thermodynamically incompatible, providing a physical interface for light scattering; further, by controlling the absolute value of the refractive index difference between the first polymer material forming the matrix phase and the second polymer material forming the dispersed phase to be greater than or equal to 0.05, the scattering intensity is significantly improved; in addition, by further controlling the average equivalent diameter of the dispersed phase particles to be not less than 90 nm, effective Mie diffuse scattering can be generated, and light entering the wire interior undergoes multiple interface reflections and refractions, thereby producing a soft, silk-like luster.

[0006] In some embodiments, the difference between the first glass transition temperature and the glass transition temperature of the first polymer material is no greater than 3°C; the difference between the second glass transition temperature and the glass transition temperature of the second polymer material is no greater than 3°C.

[0007] In some embodiments, under the conditions of non-crystalline state and test sample thickness of 2 mm: the light transmittance of the first polymer material is not less than 85%; the light transmittance of the second polymer material is not less than 85%.

[0008] In some embodiments, the first polymeric material includes one or more of polyethylene terephthalate and polylactic acid; the second polymeric material includes one or more of polymethyl methacrylate, styrene-ethylene-butene-styrene copolymer, polybutylene adipate terephthalate, polyethylene terephthalate, and polylactic acid.

[0009] In some embodiments, the average equivalent diameter of the dispersed phase particles is not less than 150 nm.

[0010] In some embodiments, the mass fraction of the dispersed phase is 5%-25% based on the total mass of the wire.

[0011] In some embodiments, the roughness Ra of the wire is ≤0.4μm.

[0012] In a second aspect of this application, a method for preparing the aforementioned wire is proposed, comprising: mixing a first polymer material and a second polymer material to obtain a first mixture; performing melt blending extrusion granulation on the first mixture to obtain a masterbatch; mixing the masterbatch and the first polymer material to obtain a second mixture; and extruding the second mixture through an extruder to form a wire; wherein the die flow channel length of the extruder is ≥150mm.

[0013] Therefore, this application selects raw materials for wire preparation to ensure that the dispersed phase and matrix phase have their own independent glass transition temperatures, and that the absolute value of the refractive index difference between the first polymer material forming the matrix phase and the second polymer material forming the dispersed phase is greater than or equal to 0.05. This allows the dispersed phase and matrix phase to form an island structure, providing a physical interface for light scattering. Furthermore, the phase interface of the island structure can act as a scattering center, causing multiple interfacial reflections and refractions as light enters the wire, resulting in a soft, silky luster. The application further employs a masterbatch pre-dispersion and secondary dilution extrusion method to prepare the wire, which reduces the agglomeration of dispersed phase particles and improves the uniformity of the dispersed phase distribution in the matrix phase. Uniformity helps to form a uniform and stable two-phase interface. At the same time, using an extruder with a longer die flow channel to extrude wire allows for a longer residence time of the melt in the die, enabling the viscoelastic strain of the polymer melt to relax more fully before exiting the die. This results in reduced and more stable exit expansion, smoothing out upstream inlet disturbances and velocity distortion. Consequently, it reduces ripples, microcracks, and die buildup on the wire surface, lowers the surface roughness of the wire, and enhances its specular reflectivity. Furthermore, as the die cavity volume and residence time increase, the collision and coalescence of dispersed phase droplets driven by interfacial tension helps to increase the average equivalent diameter of the dispersed phase, thereby further enhancing the silk-like luster of the wire.

[0014] In some embodiments, the die temperature of the extruder die head is 220°C-270°C, and optionally 230°C-250°C.

[0015] In some embodiments, the mass fraction of the second polymeric material is 20%-50% based on the mass of the first mixture; or the mass fraction of the second polymeric material is 5%-25% based on the mass of the second mixture.

[0016] In a third aspect, this application proposes a 3D printed article obtained by printing using the aforementioned filament or filament prepared by the aforementioned method. Thus, the 3D printed article possesses all the features and advantages of the aforementioned filament for 3D printing or its preparation method, which will not be repeated here. Attached Figure Description

[0017] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 The results of DSC tests on the wire, polyethylene terephthalate (PETG), and polymethyl methacrylate (PMMA) of Example 1 of this application are shown. Figure 2 SEM images of the cross-sections of the wires prepared in Examples 6, 7, 8, Comparative Example 1, and Comparative Example 4 of this application, perpendicular to the extrusion direction, at a magnification of 20K. Figure 3 These are photographs of the wires prepared in Example 6, Comparative Example 1, and Comparative Example 4 of this application; Figure 4 These are photographs of the 3D printed products prepared in Example 6, Comparative Example 1, and Comparative Example 4 of this application. Detailed Implementation

[0018] The embodiments of this application are described in detail below, with examples of these embodiments shown in the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0019] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used in this application is for the purpose of describing particular embodiments only and is not intended to limit this application; unless otherwise stated, the values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this application).

[0020] The terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are open-ended expressions, meaning they include what is specified in this application but do not exclude other aspects.

[0021] In the description of this application, all figures disclosed herein are approximate values, whether or not the words "approximately" or "about" are used. Each figure may vary by less than 10% or by a difference that is considered reasonable by one of the art, such as 1%, 2%, 3%, 4%, or 5%.

[0022] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0023] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. "First feature" and "second feature" may include one or more of the indicated feature.

[0024] In the description of this application, "multiple" means two or more.

[0025] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0026] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0027] To achieve the unique visual effect of silk luster in 3D printed products, related technologies use blending modification to add pearl powder or another polymer material to polylactic acid (PLA) or other matrices to simulate this silk luster effect. However, the final 3D printed products only have surface luster and lack the soft diffuse reflection and sense of layering that silk has. Or, although there is scattering, the surface roughness is high, causing the overall appearance to be dull and not like real silk.

[0028] This application selects the raw materials for the filament used in 3D printing. The filament is composed of two or more polymer materials, and the composite material has two independent glass transition temperatures, corresponding to the glass transition temperatures of the matrix phase and the dispersed phase, respectively. This means the matrix and dispersed phases are thermodynamically incompatible, resulting in a clear two-phase interface (island structure) that provides a physical interface for light scattering. Furthermore, by controlling the absolute value of the difference in refractive index between the matrix and dispersed phases to be greater than or equal to 0.05, the scattering intensity is significantly improved. The average equivalent diameter of the dispersed phase particles is further controlled to be no less than 90 nm, enabling effective Mie diffuse scattering. The island structure's phase interface acts as the scattering center, causing multiple interface reflections and refractions as light enters the filament, resulting in a soft, silky luster.

[0029] In a first aspect of this application, a filament for 3D printing is provided, characterized in that it comprises a continuous matrix phase and a dispersed phase distributed in the matrix phase, the matrix phase comprising a first polymeric material, the dispersed phase comprising a second polymeric material, the filament having an independent first glass transition temperature and a second glass transition temperature; the refractive index of the first polymeric material is n1, the refractive index of the second polymeric material is n2, and |n1-n2|≥0.05; the average equivalent diameter of the dispersed phase particles is not less than 90 nm. Therefore, the dispersed phase and matrix phase in the wire of this application each have their own independent glass transition temperature, indicating that the dispersed phase and matrix phase are thermodynamically incompatible, providing a physical interface for light scattering. By further controlling the absolute value of the refractive index difference between the first polymer material forming the matrix phase and the second polymer material forming the dispersed phase to be greater than or equal to 0.05, the scattering intensity is significantly improved. Furthermore, by further controlling the average equivalent diameter of the dispersed phase particles to be no less than 90 nm, effective Mie diffuse scattering can be generated. Light entering the wire's interior undergoes multiple interface reflections and refractions at the two-phase interface, thus producing a soft, silk-like luster. In summary, this application, through the selection of dispersed phase materials and matrix phase materials combined with the control of dispersed phase size, achieves a synergistic effect, resulting in a wire with a soft, silk-like luster.

[0030] The visible light wavelength range is approximately 400-700 nm. When the dispersed phase particle size is on the same order of magnitude as the visible light wavelength (i.e., 90 nm-400 nm), the scattering mechanism transitions from Rayleigh scattering to Mie scattering. The characteristics of Mie scattering are: ① the scattering intensity is weakly dependent on wavelength, scattering is uniform across the entire wavelength range, and no obvious color shift is produced; ② the proportion of forward scattering is high, yet clear high-gloss reflection is still retained (corresponding to the "sharp high-gloss" of silk); ③ there are also appropriate amounts of backscattering and lateral scattering, forming a soft diffuse reflection layering (corresponding to the "soft luster" of silk).

[0031] The refractive index difference |n1-n2| determines the scattering cross-section of a single dispersed phase particle: the larger the refractive index difference, the larger the scattering cross-section of a single particle, and the higher the scattering intensity. When |n1-n2|<0.05, the scattering cross-section is too small, and light hardly scatters, passing directly through the wire and failing to form an effective diffuse reflection effect.

[0032] When the average equivalent diameter of the dispersed phase is too small (e.g., <90nm), even if the refractive index difference meets the requirement of ≥0.05, the dispersed phase particles enter the Rayleigh scattering dominance region, resulting in excessive short-wavelength light scattering, insufficient long-wavelength light scattering, and weakened forward scattering, making it difficult to form the "high-gloss sharpness + soft diffuse reflection" balance effect required for silk luster.

[0033] Therefore, the refractive index difference between the first and second polymer materials and the average equivalent diameter of the dispersed phase particles need to be controlled in order to achieve a good silk-like luster effect.

[0034] As an example, the glass transition temperatures of the wire, the first polymer material, and the second polymer material of this application can be tested by differential scanning calorimetry (DSC).

[0035] As an example, the morphology of the dispersed phase and the matrix phase can be tested by scanning electron microscopy (SEM). Specifically, by observing the quenched cross section of the wire using SEM, the dispersed phase and the matrix phase exhibit obvious two-phase separation morphology.

[0036] As an example, the refractive indices of the first and second polymer materials were obtained by the following method: using an Abbe refractometer, referring to the polymer refractive index testing standard ISO 489, under a standard light source (sodium yellow D line, wavelength 589.3nm) and a standard constant temperature environment (23℃), the refractive indices n1 and n2 of the first and second polymer materials were measured respectively, and |n1-n2| was calculated.

[0037] As an example, the average equivalent diameter of the dispersed phase particles can be obtained by the following method: the wire is frozen in liquid nitrogen for at least 15 minutes and then subjected to brittle fracture. To enhance the contrast of the phase regions, a selective solvent that dissolves only the dispersed phase or the matrix phase can be used to lightly etch the brittle fracture surface. After drying, the fracture surface is sputter-coated with gold. A scanning electron microscope (SEM) is used to capture the microscopic morphology of the cross-section of the wire perpendicular to the extrusion direction. Within a field of view of approximately 80 μm², the equivalent diameter of at least 100 particles with equal area is counted using ImageJ software. The average value is then taken to obtain the average equivalent diameter of the dispersed phase particles.

[0038] As an example, the absolute value of the refractive index difference between the first polymer material and the second polymer material, |n1-n2|, can be 0.05, 0.052, 0.055, 0.058, 0.06, 0.062, 0.065, 0.068, 0.07, 0.072, 0.075, 0.078, 0.08, 0.09, 0.1, 0.12, 0.15, 0.2, 0.22, 0.25, 0.3, or any value range between the two.

[0039] As an example, the average equivalent diameter of the dispersed phase particles can be 90 nm, 00 nm, 120 nm, 150 nm, 180 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, or any value between the two.

[0040] In some embodiments, the difference between the first glass transition temperature and the glass transition temperature of the first polymer material is no greater than 3°C; the difference between the second glass transition temperature and the glass transition temperature of the second polymer material is no greater than 3°C. Thus, the dispersed phase and the matrix phase have only weak interactions, limited compatibility, but stable phase states, providing physical interface conditions for light scattering.

[0041] As an example, the difference between the first glass transition temperature and the glass transition temperature of the first polymer material can be 0℃, 0.5℃, 1℃, 1.5℃, 2℃, 2.5℃, 3℃, or any value range between the two.

[0042] As an example, the difference between the second glass transition temperature and the glass transition temperature of the second polymer material can be 0℃, 0.5℃, 1℃, 1.5℃, 2℃, 2.5℃, 3℃, or any value range between the two.

[0043] In some embodiments, under the conditions of amorphous state and a test sample thickness of 2 mm: the transmittance of the first polymer material is not less than 85%; the transmittance of the second polymer material is not less than 85%. This results in the matrix phase and the dispersed phase having high transmittance to visible light, allowing light to penetrate deeply into the wire and induce deep scattering.

[0044] As an example, the transmittance of the first and second polymer materials was tested using the following method: a transmittance haze meter was used, referring to the standard test method for transmittance of transparent plastics, ISO 13468. The first and second polymer materials were respectively hot-pressed into standard test samples with a thickness of 2 mm and a smooth, defect-free surface. Their total transmittance to visible light was then tested, thus obtaining the transmittance of the first and second polymer materials in a non-crystalline state under the condition that the test sample thickness was 2 mm.

[0045] As an example, under the condition of non-crystalline state and test sample thickness of 2 mm, the transmittance of the first polymer material can be 85%, 88%, 90%, 92%, 95%, 98%, 99%, 100% or any value between two; the transmittance of the second polymer material can be 85%, 88%, 90%, 92%, 95%, 98%, 99%, 100% or any value between two.

[0046] In some embodiments, the first polymeric material includes one or more of polyethylene terephthalate (PETG) and polylactic acid (PLA); the second polymeric material includes one or more of polymethyl methacrylate (PMMA), styrene-ethylene-butene-styrene copolymer (SEBS), polybutylene adipate terephthalate (PBAT), polyethylene terephthalate (PETG), and polylactic acid (PLA). Thus, the aforementioned first and second polymeric materials are adaptable to the melt extrusion processing of wires, and by selecting different materials for combination, the refractive index difference between the matrix phase and the dispersed phase can be flexibly controlled to achieve controllable internal diffuse scattering and obtain a silk-like luster; simultaneously, the mechanical properties and printing performance of the wire can be considered.

[0047] In some embodiments, the average equivalent diameter of the dispersed phase particles is not less than 150 nm. Thus, the dispersed phase particle size matches the visible light wavelength range, enabling more effective Mie diffuse scattering and further enhancing the multiple reflections and refractions of light at the interface between the two phases within the wire, thereby achieving a superior and softer silk-like luster.

[0048] In some embodiments, |n1-n2|≥0.1, and the average equivalent diameter of the dispersed phase particles is not less than 200 nm. Thus, the refractive index difference between the first and second polymer materials works synergistically with the average equivalent diameter of the dispersed phase particles. A larger refractive index difference between the first and second polymer materials allows for a more appropriate reduction in the average equivalent diameter of the matched dispersed phase. This is because a larger refractive index difference itself provides a sufficient scattering cross-section. Even if the average equivalent diameter of the dispersed phase particles is small, the total scattering per unit volume can still meet the requirements of Mie diffuse scattering, and the wire can still achieve an excellent silk-like luster.

[0049] In some embodiments, 0.05 ≤ |n1-n2| < 0.1, and the average equivalent diameter of the dispersed phase particles is not less than 230 nm. Thus, the refractive index difference between the first and second polymer materials and the average equivalent diameter of the dispersed phase particles work synergistically. Since the refractive index difference between the first and second polymer materials is relatively small, the average equivalent diameter of the matched dispersed phase can be appropriately increased. This is because a smaller refractive index difference corresponds to a limited scattering intensity per particle, requiring an increase in the average equivalent diameter of the dispersed phase particles to enhance the scattering contribution of each particle, thereby improving the overall diffuse reflection effect of the wire and giving the wire an excellent silk-like luster.

[0050] In some embodiments, the mass fraction of the dispersed phase is 5%-25% based on the total mass of the wire; alternatively, the mass fraction of the dispersed phase is 10%-20%. Thus, the dispersed phase can form a uniformly distributed and appropriately numerous microscopic scattering interface within the matrix phase, matching the visible light Mie scattering mechanism, allowing light to undergo sufficient and moderate diffuse scattering within the wire.

[0051] As an example, the mass fraction of the dispersed phase can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, or any value between the two.

[0052] In some embodiments, based on the total mass of the wire, the mass fraction of the dispersed phase is M, where 5% ≤ M ≤ 10%; the average equivalent diameter of the dispersed phase particles is ≥ 220 nm. Thus, the matching design between the mass fraction of the dispersed phase and the average equivalent diameter of the dispersed phase in the wire produces a good synergistic effect. This is because a smaller mass fraction of the dispersed phase in the wire, meaning a smaller number of dispersed phase particles per unit volume, necessitates a larger average equivalent diameter of the dispersed phase particles. This ensures that light encounters a sufficient number of scattering interfaces as it travels through the wire, forming ample diffuse reflection and giving the wire an excellent silk-like luster.

[0053] In some embodiments, based on the total mass of the wire, the mass fraction of the dispersed phase is M, where 10% < M ≤ 25%; the average equivalent diameter of the dispersed phase particles is ≥ 170 nm. Thus, the matching design between the mass fraction of the dispersed phase and the average equivalent diameter of the dispersed phase in the wire produces a good synergistic effect. This is because a large mass fraction of the dispersed phase in the wire means a sufficient number of dispersed phase particles per unit volume, allowing for a suitable reduction in the average equivalent diameter of the dispersed phase particles. The sufficient number of scattering interfaces in the dispersed phase can compensate for the insufficient scattering intensity of individual particles, still enabling the wire to achieve an excellent silk-like luster.

[0054] In some embodiments, the roughness Ra of the filament is ≤0.4μm; optionally, the roughness Ra of the filament is ≤0.2μm. Thus, lower filament surface roughness can eliminate microscopic unevenness, scratches, and particle defects on the filament surface, resulting in more uniform filament melting and spreading during fused deposition modeling (FDM) printing, higher interlayer bonding consistency, reduced macroscopic scattering and specular reflections on the surface of 3D printed products, and reduced localized glare, whitening, and uneven lighting caused by filament surface roughness.

[0055] As an example, the roughness of the wire can be tested using the following method: A contact surface roughness meter is used to measure along the length of the wire. The test conditions are: probe tip radius 2 μm, measuring force 0.75 mN, cutoff wavelength λc = 0.8 mm, and evaluation length L = 4 mm. The average of three measurements is taken to obtain the roughness of the wire.

[0056] As an example, the roughness Ra of the wire can be 0.4μm, 0.3μm, 0.2μm, 0.1μm, 0.05μm, 0.01μm or any value between the two.

[0057] In a second aspect, this application proposes a method for preparing the aforementioned wire. This method involves screening the raw materials for wire preparation to ensure that the dispersed phase and the matrix phase each have independent glass transition temperatures, and that the absolute value of the refractive index difference between the first polymer material forming the matrix phase and the second polymer material forming the dispersed phase is greater than or equal to 0.05. This allows the dispersed phase and the matrix phase to form an island structure, providing a physical interface for light scattering. Furthermore, the island structure's phase interface can act as a scattering center, causing multiple interface reflections and refractions as light enters the wire, resulting in a soft, silky luster. The method further employs a masterbatch pre-dispersion and secondary dilution extrusion process to prepare the wire, which reduces the agglomeration of dispersed phase particles and improves... The uniform distribution of the dispersed phase in the matrix phase contributes to the formation of a uniform and stable two-phase interface. Simultaneously, using an extruder with a longer die flow channel to form wire allows for a longer melt residence time within the die, enabling more thorough relaxation of the viscoelastic strain of the polymer melt before exiting the die. This results in reduced and more stable exit expansion, smoothing out upstream inlet disturbances and velocity distortion. Consequently, it reduces surface ripples, microcracks, and die buildup, lowering surface roughness and enhancing specular reflectivity. Furthermore, with increasing die cavity volume and residence time, the collision and coalescence of dispersed phase droplets driven by interfacial tension increases the average equivalent diameter of the dispersed phase, further enhancing the silk-like luster of the wire. Specifically, the method includes: S1. Mix the first polymer material and the second polymer material to obtain a first mixture, and then melt-blend and extrude the first mixture to obtain a masterbatch.

[0058] In some embodiments, the first polymer material and the second polymer material are respectively subjected to drying treatment at a temperature of 60°C-80°C for a duration of 4-12 hours. This reduces the moisture content in the raw materials and minimizes hydrolysis, foaming, and degradation of the melt at processing temperatures.

[0059] In some embodiments, the mass fraction of the second polymeric material is 20%-50%, optionally 30%-45%, based on the mass of the first mixture. Therefore, the appropriate mass proportion of the second polymeric material in the first mixture is beneficial for having a suitable dispersed phase content in the final wire to form effective Mie scattering centers; it also helps to control the size of the dispersed phase in the masterbatch and reduce the brittleness of the masterbatch.

[0060] As an example, based on the mass of the first mixture, the mass fraction of the second polymer material can be 20%, 30%, 40%, 50%, or any value between the two.

[0061] In some embodiments, the mass fraction of the first polymeric material is 50%-80% based on the mass of the first mixture.

[0062] As an example, based on the mass of the first mixture, the mass fraction of the first polymeric material can be 50%, 60%, 70%, 80%, or any value between the two.

[0063] In some embodiments, the equipment for melt blending and extrusion granulation of the first mixture is a twin-screw extruder. Thus, the twin-screw extruder possesses excellent shearing, crushing, and mixing capabilities, ensuring that the second polymer material is uniformly dispersed within the first polymer material under the premise of sufficient melt plasticization, thereby constructing a uniform and stable two-phase microstructure. Pre-dispersion of the masterbatch using a twin-screw extruder provides a structurally uniform and performance-stable masterbatch raw material for subsequent secondary dilution extrusion to form wire.

[0064] In some embodiments, the first mixture is melt-blended and extruded into granules using a twin-screw extruder, wherein the temperature of the melt section of the twin-screw extruder is 220°C-250°C. This facilitates the complete melting and plasticization of the first and second polymer materials.

[0065] S2. The masterbatch and the first polymer material are mixed to obtain a second mixture, and the second mixture is extruded through an extruder to form a wire; wherein the die flow channel length of the extruder is ≥150mm.

[0066] In some embodiments, the second mixture is dried at a temperature of 60°C-80°C for 4-12 hours. This reduces the moisture content of the raw materials and minimizes hydrolysis, foaming, and degradation of the melt at processing temperatures.

[0067] In some embodiments, the mass fraction of the second polymer material is 5%-25% based on the mass of the second mixture. Thus, the adjustable mass percentage of the dispersed phase in the wire (5%-25%) helps the dispersed phase form a uniformly distributed and appropriately abundant microscopic scattering interface in the matrix phase, matching the visible light Mie scattering mechanism and enabling sufficient and appropriate diffuse scattering of light within the wire.

[0068] In this application, the second polymer material in the second mixture is derived from the second polymer material in the masterbatch.

[0069] As an example, based on the mass of the second mixture, the mass fraction of the second polymeric material can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, or any value between the two.

[0070] In some embodiments, the mass fraction of the first polymeric material is 75%-95% based on the mass of the second mixture.

[0071] In some embodiments, the equipment for extruding the second mixture into wire is a single-screw extruder. Therefore, the single-screw extruder provides gentle shearing, which better preserves the original island-island phase morphology in the masterbatch, reduces excessive shearing and breakage of dispersed phase particles, and ensures the integrity of the two-phase interface, thereby maintaining the light scattering effect inside the wire and obtaining a stable silk-like luster. Simultaneously, the single-screw extruder can output stable and uniform melt pressure, which is beneficial for obtaining wires with uniform diameter.

[0072] In some embodiments, the extruder die length is ≥150mm. This allows for a longer melt residence time within the die, enabling more thorough relaxation of the viscoelastic strain of the polymer melt before exiting the die, resulting in reduced and more stable exit expansion. Upstream inlet disturbances and velocity distortion are smoothed out, thereby reducing surface ripples, microcracks, and die buildup on the wire, lowering surface roughness, and enhancing the wire's specular reflectivity. Furthermore, as the die cavity volume and residence time increase, the dispersed phase droplets collide and coalesce under interfacial tension, which helps increase the average equivalent diameter of the dispersed phase in the wire, thus improving the wire's silky luster.

[0073] As an example, the length of the extruder die can be 150mm, 160mm, 164mm, 170mm, 180mm, 190mm, 200mm or any value between the two.

[0074] In some embodiments, the die temperature of the extruder die head is 220°C-270°C, optionally 230°C-250°C. This allows the viscosity of the dispersed phase and the matrix phase to be controlled within a suitable range, thereby reducing the breakage of dispersed phase droplets during extrusion and helping to increase the average equivalent diameter of the dispersed phase in the wire.

[0075] As an example, the die temperature of the extruder die head can be 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, or any value between two of these.

[0076] In a third aspect, this application proposes a 3D printed article obtained by printing using the aforementioned filament or filament prepared by the aforementioned method. Thus, the 3D printed article possesses all the features and advantages of the aforementioned filament for 3D printing or its preparation method, which will not be repeated here.

[0077] In some embodiments, the 3D printed article is obtained by fused deposition modeling (FDM) using the aforementioned filament or filament prepared by the aforementioned method.

[0078] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.

[0079] The following specific embodiments illustrate the solution of this application. It should be noted that these embodiments are for illustrative purposes only and should not be considered as limiting the scope of this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0080] Example 1 <Wire Preparation> S1. Preparation of Masterbatch: Polyethylene terephthalate (PETG, refractive index n1 of 1.568, light transmittance of 88%, Honggang Petrochemical, HG-2601) and polymethyl methacrylate (PMMA, refractive index n2 of 1.490, light transmittance of 92%, Wanhua Chemical, OD02) were weighed at a mass ratio of 60:40. PETG and PMMA were dried in forced-air ovens at 70℃ and 80℃ respectively for 4 hours. The dried PETG and PMMA were mixed to obtain the first mixture, which was then fed into a twin-screw extruder (length-to-diameter ratio L / D of 40:1) for melt blending extrusion granulation. The extruder temperatures are set as follows: 150℃ (conveyor section) / 210℃ / 240℃ (melting section) / 240℃ / 230℃ (mixing section) / 220℃ (venting section) / 220℃ / 220℃ / 220℃ (homogenization section) / 220℃ (die head). The main extruder speed is 300 rpm. Water-cooled pellets are drawn and granulated to obtain masterbatch, in which the mass fraction of PMMA (the second polymer material) is 40%.

[0081] S2, Wire extrusion molding: The masterbatch prepared above was mixed with the first polymer material PETG at a mass ratio of 1:3 to obtain a second mixture (the mass fraction of the second polymer material PMMA in the second mixture was 10%). The second mixture was placed in a 70°C forced-air oven and dried for 4 h. The dried second mixture was then fed into a single-screw extruder (length-to-diameter ratio L / D≈28:1) for extrusion molding to obtain wire with a diameter of 1.75 mm.

[0082] The single-screw extruder is connected to a die head, characterized by a flow channel length of 164.0 mm. The temperature settings for each section of the single-screw extruder are as follows: feed section 180℃, compression section 230℃, melting section 245℃, and die zone 240℃.

[0083] Examples 2 to 3 Except for the section on "Preparation of Wires", which adjusts the type of the first or second polymer material according to Table 1, the rest is the same as in Example 1.

[0084] In Example 2, the second polymer material, styrene-ethylene-butene-styrene copolymer (SEBS, Zhongli Technology, S6553), has a refractive index n2 of 1.500 and a light transmittance of 85%; in Example 3, the first polymer material, polylactic acid (PLA, Fengyuan, FY-802), has a refractive index n1 of 1.450 and a light transmittance of 90%.

[0085] Examples 4 to 6 Except for the preparation of the wire, in which the mass ratio of the masterbatch to the first polymer material in S2 is adjusted to adjust the mass fraction of the second polymer material in the second mixture, and wires with different dispersed phase mass fractions as shown in Table 1 are prepared, the rest is the same as in Example 1.

[0086] Examples 7 to 9 Except for adjusting the temperature of the die zone of the single-screw extruder in S2 during the <Wire Preparation> process, the process is the same as in Example 1. Specifically, the die zone temperature of the single-screw extruder in Example 7 is 230°C, the die zone temperature of the single-screw extruder in Example 8 is 220°C, and the die zone temperature of the single-screw extruder in Example 9 is 270°C.

[0087] Comparative Example 1 Except for the section on "Preparation of Wire", which uses only PETG as raw material for direct S2 wire extrusion molding, the rest is the same as in Example 1.

[0088] Comparative Example 2 Except for the section on "Preparation of Wires," where the type of the second polymer material is adjusted to styrene-acrylonitrile copolymer (SAN, D-178HF Chimei) according to Table 1, the rest is the same as in Example 1. The second polymer material, styrene-acrylonitrile copolymer (SAN), has a refractive index of 1.570 and a light transmittance of 89%.

[0089] Comparative Example 3 Except for the section on "Preparation of Wires", which adjusts the type of the first polymer material to polylactic acid (PLA) and the type of the first polymer material to polymethyl methacrylate (PMMA) according to Table 1, the rest is the same as in Example 1.

[0090] Comparative Example 4 Except for the section on "Preparation of Wire," in which the length of the die runner of the single-screw extruder is adjusted to 104 mm during the S2 wire extrusion molding process, the rest is the same as in Example 1.

[0091] Performance testing: Testing of wire roughness The surface roughness of the wire was measured along its length using a contact surface roughness tester. The test conditions were: probe tip radius 2 μm, measuring force 0.75 mN, cutoff wavelength λc = 0.8 mm, and evaluation length L = 4 mm. The roughness of the wire was obtained by averaging three measurements.

[0092] Testing the roughness of 3D printed products The filament prepared above was fused deposition modeled to obtain a 3D printed product. The printing equipment was a Topzhu P1S, and the printing model was a 4-layer cube (100mm cube). When the matrix material was PETG, the printing speed was 50mm / s and the printing temperature was 260℃; when the matrix material was PLA, the printing speed was 50mm / s and the printing temperature was 230℃. A digital microscope with 3D morphology analysis function was used, and the surface of the single-layer filament of the 3D printed part was subjected to high-magnification optical imaging and 3D morphology reconstruction according to the non-contact surface morphology measurement standard ISO25178. Subsequently, using morphology analysis software, the cross-sectional contour line was extracted along the XY direction (i.e., the forming direction) parallel to the extrusion path, and the arithmetic mean roughness in this direction was calculated and derived.

[0093] Testing the gloss of 3D printed products The filament prepared above was used to form a 3D printed product through fused deposition modeling. The printing equipment was a Topzhu P1S, and the printing model was a 4-layer cube (100mm cube). When the matrix material was PETG, the printing speed was 50mm / s and the printing temperature was 260℃; when the matrix material was PLA, the printing speed was 50mm / s and the printing temperature was 230℃. The gloss of the 3D printed product was measured using a gloss meter at a 60° angle, according to ASTM D523 standard.

[0094] Sensory evaluation of 3D printed products (rating for silk-like luster) The filament prepared above was fused deposition modeled to obtain a 3D printed product. The printing equipment was a Topzhu P1S, and the printing model was a 4-layer square frame (100mm cube). When the matrix material was PETG, the printing speed was 50mm / s and the printing temperature was 260℃. When the matrix material was PLA, the printing speed was 50mm / s and the printing temperature was 230℃. A corrugated board model was selected as the standard test piece.

[0095] Testing the interlayer strength of 3D printed products The filament prepared above was subjected to fused deposition modeling (FDM) to obtain a 3D printed product. The printing equipment was a Tuozhu P1S, printing dumbbell-shaped tensile strips along the Z-axis. When the matrix material was PETG, the printing speed was 50 mm / s and the printing temperature was 260℃; when the matrix material was PLA, the printing speed was 50 mm / s and the printing temperature was 230℃. The interlayer strength of the 3D printed product was measured using an MTS universal testing machine at a fixed speed of 10 mm / min, in accordance with standard ISO 527.

[0096] The preparation parameters and performance parameters of the examples and comparative examples are shown in Tables 1 and 2.

[0097] Table 1

[0098] Note: The DSC curves of the wires in Examples 1 to 9 all have two independent first glass transition temperatures and first glass transition temperatures; T1 is the difference between the first glass transition temperature of the wire and the glass transition temperature of the first polymer material, and T2 is the difference between the second glass transition temperature of the wire and the glass transition temperature of the second polymer material; " / " in Table 1 indicates that there are no relevant preparation parameters.

[0099] Table 2

[0100] As shown in Table 2, the matrix phase of the filament includes a first polymer material, and the dispersed phase includes a second polymer material. The filament has two independent glass transition temperatures, the refractive index difference between the first and second polymer materials is greater than or equal to 0.05, and the average equivalent diameter of the dispersed phase particles is not less than 90 nm. The resulting filament has low roughness, and the 3D printed products prepared from the filament have good gloss and a good silk-like luster. Furthermore, the interlayer strength of the 3D printed products is high, meeting the application requirements. In contrast, the filament of Comparative Example 1 only includes a matrix phase, the refractive index difference between the first and second polymer materials in Comparative Examples 2 and 3 is less than 0.05, and the average equivalent diameter of the dispersed phase particles in the filament of Comparative Example 4 is only 70 nm. The 3D printed products prepared from the filaments of Comparative Examples 1 to 4 all have low gloss and lack a silk-like texture or have a poor silk-like texture.

[0101] from Figure 1 It can be seen that Embodiment 1 of this application has two independent glass transition temperatures, and the difference between the first glass transition temperature of the wire and the glass transition temperature of the single-component PTEG material is small, only 1.86℃. The difference between the second glass transition temperature of the wire and the glass transition temperature of the single-component PMMA material is also only 1.84℃. This indicates that the matrix phase and the dispersed phase of the wire in Embodiment 1 have thermodynamic incompatibility, which can provide physical interface conditions for light scattering.

[0102] from Figure 2 The SEM images of the wires from Examples 6, 7, 8, Comparative Example 1, and Comparative Example 2, taken perpendicular to the extrusion direction, show that the dispersed phase in Examples 6 to 8 is uniformly distributed in the matrix phase, with the dispersed phase in Example 6 having the largest diameter. Comparative Example 1, however, consists only of a single matrix phase with no dispersed phase; the dispersed phase in Comparative Example 4 has a smaller diameter and a wider particle size distribution.

[0103] Figure 3These are photographs of the wires prepared in Example 6, Comparative Example 1, and Comparative Example 4 of this application. Figure 3 It can be seen that the surface of the wire prepared in Example 6 is smooth and bright, while the surface of the wire prepared in Comparative Example 1 has a general gloss, and the surface of the wire prepared in Comparative Example 4 is relatively dull.

[0104] Figure 4 The images show photographs of the 3D printed products prepared in Example 6, Comparative Example 1, and Comparative Example 4 of this application. As can be seen from the images, the 3D printed product prepared in Example 6 has sharp highlights, a strong sense of light flow, and a distinct silk-like texture; while the 3D printed product prepared in Comparative Example 1 has no silk-like texture and only has ordinary transparent luster; the 3D printed product prepared in Comparative Example 4 has poor texture and blurred highlights.

[0105] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A wire for 3D printing, characterized in that, It includes a continuous matrix phase and a dispersed phase distributed in the matrix phase, the matrix phase including a first polymer material, the dispersed phase including a second polymer material, and the wire having its own independent first glass transition temperature and second glass transition temperature. The refractive index of the first polymer material is n1, the refractive index of the second polymer material is n2, and |n1-n2|≥0.05; The average equivalent diameter of the dispersed phase particles is not less than 90 nm.

2. The wire of claim 1, wherein The difference between the first glass transition temperature and the glass transition temperature of the first polymer material is no greater than 3°C; the difference between the second glass transition temperature and the glass transition temperature of the second polymer material is no greater than 3°C.

3. The wire according to claim 1, characterized in that, Under the conditions of non-crystalline state and test sample thickness of 2 mm: the light transmittance of the first polymer material is not less than 85%; the light transmittance of the second polymer material is not less than 85%.

4. The wire according to any one of claims 1-3, characterized in that, The first polymeric material includes one or more of polyethylene terephthalate and polylactic acid; the second polymeric material includes one or more of polymethyl methacrylate, styrene-ethylene-butene-styrene copolymer, polybutylene adipate-terephthalate, polyethylene terephthalate, and polylactic acid.

5. The wire according to any one of claims 1-3, characterized in that, The average equivalent diameter of the dispersed phase particles is not less than 150 nm.

6. The wire according to any one of claims 1-3, characterized in that, Based on the total mass of the wire, the mass fraction of the dispersed phase is 5%-25%.

7. The wire according to any one of claims 1-3, characterized in that, The roughness Ra of the wire is ≤0.4μm.

8. A method for preparing a wire as described in any one of claims 1-7, characterized in that, include: The first polymer material and the second polymer material are mixed to obtain a first mixture. The first mixture is then melt-blended, extruded, and granulated to obtain a masterbatch. The masterbatch and the first polymer material are mixed to obtain a second mixture, and the second mixture is extruded through an extruder to form wire. The extruder die flow channel length is ≥150mm.

9. The method according to claim 8, characterized in that, The die temperature of the extruder die head is 220℃-270℃, and can be selected as 230℃-250℃.

10. The method according to claim 8 or 9, characterized in that, Based on the mass of the first mixture, the mass fraction of the second polymer material is 20%-50%; based on the mass of the second mixture, the mass fraction of the second polymer material is 5%-25%.

11. A 3D printed product, characterized in that, The wire prepared using the wire as described in any one of claims 1-7 or the method described in any one of claims 8-10 is printed.