A carbon nanomaterial-reinforced PA66, its preparation method and application
By introducing modified graphene oxide into PA66 resin, the problems of heavy weight, easy corrosion and complex molding of drone robotic arm materials have been solved, realizing high strength, rigidity and water-resistant carbon nanomaterial-reinforced PA66, which is suitable for agricultural drone robotic arms.
Patent Information
- Application Number
- CN202611380251.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing materials for drone robotic arms suffer from problems such as heavy weight, susceptibility to corrosion, high molding costs, complex processing, and limited resistance to media penetration in agricultural environments, making it difficult to meet the requirements of lightweight, corrosion resistance, and structural stability.
PA66 is reinforced with carbon nanomaterials by introducing modified graphene oxide into the PA66 resin. The modified graphene oxide has long-chain aliphatic segments grafted on its surface and contains carboxyl groups, which improves the dispersion uniformity and interfacial interaction, and enhances the mechanical properties and water permeability of the composite material.
The method achieves high strength, rigidity, toughness, and water resistance of PA66 reinforced with carbon nanomaterials, reduces the material's water absorption tendency, improves the performance retention rate after humid heat aging, and meets the application requirements of agricultural drone arms.
Smart Images

Figure CN123107352A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of modified materials technology, specifically relating to a carbon nanomaterial-reinforced PA66, its preparation method and application, and particularly a carbon nanomaterial-reinforced PA66 for the arm of an agricultural drone and its preparation method. Background Technology
[0002] With the increasing application of agricultural drones in scenarios such as plant protection spraying, farmland inspection, crop sampling, and fruit and vegetable harvesting assistance, the demand for drones equipped with robotic arms or end effectors is gradually increasing. Robotic arms can be used to connect nozzles, grippers, samplers, sensors, or other auxiliary operating components, enabling drones to have a certain degree of stationary operation capability.
[0003] Existing drone robotic arms are typically made of aluminum alloy, stainless steel, carbon fiber composites, or ordinary engineering plastics. While metal materials offer good strength and connection stability, their greater weight increases the drone's load, affecting endurance and flight stability. Furthermore, agricultural operating environments often involve water mist, pesticide droplets, fertilizer solutions, mud, high humidity, and fluctuating temperatures, making metal robotic arms or connecting components prone to corrosion, rust, and increased maintenance costs after prolonged use. Carbon fiber composites offer significant lightweight advantages, but their molding costs are high, and their processing and connection structure design require sophisticated techniques; some complex structural components are not suitable for low-cost mass production. While ordinary engineering plastics are lightweight, their rigidity, bending and torsional strength, impact resistance, and long-term environmental stability are limited, making it difficult to simultaneously meet the requirements of lightweight, corrosion resistance, and structural stability for agricultural drone robotic arms.
[0004] PA66, as a commonly used engineering plastic, has good mechanical properties, wear resistance and processing performance. It can be used to prepare structural parts through injection molding, extrusion, compression molding and other methods. However, PA66 material alone may still have problems such as insufficient dimensional stability, limited resistance to media penetration and easy deformation of stressed parts under long-term stress, humid environment and pesticide and fertilizer media.
[0005] Therefore, there is a need to provide a lightweight, corrosion-resistant, and anti-aging material suitable for agricultural drones to meet application requirements. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a carbon nanomaterial-reinforced PA66, its preparation method, and its application. The carbon nanomaterial-reinforced PA66 provided by the present invention has the advantages of being lightweight, corrosion-resistant, and anti-aging, and can fully meet the application requirements of agricultural drone arms.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] In a first aspect, the present invention provides a carbon nanomaterial-reinforced PA66, comprising, by weight, 98-100 parts of PA66 resin, 0.3-1 parts of modified graphene oxide, and 0.4-1.5 parts of processing aids, wherein:
[0009] The modified graphene oxide surface is grafted with C10-C15 aliphatic alkyl chains with carboxyl groups at the ends.
[0010] This invention introduces modified graphene oxide with long-chain aliphatic segments grafted onto its surface and carboxyl groups at the ends. Graphene oxide can serve as a reinforcing phase in composite materials to improve their mechanical properties. The long-chain aliphatic segments reduce the excessive hydrophilicity of the graphene oxide sheet surface and inhibit re-agglomeration, thereby improving the dispersion uniformity of graphene oxide. The retained polar groups (such as carboxyl groups) can form an interfacial interaction with PA66 amide groups, further improving the dispersion uniformity of graphene oxide.
[0011] Therefore, by introducing modified graphene oxide into PA66 resin, this invention can solve the problems of easy agglomeration of graphene oxide, insufficient interfacial bonding with PA66, and excessive hydrophilic oxygen-containing groups. The resulting carbon nanomaterial-reinforced PA66 not only has excellent processability and toughness, but also significantly improves its strength, rigidity, water permeability resistance, and performance retention rate after humid heat aging.
[0012] In this invention, the PA66 resin comprises 98-100 parts, for example 98 parts, 98.5 parts, 99 parts, 99.5 parts, 100 parts or any of the above values; the modified graphene oxide comprises 0.3-1 parts, for example 0.3 parts, 0.45 parts, 0.6 parts, 0.75 parts, 1 part or any of the above values; and the processing aid comprises 0.4-1.5 parts.
[0013] In some embodiments, the mass percentage of PA66 resin is 98-99.3%, for example, 98%, 98.2%, 98.5%, 98.8%, 99%, 99.3%, or any range of the above values, based on the total mass of the carbon nanomaterial-reinforced PA66 as 100%.
[0014] In some embodiments, based on the total mass of the carbon nanomaterial-reinforced PA66 as 100%, the mass percentage of the modified graphene oxide is 0.3-1%, for example 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or any of the above values, preferably 0.5%.
[0015] The modified graphene oxide described in this invention can exert reinforcing and barrier effects at relatively low addition levels, which is beneficial for improving the strength and rigidity of PA66 composite materials while maintaining good toughness. Furthermore, the modified graphene oxide sheets and their surface-modified structures can extend the diffusion path of moisture and agricultural media within the material, reducing the material's water absorption tendency and improving the retention rate of mechanical properties after exposure to humid heat and pesticide / fertilizer media. If the addition amount is too high, it may increase melt viscosity and affect toughness; if the addition amount is too low, the reinforcing and barrier effects on the material will be limited.
[0016] The modified graphene oxide of this invention is prepared by grafting graphene oxide and a modifier (preferably 11-aminoundecanoic acid) together. The carboxyl groups on the surface of the graphene oxide form an active ester intermediate under the action of EDC / NHS, which then undergoes an amidation reaction with the primary amino group in the modifier, thereby introducing a long-chain aliphatic structure and terminal carboxyl groups onto the surface of the graphene oxide. Specific steps include:
[0017] Graphene oxide is activated and then subjected to an amidation reaction with a C10-C15 aliphatic alkyl modifier with a carboxyl group at the end to obtain the modified graphene oxide, wherein the modifier contains an amino group.
[0018] In some embodiments, the mass ratio of the modifier to graphene oxide is (1-5):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1 or any range between the above values.
[0019] In some embodiments, the amidation reaction is carried out at a temperature of 40-60°C, such as 40°C, 45°C, 50°C, 55°C, 60°C or any of the above values, and for a time of 6-24 h, such as 6 h, 9 h, 12 h, 18 h, 24 h or any of the above values.
[0020] In some embodiments, the modifier is 11-aminoundecanoic acid and / or 12-aminododecanoic acid.
[0021] In some embodiments, the method for preparing the modified graphene oxide includes:
[0022] S1. Dispersion: Graphene oxide is dispersed in a solvent to obtain a graphene oxide dispersion;
[0023] S2. Carboxyl group activation: Activation is performed by mixing graphene oxide dispersion with EDC / NHS;
[0024] S3. Grafting reaction: The modifier solution is mixed with the activated graphene oxide dispersion and amidation reaction (grafting reaction) is carried out at 40-60℃ for 6-24 h;
[0025] S4. After the reaction is complete, collect the solid, wash and dry it to obtain the modified graphene oxide.
[0026] In some embodiments, the concentration of the graphene oxide dispersion is 0.5-2 mg / mL, for example, 0.5 mg / mL, 1.0 mg / mL, 1.5 mg / mL, 2.0 mg / mL or any of the above values; the pH value of the dispersion is 5.0-6.0, for example, 5.0, 5.3, 5.5, 5.6, 5.8, 6.0 or any of the above values; and preferably, the dispersion time is 30-60 min, for example, 30 min, 40 min, 45 min, 50 min, 60 min or any of the above values.
[0027] In some embodiments, the solvent used in the graphene oxide dispersion is MES buffer or other aqueous dispersion medium.
[0028] In some embodiments, the mass ratio of graphene oxide, EDC, and NHS is 1:(2-5):(1-3), where 2-5 can be 2, 2.5, 3, 3.5, 4, 4.4, 5, or any of the above values, and 1-3 can be 1, 1.5, 2, 2.5, 3, or any of the above values. Preferably, the activation temperature is 20-30°C, such as 20°C, 23°C, 25°C, 28°C, 30°C, or any of the above values, and the activation time is 30-120 min, such as 30 min, 50 min, 70 min, 90 min, 120 min, or any of the above values.
[0029] In some embodiments, the concentration of the modifier solution is 0.01-0.03 g / mL, for example 0.01 g / mL, 0.015 g / mL, 0.02 g / mL, 0.025 g / mL, 0.03 g / mL or any of the above values, the dispersion medium used in the solution includes DMF, ethanol / water, etc., and the pH value of the amidation reaction is 7.0-8.0, for example 7.0, 7.3, 7.5, 7.8, 8.0 or any of the above values.
[0030] In some embodiments, the method of collecting solids includes centrifugation or filtration, and the drying method includes freeze drying or low-temperature vacuum drying, wherein the low temperature includes 50-70°C, for example 50°C, 55°C, 60°C, 65°C, 70°C or any range between the above values.
[0031] In some embodiments, the method for preparing the modified graphene oxide includes:
[0032] S1. Dispersion: Graphene oxide is ultrasonically dispersed in a solvent for 30-60 min, and the pH value is adjusted to 5.0-6.0 to obtain a uniform and stable graphene oxide dispersion with a concentration of 0.5-2.0 mg / mL.
[0033] S2. Carboxyl activation: EDC / NHS was added to the graphene oxide dispersion and mixed according to the mass ratio of graphene oxide, EDC and NHS of 1:(2-5):(1-3). The mixture was activated at 20-30℃ for 30-120 min to form intermediates with amine reactivity on the surface of graphene oxide.
[0034] S3. Grafting reaction: The modifier is dispersed / dissolved in media such as DMF, ethanol / water to obtain a modifier solution. The modifier solution is slowly added to the activated graphene oxide dispersion. The pH of the reaction system is adjusted to 7.0-8.0, and the reaction is carried out at 40-60℃ for 6-24 h, so that the modifier (amino) is grafted onto the surface of graphene oxide through amide bonds.
[0035] S4. After the reaction is complete, centrifuge or filter to collect the solid. Wash the solid sequentially with the reaction solvent, ethanol and deionized water to remove unreacted modifier and activating agent. Freeze-dry the washed solid or vacuum dry it at 50-70℃ to constant weight to obtain the modified graphene oxide.
[0036] The graphene oxide described in this invention can be commercially available graphene oxide or graphene oxide obtained through a preparation method. Any graphene oxide that meets the application requirements can be used in this invention, and will not be listed in detail here. In some embodiments, this invention preferably obtains graphene oxide through a preparation method. This invention can control the sheet morphology and surface oxygen-containing functional group state of graphene oxide by controlling graphite raw materials, exfoliation conditions, oxidation degree, etc., which is beneficial to maintaining the consistency of different batches of raw materials and providing a more stable substrate for the subsequent grafting reaction of long-chain aliphatic modifiers.
[0037] In some embodiments, the method for preparing graphene oxide includes sequentially oxidizing, exfoliating, washing, drying and grinding the raw materials; the preparation method provided by the present invention can introduce oxygen-containing functional groups on the surface and between the graphite sheets, and form sheet-like graphene oxide through subsequent exfoliation treatment.
[0038] The graphene oxide prepared by this invention has an irregular sheet-like structure, with curled, wrinkled and locally folded morphologies at the edges of the sheets.
[0039] In some embodiments, the raw material includes any one or a combination of at least two of natural flake graphite, graphite powder, or expanded graphite.
[0040] In some embodiments, the method for preparing the graphene oxide includes:
[0041] (1) Raw material pretreatment: The raw materials are dried;
[0042] (2) Oxidation reaction: Under acidic conditions, the raw materials and oxidant are mixed to carry out an oxidation reaction to obtain an oxidized graphite reaction solution;
[0043] (3) Termination of reaction: After the oxidation reaction is complete, hydrogen peroxide solution is added to the reaction system to terminate the reaction of residual oxidant, and a dispersion of crude graphite oxide product is obtained;
[0044] (4) Washing and purification: The crude product dispersion was centrifuged or filtered, and the resulting solid was washed successively with dilute sulfuric acid solution and deionized water to obtain graphite oxide;
[0045] (5) Exfoliation process: The graphene oxide is redispersed and the dispersion is exfoliated to form a graphene oxide dispersion.
[0046] (6) Drying to prepare powder: Dry the graphene oxide dispersion to obtain graphene oxide powder. Preferably, after drying, the powder is ground or sieved to obtain the graphene oxide.
[0047] In some embodiments, the method for preparing the graphene oxide includes:
[0048] (1) Raw material pretreatment: The raw material is dried to remove the adsorbed moisture. The drying temperature is preferably 60-80℃, such as 60℃, 65℃, 70℃, 75℃, 80℃ or any of the above values, and the time is 6-12h, such as 6h, 8h, 9h, 10h, 12h or any of the above values. The dried raw material is then ready for use.
[0049] (2) Oxidation reaction: Under acidic conditions, the raw material and oxidant are mixed to carry out an oxidation reaction, wherein the oxidation reaction gradually occurs between the layers of the raw material (graphite); the acidic environment can be a concentrated sulfuric acid system, or a mixed system of concentrated sulfuric acid and phosphoric acid, preferably the mass ratio of the raw material to the acidic environment is 1:(30-50), for example 1:30, 1:35, 1:40, 1:45, 1:50 or any of the above values, and the mixing is carried out in an ice bath or at low temperature (0-10℃, for example 0℃, 1℃, 2℃, 5℃, 8℃, 10℃ or The reaction is carried out within the range of any of the above values. Preferably, the oxidant includes potassium permanganate. Preferably, the mass ratio of the raw material to the oxidant is 1:(1-5), for example, 1:1, 1:2, 1:3, 1:4, 1:5 or any of the above values. Preferably, the feeding rate of the oxidant is controlled to avoid a rapid increase in the system temperature. Preferably, after the oxidant is completely added, the temperature of the reaction system is raised to 35-50°C, for example, 35°C, 40°C, 45°C, 48°C, 50°C or any of the above values, and the reaction is continued with stirring for 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours or any of the above values, so that the raw material sheets are fully oxidized to obtain an oxidized graphite reaction solution.
[0050] (3) Termination of reaction: After the oxidation reaction is complete, the reaction system is slowly added to deionized water for dilution and the temperature change is controlled. Then, hydrogen peroxide solution is added to terminate the reaction of residual oxidant, so that the color of the system gradually changes from dark to brownish-yellow or yellowish-brown, and a dispersion of crude graphite oxide product is obtained.
[0051] (4) Washing and purification: Centrifuge or filter the crude product dispersion to remove the supernatant or filtrate. The resulting solid is washed with dilute sulfuric acid solution and deionized water in sequence to remove residual metal ions, acid and reaction by-products. Wash until the washing solution is close to neutral or meets the requirements for subsequent use. It is preferable to use dialysis to further remove residual small molecule impurities and salts.
[0052] (5) Exfoliation treatment: The treated graphene oxide is redispersed to obtain a dispersion. Preferably, the concentration of the dispersion is 1-2 mg / mL, such as 1 mg / mL, 1.2 mg / mL, 1.5 mg / mL, 1.6 mg / mL, 1.8 mg / mL, 2 mg / mL or any of the above values. Preferably, the dispersion solvent includes deionized water and / or ethanol. The dispersion is exfoliated, preferably by ultrasonic exfoliation and / or mechanical stirring exfoliation, to form a graphene oxide dispersion. Preferably, the ultrasonic exfoliation time is 30-120 min, such as 30 min, 50 min, 70 min, 90 min, 120 min or any of the above values.
[0053] (6) Drying to prepare powder: The graphene oxide dispersion is dried, preferably by freeze drying, vacuum drying at 50-70℃ or spray drying, to obtain graphene oxide powder. Freeze drying or low temperature (50-60℃, for example 50℃, 52℃, 55℃, 58℃, 60℃ or any of the above values) vacuum drying is further preferred to reduce the agglomeration of the sheets. After drying, the powder is ground or sieved to obtain the graphene oxide.
[0054] The graphene oxide prepared by the method provided in this invention exhibits an irregular distribution of nanosheets with varying sheet sizes, some overlap, and some inter-sheet bonding. However, it still maintains a relatively thin sheet structure overall, with visible curling, wrinkling, and local folding at the edges. In this invention, the sheet-like and wrinkled structure helps to increase the contact area between graphene oxide and the PA66 matrix. After being dispersed in the PA66 matrix, it can form a reinforcing support structure within the material, improving the stress transmission capacity of the composite material under stress. Simultaneously, the graphene oxide sheets can also form tortuous media diffusion paths within the PA66 matrix, delaying the entry of media such as moisture, pesticide droplets, and fertilizer solutions into the material, thereby improving the corrosion resistance and environmental aging resistance of the robotic arm body.
[0055] In some embodiments, the relative viscosity of the PA66 resin is 2.5-3.0, for example, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0 or any of the above values, preferably 2.62-2.72.
[0056] In some embodiments, the processing aid includes any one or a combination of at least two of antioxidants, lubricants, or weathering agents.
[0057] In some embodiments, the antioxidant is included in parts by weight of 0.2-0.5 parts, such as 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, or any range of the above values.
[0058] In some embodiments, the lubricant comprises 0.2-0.8 parts by weight, such as 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, or any range of the above values.
[0059] In some embodiments, the weathering agent is included in 0.2-0.5 parts by weight, for example, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts or any range between the above values. Preferably, the weathering agent includes hindered amine light stabilizers and / or ultraviolet absorbers, etc.
[0060] In some embodiments, the antioxidant includes any one or a combination of at least two of antioxidant 1098, antioxidant 1010, antioxidant 1076, or antioxidant 168;
[0061] In some embodiments, the lubricant comprises any one or a combination of at least two of ethylene bis-stearamide, calcium stearate, zinc stearate, or polyethylene wax.
[0062] In a second aspect, the present invention provides a method for preparing carbon nanomaterial-reinforced PA66 as described in the first aspect, the method comprising:
[0063] The components in the formula are mixed, melt-extruded, cooled and granulated to obtain the carbon nanomaterial-reinforced PA66.
[0064] In some embodiments, the preparation method includes:
[0065] The raw materials are first dried, and then the components are mixed and melt-blended in a twin-screw extruder. The extrusion temperature is controlled at 265-285℃, for example, 265℃, 268℃, 270℃, 272℃, 275℃, 278℃, 280℃, 282℃, 285℃ or any of the above values. The screw speed is 100-300 r / min, for example, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min or any of the above values.
[0066] Thirdly, the present invention provides an application of carbon nanomaterial-reinforced PA66 as described in the first aspect in the arm of an agricultural drone.
[0067] The carbon nanomaterial-reinforced PA66 described in this invention can be used in the main body of the arm of an agricultural drone. While meeting the requirements of arm load-bearing capacity and structural stability, it helps to reduce the weight of components and avoids the corrosion problem of traditional metal materials in humid and agricultural operating environments. It has good processing feasibility and application adaptability.
[0068] In some embodiments, the main body of the agricultural drone arm of the present invention is prepared by injection molding using carbon nanomaterial-reinforced PA66.
[0069] In some embodiments, the main body of the arm may be in the form of a long strip, a tube, a beam, or an irregularly shaped support structure, used to support, connect, and transfer loads during the operation of the agricultural drone.
[0070] In some embodiments, one end of the main body of the arm can be connected to the drone body, mounting base, or connecting joint, while the other end can be connected to a nozzle, gripper, sampler, lever, sensor mounting base, or other agricultural operating components. Depending on actual usage requirements, connection holes, mounting grooves, locally thickened connection ends, or insert connection portions can be provided on the main body of the arm to improve assembly stability and connection reliability; however, this invention does not impose excessive limitations on these aspects.
[0071] Compared with the prior art, the present invention has the following beneficial effects:
[0072] (1) By introducing modified graphene oxide into PA66 resin, this invention can solve the problems of easy agglomeration of graphene oxide, insufficient interfacial bonding with PA66 and excessive hydrophilic oxygen groups. The resulting carbon nanomaterials enhance PA66, which has excellent processability and toughness, while significantly improving its strength, rigidity, water resistance and performance retention after humid heat aging.
[0073] (2) The carbon nanomaterial-reinforced PA66 provided by this invention has a tensile strength ≥81.5 MPa, a tensile modulus ≥2.74 GPa, an elongation at break ≥25%; a flexural strength ≥79.3 MPa, a flexural modulus ≥2.04 GPa; and a notched impact strength ≥8.0 kJ·m. -2 Water absorption rate ≤1.06% after 24 h; bending strength retention rate after soaking in pesticide solution ≥92%, bending strength retention rate after soaking in fertilizer solution ≥89.6%, bending strength retention rate after wet heat aging ≥87.8%. Attached Figure Description
[0074] Figure 1 SEM image of the graphene oxide obtained in Example 1 Figure 1 (20 nm scale bar);
[0075] Figure 2 SEM image of the graphene oxide obtained in Example 1 Figure 2 (100 nm scale bar);
[0076] Figure 3 FTIR spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Preparation Example 1;
[0077] Figure 4 XPS full spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Preparation Example 1;
[0078] Figure 5 N1s high-resolution spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Preparation Example 1. Detailed Implementation
[0079] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0080] Unless otherwise specified, the raw materials involved in the following specific embodiments of the present invention are all conventional materials in the art, and can be purchased from commercially available products. Some raw material information is as follows:
[0081] PA66: Purchased from Pingdingshan Shenma Engineering Plastics Co., Ltd., model: EPR27;
[0082] Graphite powder: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., item number: G123645;
[0083] 11-Aminoundecanoic acid: purchased from Shanghai Maclean Biochemical Technology Co., Ltd., product number: A800368;
[0084] 12-Aminododecanoic acid: purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd., item number: A0932;
[0085] 8-Aminooctanoic acid: purchased from Sigma-Aldrich, product number: 855294;
[0086] EDC·HCL: Purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., item number: E106172;
[0087] NHS: Purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., item number: H109330;
[0088] KH550 coupling agent: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: A107147;
[0089] Antioxidant 1098: Purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd., item number: H1704;
[0090] Lubricating processing aid: Ethylene bis-stearamide, abbreviated as EBS, purchased from Shanghai Maclean Biochemical Technology Co., Ltd., item number: N829520;
[0091] Graphene oxide (commercially available): Purchased from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., product name: single-layer graphene oxide powder, sheet diameter 0.5-5 μm, thickness 0.8-1.2 nm;
[0092] Concentrated sulfuric acid, potassium permanganate, hydrogen peroxide solution, hydrochloric acid, and anhydrous ethanol were all purchased from Sinopharm Chemical Reagent Co., Ltd.
[0093] Preparation Example 1
[0094] This preparation example provides a method for preparing graphene oxide, as follows:
[0095] (1) Raw material pretreatment: Graphite powder is dried at 70℃ for 10 h and then used for later use;
[0096] (2) Oxidation reaction: Under ice bath, the dried graphite powder was added to concentrated sulfuric acid and mixed. The mass ratio of graphite powder to concentrated sulfuric acid was 1:40. Then potassium permanganate was added. The mass ratio of graphite powder to potassium permanganate was 1:3. Potassium permanganate was added in batches. After the addition was complete, the temperature was raised to 40℃ and the reaction was continued for 4 hours to obtain the graphite oxide reaction solution.
[0097] (3) Termination of reaction: After the oxidation reaction is complete, the reaction system is slowly added to deionized water for dilution. The mass ratio of graphite powder to deionized water is 1:100. During the addition process, the system temperature is controlled not to exceed 30°C. Then, a 30% hydrogen peroxide solution is added. The mass ratio of graphite powder to hydrogen peroxide solution is 1:3.7 to terminate the reaction of the residual oxidant and obtain a crude graphite oxide product dispersion.
[0098] (4) Washing and purification: Centrifuge the crude product dispersion to remove the supernatant, and wash the resulting solid with dilute sulfuric acid solution and deionized water in sequence;
[0099] (5) Exfoliation treatment: The treated graphene oxide was redispersed in deionized water at a concentration of 1 mg / mL. The dispersion was ultrasonically exfoliated for 60 min to form a graphene oxide dispersion.
[0100] (6) Drying to prepare powder: The graphene oxide dispersion was freeze-dried to obtain the graphene oxide.
[0101] Structural characterization:
[0102] (1) Microstructure characterization: SEM characterization of graphene oxide was performed, and the results are as follows:
[0103] Figure 1 SEM of graphene oxide Figure 1 (20 nm scale bar) Figure 2 SEM of graphene oxide Figure 2 (100 nm scale); At the 20 nm scale, curling, wrinkling and local folding can be observed at the edges of graphene oxide sheets, and there is some overlap between the sheets; At 100 nm, the graphene oxide as a whole is observed to be distributed as irregular nanosheets with some differences in sheet size and some overlapping areas, but the overall structure still shows a relatively thin sheet structure.
[0104] Preparation Example 2
[0105] This preparation example provides a modified graphene oxide-1 and its preparation method, as follows:
[0106] S1. Weigh 1.0 g of graphene oxide (provided in Preparation Example 1), add it to 1000 mL of 0.1 mol / L MES buffer (pH 5.5), and sonicate for 45 min to obtain a uniform graphene oxide dispersion with a concentration of 1.0 mg / mL.
[0107] S2. Under continuous stirring, 3.0 g EDC and 2.0 g NHS were added sequentially, and the mixture was activated at 25 °C for 60 min to obtain the intermediate.
[0108] S3. 3.0 g of 11-aminoundecanoic acid was added to 150 mL of deionized water, stirred continuously at 50 °C, and the pH was slowly adjusted to about 8.5 with 0.5 mol / L NaOH solution to obtain the modifier solution;
[0109] The modifier solution was slowly added to the activated graphene oxide dispersion over 30 min. After the addition was completed, the pH of the reaction system was adjusted to 7.5, and the reaction was continuously stirred at 50 °C for 12 h.
[0110] S4. After the reaction was completed, the solid product was collected by filtration. It was first washed thoroughly with deionized water three times, then washed with ethanol twice, and finally washed with deionized water until the last washing solution was close to neutral. The obtained solid was dried under vacuum at 60°C for 12 h to constant weight to obtain modified graphene oxide-1.
[0111] Structural characterization: Structural characterization of modified graphene oxide
[0112] To verify whether 11-aminoundecanoic acid was successfully grafted onto the surface of graphene oxide, the self-made graphene oxide obtained in Preparation Example 1 and the modified graphene oxide-1 were used as test samples for Fourier transform infrared spectroscopy (FTIR) and X-ray photoelectron spectroscopy (XPS). The FTIR measurement range was 4000–500 cm⁻¹. -1 XPS testing included full-spectrum scanning and N1s high-resolution scanning, with charge correction performed using the C1s binding energy of 284.8 eV. The results are as follows:
[0113] Figure 3 The FTIR spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Example 1 are shown in the figure. As can be seen from the figure, modified graphene oxide-1 has a peak density of approximately 2922 cm⁻¹. -1 and 2852 cm -1The presence of both asymmetric and symmetric stretching vibration peaks of methylene-CH2- at approximately 1640 cm⁻¹ indicates the introduction of long-chain aliphatic structures onto the graphene oxide surface; these peaks are observed at approximately 1640 cm⁻¹. -1 The absorption band is significantly enhanced at approximately 1545 cm⁻¹. -1 Shoulder peaks appear nearby, which can be attributed to amide I and amide II bands, respectively. Furthermore, modified graphene oxide-1 shows a peak at approximately 1720 cm⁻¹. -1 The absorption signal of the carboxyl group C=O can still be observed nearby, indicating that the carboxyl structure still exists in the modified material. Combined with the newly emerging long-chain methylene and amide bond related absorption signals, this result is consistent with the structural feature that the terminal carboxyl group is retained after grafting with 11-aminoundecanoic acid.
[0114] Figure 4 XPS full spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Example 1 are shown in the figure. As can be seen from the figure, graphene oxide mainly exhibits C1s and O1s signals, while modified graphene oxide-1, in addition to C1s and O1s signals, shows an N1s signal at about 400.1 eV, indicating that nitrogen-containing groups were introduced on the surface of the modified graphene oxide.
[0115] Figure 5 The N1s high-resolution spectra of graphene oxide (GO) and modified graphene oxide-1 (mGO-1) provided in Example 1 were obtained by peak fitting. The major peak at approximately 400.1 eV was attributed to -NC=O- in the amide structure, and the minor peak at approximately 399.2 eV was attributed to CN and / or a small amount of unreacted amino groups. The amide nitrogen peak was the main component in the N1s spectrum. Combined with the absorption signals related to long-chain methylene groups and amide bonds in the FTIR spectrum, this indicates that the carboxyl groups on the surface of graphene oxide underwent an amidation reaction with the amino group of 11-aminoundecanoic acid.
[0116] Therefore, by Figure 3-5 It can be seen that 11-aminoundecanoic acid is grafted onto the surface of graphene oxide via amide bonds to obtain 11-aminoundecanoic acid grafted and modified graphene oxide.
[0117] Preparation Example 3
[0118] This preparation example provides a modified graphene oxide-2 and its preparation method.
[0119] The difference from Preparation Example 2 is that, in this Preparation Example, 11-aminoundecanoic acid is replaced with an equal mass of 12-aminododecanoic acid.
[0120] Preparation Examples 4-5
[0121] This preparation example provides a modified graphene oxide and its preparation method.
[0122] The difference from Preparation Example 2 is that in this preparation example, the mass ratio of graphene oxide to 11-aminoundecanoic acid is 1:1 (modified graphene oxide-3, Preparation Example 4) and 1:5 (modified graphene oxide-4, Preparation Example 5).
[0123] Preparation Example 6
[0124] This preparation example provides a modified graphene oxide-5 and its preparation method.
[0125] The difference from Preparation Example 2 is that in this preparation example, graphene oxide is replaced with commercially available graphene oxide.
[0126] Comparative Preparation Example 1
[0127] This preparation example provides a modified graphene oxide-6 and its preparation method.
[0128] The difference from Preparation Example 2 is that, in this preparation example, 11-aminoundecanoic acid is replaced with an equal mass of 8-aminooctanoic acid.
[0129] Comparative Preparation Example 2
[0130] This preparation example provides a modified graphene oxide-7 and its preparation method.
[0131] The difference from Preparation Example 2 is that, in this preparation example, 11-aminoundecanoic acid was replaced with an equal mass of KH550 coupling agent.
[0132] Examples 1-8
[0133] Examples 1-8 provide a carbon nanomaterial-reinforced PA66, and the components and their amounts are shown in Table 1:
[0134] Table 1
[0135]
[0136] Table 2
[0137]
[0138] The preparation method is as follows:
[0139] PA66 resin was dried at 100℃ for 6 h, and modified graphene oxide was dried at 70℃ for 10 h.
[0140] The dried PA66, modified graphene oxide, antioxidant 1098 and EBS, and optionally a modifier (if any), are mixed evenly in the above proportions and then fed into a twin-screw extruder for melt blending. The extrusion temperature is controlled at 270°C and the screw speed is 220 r / min. The extrudate is cooled, pelletized and dried to obtain the carbon nanomaterial-reinforced PA66.
[0141] After drying, it can be injection molded to obtain the required sample size at an injection temperature of 275℃.
[0142] Performance testing
[0143] The performance of the samples provided in the examples and comparative examples was tested using the following methods:
[0144] (1) Tensile properties: The test was conducted in accordance with GB / T 1040.2-2022. A type 1A standard dumbbell specimen was used. The specimen thickness was 4.0 mm, the width of the narrow parallel section was 10 mm, and the gauge length was 75 mm. The tensile strength test rate was 50 mm / min, and the tensile modulus test rate was 1 mm / min.
[0145] (2) Bending performance: The test was conducted in accordance with GB / T 9341-2008. The sample size was 80 mm × 10 mm × 4 mm, the support span was 64 mm, and the test rate was 2 mm / min.
[0146] (3) 24 h water absorption rate: Refer to Method 1 of GB / T 1034-2008. The sample size is 60 mm × 60 mm × 1.0 mm. After drying the sample at 50℃ for 24 h to constant weight, it is soaked in distilled water at 23±1℃ for 24 h. After taking it out and wiping off the surface moisture, it is weighed and the water absorption rate is calculated.
[0147] (4) Bending strength retention rate after soaking in agricultural media: The pesticide medium was a commercially available glyphosate isopropylamine salt solution with a mass fraction of 41%, which was diluted with deionized water to a mass fraction of 1.0% for glyphosate isopropylamine salt; the fertilizer medium was a commercially available compound fertilizer with an N-P2O5-K2O mass ratio of 15-15-15, which was prepared with deionized water to a mass fraction of 5.0%; the samples were soaked in the above media at 40±2℃ for 168 h, and after being taken out, they were rinsed with deionized water and dried. The bending strength was tested according to GB / T9341-2008, and the bending strength retention rate was calculated.
[0148] (5) Bending strength retention rate after damp heat aging: The damp heat treatment was carried out in accordance with GB / T 2423.3-2016, and the treatment was carried out at 40±2℃ and 93±3%RH for 96 h; after returning to room temperature, the bending strength was tested according to GB / T 9341-2008, and the bending strength retention rate was calculated.
[0149] The test results are as follows:
[0150] Table 3
[0151]
[0152] As can be seen from the examples and performance tests, the carbon nanomaterial-reinforced PA66 provided by the present invention has excellent processability and toughness, while its strength, rigidity, water resistance and performance retention after humid heat aging are significantly improved.
[0153] As can be seen from the comparison of Examples 2, 5-8 and Comparative Examples 1-2, compared with the treatment using conventional coupling agents or the treatment using modifiers not limited to the scope of this invention, this invention can improve the interfacial compatibility between graphene oxide and PA66 by introducing C10-C15 aliphatic alkyl chains with carboxyl groups at the end, reduce the re-agglomeration of sheets during drying and melt processing, and significantly improve the overall performance of PA66.
[0154] As can be seen from the comparison between Example 2 and Comparative Example 5, compared with the direct blending modification of modifier and graphene oxide, the present invention can significantly improve the overall performance of PA66 by introducing modified graphene oxide.
[0155] The present invention has been illustrated through the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A carbon nanomaterial-reinforced PA66, characterized in that, By weight, it comprises 98-100 parts PA66 resin, 0.3-1 parts modified graphene oxide, and 0.4-1.5 parts processing aids, wherein: The modified graphene oxide surface is grafted with C10-C15 aliphatic alkyl chains with carboxyl groups at the ends.
2. The carbon nanomaterial-reinforced PA66 according to claim 1, characterized in that, The method for preparing the modified graphene oxide includes: Graphene oxide is activated and then subjected to an amidation reaction with a C10-C15 aliphatic alkyl modifier with a carboxyl group at the end to obtain the modified graphene oxide, wherein the modifier contains an amino group.
3. The carbon nanomaterial-reinforced PA66 according to claim 2, characterized in that, The mass ratio of the modifier to graphene oxide is (1-5):1; And / or, the amidation reaction is carried out at a temperature of 40-60°C for a time of 6-24 h.
4. The carbon nanomaterial-reinforced PA66 according to claim 2 or 3, characterized in that, The modifier is 11-aminoundecanoic acid and / or 12-aminododecanoic acid.
5. The carbon nanomaterial-reinforced PA66 according to any one of claims 1-4, characterized in that, The method for preparing the graphene oxide includes sequentially oxidizing, peeling, washing, drying and grinding the raw materials. Preferably, the raw material includes any one or a combination of at least two of natural flake graphite, graphite powder, or expanded graphite.
6. The carbon nanomaterial-reinforced PA66 according to any one of claims 1-5, characterized in that, The relative viscosity of the PA66 resin is 2.5-3.0, preferably 2.62-2.
72.
7. The carbon nanomaterial-reinforced PA66 according to any one of claims 1-6, characterized in that, The processing aids include any one or a combination of at least two of antioxidants, lubricants, or weather-resistant agents; Preferably, it includes 0.2-0.5 parts by weight of antioxidant; Preferably, the mixture comprises 0.2-0.8 parts by weight of lubricant; Preferably, the mixture includes 0.2-0.5 parts by weight of weathering agent.
8. The carbon nanomaterial-reinforced PA66 according to claim 7, characterized in that, The antioxidant includes any one or a combination of at least two of antioxidants 1098, 1010, 1076, or 168. And / or, the lubricant comprises any one or a combination of at least two of ethylene bis-stearamide, calcium stearate, zinc stearate, or polyethylene wax.
9. A method for preparing carbon nanomaterial-reinforced PA66 as described in any one of claims 1-8, characterized in that, The preparation method includes: The components in the formula are mixed, melt-extruded, cooled and granulated to obtain the carbon nanomaterial-reinforced PA66.
10. An application of carbon nanomaterial-reinforced PA66 as described in any one of claims 1-8 in the arm of an agricultural drone; Preferably, the arm of the agricultural drone is obtained by injection molding of the carbon nanomaterial-reinforced PA66.