A thermally conductive gel, its preparation method and application
By using single-crystal diamond with specific sphericity and particle size and a silicon-oxygen chain structure powder treatment agent, the problem of high interface thickness of thermal conductive gel was solved, and a thermal conductive gel with high thermal conductivity and low interface thickness was achieved, which is suitable for the heat dissipation needs of electronic components.
Patent Information
- Application Number
- CN202611526009.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing thermal conductive gels have a high interface thickness with a thermal conductivity of up to 20 W/mk, which makes it difficult to meet the heat dissipation requirements of electronic components, especially as they exert a large compressive stress on the silicon substrate.
Using a powder treatment agent with a silicon-oxygen chain structure and single-crystal diamond with specific sphericity and particle size as thermally conductive powder, combined with vinyl silicone oil, hydrogen-containing silicone oil and a single-component platinum catalyst, a high-thermal-network structure is constructed by controlling the ratio of large and small-sized diamond particles, which disperses vertical pressure and reduces interface thickness.
While achieving a thermal conductivity of over 20 W/mk, the interface thickness was reduced to below 200 μm, avoiding localized stress concentration on electronic components and improving heat dissipation efficiency and service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of thermally conductive gels, specifically relating to a thermally conductive gel, its preparation method, and its application. Background Technology
[0002] With the development of electronic technology, the size requirements of electronic components are becoming smaller and smaller, trending towards high integration and high assembly density. This leads to increasingly higher heat flux density, making it difficult to dissipate heat quickly and effectively, which seriously affects the performance and lifespan of electronic components. Thermal conductive gel, as a paste-like thermally conductive interface material that can be dispensed and has extremely low thermal resistance, is widely used in heat dissipation devices.
[0003] The rapid development of AI and other businesses is driving an increasing demand for high-speed data transmission, with 400G, 800G, and even 1.6T optical modules rapidly iterating and evolving. High-speed data transmission generates more heat, resulting in a high heat flux density per unit area, thus requiring higher heat dissipation efficiency. The market demands thermal interface materials with very high thermal conductivity; currently, a thermal conductivity of 20W / mK is required to meet heat dissipation needs. The thermally conductive powder used in 20W thermal conductive gels is typically diamond, which has a very high intrinsic thermal conductivity, reaching 2000~2200W / mK. However, due to its hardness, diamond causes significant compressive stress during application, which can damage the silicon substrate and affect its use. This necessitates that diamond thermal conductive materials maintain a low bond line thickness (BLT) to ensure low compressive stress. However, currently, the BLT of 20W thermal conductive gels developed using diamond fillers on the market is generally above 220μm, which is insufficient to meet the application requirements. Summary of the Invention
[0004] The primary objective of this invention is to overcome the shortcomings of existing thermally conductive gels, which have a high interface thickness despite having a thermal conductivity of 20 W / mk, and to provide a thermally conductive gel with a thermal conductivity of 20 W / mk and a low interface thickness.
[0005] A second objective of this invention is to provide a method for preparing the above-mentioned thermally conductive gel.
[0006] A third objective of this invention is to provide the application of the above-mentioned thermally conductive gel in electronic components.
[0007] The thermally conductive gel provided by this invention contains vinyl silicone oil, hydrogen-containing silicone oil, a single-component platinum catalyst, a powder treatment agent, and thermally conductive powder. The powder treatment agent has a silicon-oxygen chain main chain and single-ended alkoxy end caps. The thermally conductive powder contains more than 50 wt% of diamond, which is a single-crystal diamond with a sphericity of 0.7 or higher. The diamond contains large-diameter diamond and small-diameter diamond in a mass ratio of 1:(0.1~0.7). The large-diameter diamond has a particle size D90 of 100 μm to 150 μm, and the small-diameter diamond has a particle size D90 of 40 μm to 95 μm.
[0008] The key to the thermally conductive gel provided by this invention lies in the use of a powder treatment agent with a silicon-oxygen chain structure main chain and single-ended alkoxy end caps, and the use of single-crystal diamond with specific sphericity and particle size as the thermally conductive powder. This not only effectively constructs a high thermal network structure, achieving a thermal conductivity of over 20 W / mk, but also ensures that when the thermally conductive gel is compressed, the vertical pressure can be effectively dispersed in all directions, avoiding local stress concentration and damage to electronic components, and achieving an interface thickness of less than 200 μm. The reasons for this are speculated to be as follows: Firstly, large-diameter diamonds have excellent interlocking properties. Controlling the content of interlocking diamonds to above 50wt% can reduce compressive stress during use, allowing them to fill thinner gaps and thus significantly reducing the interfacial thickness of the thermally conductive gel. Secondly, controlling the sphericity of the interlocking diamonds to above 0.7 can reduce viscosity and increase extrusion rate, thus achieving a low interfacial thickness under minimal pressure. Thirdly, small-diameter diamonds filling the gaps between large-diameter diamonds result in a denser filling within the same volume. If the proportion of small-diameter diamonds is too high, it will stretch the large-diameter diamonds, disrupting the thermal conductivity pathway and reducing the thermal conductivity and extrusion rate. Conversely, if the proportion of small-diameter diamonds is too low, the gaps between the large-diameter diamonds cannot be completely filled, reducing the thermal conductivity. Therefore, a combination of large-diameter diamonds (D90 100μm~150μm) and small-diameter diamonds (D90...) is ideal. The mass ratio of 40μm to 95μm is controlled at 1:(0.1 to 0.7), which can both fill the gaps between the main heat conduction channels to improve the thermal conductivity and avoid the destruction of the heat conduction channels, thus improving the thermal conductivity performance. Detailed Implementation
[0009] The thermally conductive gel provided by this invention contains vinyl silicone oil, hydrogen-containing silicone oil, a single-component platinum catalyst, a powder treatment agent, and thermally conductive powder. The preferred mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:(0.01~1), such as 1:0.01, 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, or any value between them. The preferred mass ratio of the vinyl silicone oil to the single-component platinum catalyst is 1:(0.0001~0.01), such as 1:0.0001, 1:0.0005, 1:0.0008, 1:0.001, 1:0.005, 1:0.008, 1:0.01, or any value between them. The preferred mass ratio of the powder treatment agent to the thermally conductive powder is 1:(20~650), such as 1:20, 1:50, 1:80, 1:100, 1:120, 1:150, 1:180, 1:200, 1:220, 1:250, 1:280, 1:300, 1:320, 1:350, 1:380, 1:400, 1:420, 1:450, 1:480, 1:500, 1:520, 1:550, 1:580, 1:600 or any value between them. The ratio of the content of the powder treatment agent to the total content of vinyl silicone oil, hydrogen-containing silicone oil, single-component platinum catalyst and thermally conductive powder is preferably 1:(30~500), such as 1:30, 1:50, 1:80, 1:100, 1:120, 1:150, 1:180, 1:200, 1:250, 1:300, 1:350, 1:400, 1:450, 1:500 or any value between them.
[0010] In the aforementioned thermally conductive gel, the powder treatment agent has a siloxane chain backbone and single-ended alkoxy groups. The number-average molecular weight of the powder treatment agent is preferably 1000-20000. At this value, the powder treatment agent can uniformly and effectively coat the surface of the thermally conductive powder, and the viscosity is suitable, with a coating thickness that is not too thick, further improving the thermal conductivity. Specifically, the number-average molecular weight of the powder treatment agent can be 1000, 2000, 5000, 8000, 10000, 12000, 14000, 16000, 18000, 20000, or any value between them. The number of carbon atoms in the alkoxy groups of the powder treatment agent is preferably 1-10. This avoids both the defect of insufficient modified powder after alkoxy hydrolysis due to too few carbon atoms and the defect of poor compatibility with vinyl silicone oil and hydrogen-containing silicone oil due to too many carbon atoms. The number of alkoxy carbon atoms in the powder treatment agent can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or any value between them.
[0011] In the aforementioned thermally conductive gel, the vinyl silicone oil can be selected from at least one of double-ended vinyl silicone oil, single-ended vinyl silicone oil, side-ended vinyl silicone oil, and end-side vinyl silicone oil. Specifically, double-ended vinyl silicone oil refers to silicone oil with vinyl groups at both ends. Single-ended vinyl silicone oil refers to silicone oil with vinyl groups at only one end. Side-ended vinyl silicone oil refers to silicone oil with vinyl groups on its side chains. End-side vinyl silicone oil refers to silicone oil with vinyl groups at both the end and the side chains. The viscosity of the vinyl silicone oil at 25°C is preferably 10 cps to 200 cps, more preferably 15 to 100 cps, such as 15 cps, 20 cps, 25 cps, 30 cps, 35 cps, 40 cps, 45 cps, 50 cps, 60 cps, 70 cps, 80 cps, 90 cps, 100 cps, or any value between these values. The vinyl content in the vinyl silicone oil is preferably 0.05% to 3%, such as 0.05%, 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, or any value between them.
[0012] In the aforementioned thermally conductive gel, the hydrogen-containing silicone oil can be selected from at least one of double-ended hydrogen-containing silicone oil, single-ended hydrogen-containing silicone oil, side-ended hydrogen-containing silicone oil, and end-side hydrogen-containing silicone oil. Specifically, the double-ended hydrogen-containing silicone oil refers to a silicone oil with active hydrogen at both ends. The single-ended hydrogen-containing silicone oil refers to a silicone oil with active hydrogen at only one end. The side-ended hydrogen-containing silicone oil refers to a silicone oil with active hydrogen in its side chains. The end-side hydrogen-containing silicone oil refers to a silicone oil with active hydrogen in both its end and side chains. The hydrogen content in the hydrogen-containing silicone oil is preferably 0.05% to 1.5%, such as 0.05%, 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, or any value between these values.
[0013] In the above-mentioned thermally conductive gel, the single-component platinum catalyst is preferably a phase change wax-coated platinum catalyst. The content of platinum catalyst in the phase change wax-coated platinum catalyst is preferably 1000ppm to 10000ppm, more preferably 2000ppm to 6000ppm, such as 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, or any value between these values.
[0014] In the aforementioned thermally conductive gel, the thermally conductive powder contains at least 50 wt% of diamond. If the diamond content in the thermally conductive powder is less than 50 wt%, the interface thickness of the thermally conductive gel will be significantly increased, and the interface thickness cannot be reduced below 200 μm. Specifically, the diamond content in the thermally conductive powder is at least 50 wt%, specifically 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, 100 wt%, or any value between these values. In a preferred embodiment, the thermally conductive powder contains 50 wt% to 100 wt% of diamond and 0 wt% to 50 wt% of other thermally conductive powders. The content of the other thermally conductive powders can be 0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, or any value between these values. Other thermally conductive powders may include at least one of alumina, zinc oxide, aluminum nitride, boron nitride, carbon fiber, silicon carbide, graphene, aluminum powder, and silver powder. In a preferred embodiment, the thermally conductive powder is composed of diamond, aluminum nitride, alumina, and zinc oxide. Although diamond has good thermal conductivity, it suffers from oil separation. The use of aluminum nitride not only compensates for the oil separation problem of diamond but also fills the gap in the inability of diamond to synthesize small-particle-size particles. The high sphericity of alumina and the lubricating effect of zinc oxide can reduce the viscosity of the thermally conductive gel and improve its fluidity. Therefore, this specific combination can further improve the thermal conductivity of the thermally conductive gel and further reduce the interface thickness. The preferred mass ratio of diamond, aluminum nitride, alumina, and zinc oxide in the thermally conductive powder is 1:(0.2~0.8):(0.1~0.5):(0.05~0.4), more preferably 1:(0.3~0.6):(0.2~0.4):(0.1~0.3). Controlling the mass ratio of diamond, aluminum nitride, aluminum oxide, and zinc oxide in the thermally conductive powder within the aforementioned preferred range can improve the filling density, establish multiple thermal conduction pathways, and further enhance the thermal conductivity. Specifically, the preferred mass ratio of diamond to aluminum nitride is 1:(0.2~0.8), more preferably 1:(0.3~0.6), such as 1:0.3, 1:0.32, 1:0.35, 1:0.38, 1:0.4, 1:0.42, 1:0.45, 1:0.48, 1:0.5, 1:0.52, 1:0.55, 1:0.58, 1:0.6, or any value between them.The preferred mass ratio of the diamond to alumina is 1:(0.1~0.5), more preferably 1:(0.2~0.4), such as 1:0.2, 1:0.22, 1:0.24, 1:0.26, 1:0.28, 1:0.3, 1:0.32, 1:0.34, 1:0.36, 1:0.38, 1:0.4, or any value between them. The preferred mass ratio of the diamond to zinc oxide is 1:(0.05~0.4), more preferably 1:(0.1~0.3), such as 1:0.1, 1:0.12, 1:0.15, 1:0.18, 1:0.2, 1:0.22, 1:0.25, 1:0.28, 1:0.3, or any value between them. The particle size D90 of the aluminum nitride is preferably 0.5 μm to 50 μm, such as 0.5 μm, 1 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, or any value between them. The particle size D90 of the alumina is preferably 0.2 μm to 10 μm, such as 0.2 μm, 0.5 μm, 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, or any value between them. The particle size D90 of the zinc oxide is preferably 0.1 μm to 1 μm, such as 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, or any value between them. The sphericity of the diamond used for breaking is 0.7 or higher, such as 0.7, 0.72, 0.74, 0.76, 0.78, 0.8, 0.82, 0.84, 0.86, 0.88, 0.9, 0.92, 0.94, 0.96, 0.98, 1, or any value between them. If the sphericity of the diamond is lower than 0.7, it cannot roll well, which will increase the viscosity and extrusion rate of the thermally conductive gel and increase the interface thickness. In this invention, the sphericity is determined by optical microscopy. The particle size D90 of the diamond used for breaking is 40μm to 150μm, such as 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 120μm, 140μm, 150μm, or any value between them. If the particle size of the diamond is less than 40μm, the thermal conductivity is too low; if the particle size is greater than 150μm, the particle size exceeds the interface thickness requirement, and the powder needs to be broken to achieve the interface thickness, which is not conducive to reducing the interface thickness and increases the compressive stress.
[0015] In a preferred embodiment, the diamond core contains both large-diameter and small-diameter diamonds. This has the advantage of improving the overall thermal conductivity because diamond has a very high intrinsic thermal conductivity, so more of it is needed. However, using too much diamond can lead to oil separation problems. The particle size D90 of the large-diameter diamonds is preferably 100μm to 150μm, such as 100μm, 105μm, 110μm, 115μm, 120μm, 125μm, 130μm, 135μm, 140μm, 145μm, 150μm, or any value between them. The particle size D90 of the small-diameter diamonds is preferably 40μm to 95μm, such as 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, or any value between them. The preferred mass ratio of large-diameter diamonds to small-diameter diamonds is 1:(0.1~0.7), such as 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, or any value between them. Using a specific ratio of large and small diameter diamonds, with the small-diameter diamonds filling the gaps between the large-diameter diamonds, results in a denser filling within the same volume. If the proportion of small-diameter diamonds is too high, it will stretch the large-diameter diamonds, disrupting the heat conduction pathway and reducing the thermal conductivity and extrusion rate. Conversely, if the proportion of small-diameter diamonds is too low, the gaps between the large-diameter diamonds cannot be completely filled, further reducing the thermal conductivity.
[0016] The method for preparing the thermally conductive gel provided by this invention includes uniformly mixing vinyl silicone oil, hydrogen-containing silicone oil, a single-component platinum catalyst, a powder treatment agent, and thermally conductive powder. The mixing method is not particularly limited, but preferably, the uniform mixing method includes pre-mixing the vinyl silicone oil, hydrogen-containing silicone oil, powder treatment agent, and thermally conductive powder, and then deeply mixing the resulting semi-finished product with the single-component platinum catalyst. Preferably, the pre-mixing method includes stirring for 60s to 180s at a stirring speed of 1000rpm to 2000rpm and a pressure below -0.1MPa, followed by placing the resulting mixture at 40℃ to 120℃ for 2h to 24h, and then cooling to room temperature. In the premixing stage, the stirring speed can be 1000 rpm, 1200 rpm, 1400 rpm, 1600 rpm, 1800 rpm, 2000 rpm, or any value between them; the pressure can be -0.1 MPa, -0.12 MPa, -0.15 MPa, -0.18 MPa, -0.2 MPa, -0.22 MPa, -0.25 MPa, -0.28 MPa, -0.3 MPa, or other pressures. The stirring time can be any value between these values; the stirring time can be 60s, 80s, 100s, 120s, 140s, 160s, 180s, or any value between them; the placement temperature can be 40℃, 60℃, 80℃, 100℃, 120℃, or any value between them; the placement time can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, or any value between them. The preferred conditions for deep mixing include a stirring speed of 600rpm~1500rpm, a pressure below -0.1MPa, and a stirring time of 60s~300s. During the deep mixing stage, the stirring speed can be 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, 1500 rpm, or any value between them; the pressure can be -0.1 MPa, -0.12 MPa, -0.15 MPa, -0.18 MPa, -0.2 MPa, -0.22 MPa, -0.25 MPa, -0.28 MPa, -0.3 MPa, or any value between them; the stirring time can be 60 s, 80 s, 100 s, 120 s, 150 s, 180 s, 200 s, 220 s, 250 s, 280 s, 300 s, or any value between them.
[0017] The present invention also provides the application of the thermally conductive gel in electronic components.
[0018] In the following examples and comparative examples, the parts of each raw material refer to parts by weight.
[0019] Example 1 This embodiment illustrates the thermally conductive gel and its preparation method provided by the present invention.
[0020] 0.2 parts of siloxane-containing silicone oil treatment agent (manufacturer: JNC Japan, FM-0815J, number average molecular weight: 3000, molecular formula: (CH3O)3Si-O-[Si(CH3)2-O]). n -Si(CH3)2-C4H9), 14 parts vinyl silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-Vi321, viscosity at 25℃: 110cps, vinyl content: 1.06%), 1 part hydrogen-containing silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-H3, hydrogen content: 0.3%), 40 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade LD340 110 / 120, particle size D90: 120μm, sphericity: 0.75), 20 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade LD340). 30 / 40 parts (particle size D90: 40 μm, sphericity: 0.75), 30 parts aluminum nitride (manufacturer: Ya'an Baitu High-Tech Materials Co., Ltd., grade TAF20, particle size D50: 20 μm), 15 parts single-crystal alumina (manufacturer: Sumitomo Chemical Co., Ltd., Japan, grade AA-1.5, particle size D50: 1.5 μm), and 10 parts zinc oxide (manufacturer: Zochem Inc., grade Zoco103, particle size D50: 0.2 μm) were evenly distributed. The mixture was mixed in a high-performance liquid mixer at a stirring speed of 1600 rpm, a pressure of -0.1 MPa, and a stirring time of 90 s. The mixture was then placed in a 60℃ constant temperature oven and kept at that temperature for 6 hours. After cooling to room temperature, a semi-finished product was obtained. 0.008 parts of a single-component platinum catalyst (Guangzhou Tianjiang High-Tech Materials Co., Ltd., grade TP-J-2500) were added, and the mixture was stirred for another 90 s at a stirring speed of 900 rpm and a pressure of -0.1 MPa to obtain a thermally conductive gel, denoted as DSi-1.
[0021] Example 2 This embodiment illustrates the thermally conductive gel and its preparation method provided by the present invention.
[0022] 0.2 parts of siloxane-containing silicone oil treatment agent (manufacturer: JNC Japan, FM-0815J, number average molecular weight: 3000, molecular formula: (CH3O)3Si-O-[Si(CH3)2-O]). n-Si(CH3)2-C4H9), 12 parts vinyl silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-Vi321, viscosity at 25℃: 110cps, vinyl content: 1.06%), 2 parts hydrogen-containing silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-H3, hydrogen content: 0.3%), 44 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade RVD 110 / 120, particle size D90: 120μm, sphericity: 0.80), 21 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade RVD...). 30 / 40 parts (particle size D90 of 40 μm, sphericity of 0.80), 32 parts aluminum nitride (manufacturer: Ya'an Baitu High-tech Materials Co., Ltd., grade TAF20, particle size D50 of 20 μm), 16 parts 1.5 μm single crystal alumina (manufacturer: Sumitomo Chemical Co., Ltd., Japan, grade AA-1.5), and 12 parts zinc oxide (manufacturer: Zochem Inc., USA, grade Zoco103, particle size D50 of 0.2 μm) were placed in a homogenizer. Mix the ingredients, stirring at 1600 rpm, pressure at -0.1 MPa, and stirring for 90 seconds. Place the mixture in a 60℃ constant temperature oven and keep it at that temperature for 6 hours. After cooling to room temperature, a semi-finished product is obtained. Add 0.008 parts of a single-component platinum catalyst (Guangzhou Tianjiang High-Tech Materials Co., Ltd., grade TP-J-2500) and continue stirring at 900 rpm and pressure at -0.1 MPa for 90 seconds to obtain a thermally conductive gel, denoted as DSi-2.
[0023] Example 3 This embodiment illustrates the thermally conductive gel and its preparation method provided by the present invention.
[0024] 0.2 parts of siloxane-containing silicone oil treatment agent (manufacturer: JNC Japan, FM-0815J, number average molecular weight: 3000, molecular formula: (CH3O)3Si-O-[Si(CH3)2-O]). n-Si(CH3)2-C4H9), 8 parts vinyl silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-Vi321, viscosity at 25℃: 110cps, vinyl content: 1.06%), 1 part hydrogen-containing silicone oil (manufacturer: Zhejiang Runhe Organosilicon New Material Co., Ltd., grade RH-LHC-3, hydrogen content: 0.8%), 30 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade RVD 110 / 120, particle size D90: 120μm, sphericity: 0.85), 20 parts diamond (manufacturer: Henan Liliang Diamond Co., Ltd., grade RVD...). 30 / 40 parts (particle size D90 of 40 μm, sphericity of 0.75), 15 parts aluminum nitride (manufacturer: Ya'an Baitu High-tech Materials Co., Ltd., grade TAF20, particle size D50 of 20 μm), 10 parts 1.5 μm single crystal alumina (manufacturer: Sumitomo Chemical Co., Ltd., Japan, grade AA-1.5), and 5 parts zinc oxide (manufacturer: Zochem Inc., USA, grade Zoco103, particle size D50 of 0.2 μm) were placed in a homogenizer. Mix the ingredients, stirring at 1600 rpm, pressure at -0.1 MPa, and stirring for 90 seconds. Place the mixture in a 60℃ constant temperature oven and keep it at that temperature for 6 hours. After cooling to room temperature, a semi-finished product is obtained. Add 0.008 parts of a single-component platinum catalyst (Guangzhou Tianjiang High-Tech Materials Co., Ltd., grade TP-J-2500) and continue stirring at 900 rpm and pressure at -0.1 MPa for 90 seconds to obtain a thermally conductive gel, denoted as DSi-3.
[0025] Example 4 The thermally conductive gel was prepared according to the method of Example 1, except that the single-crystal alumina was replaced with the same amount of aluminum nitride by weight, and the other conditions were the same as in Example 1. The resulting thermally conductive gel was denoted as DSi-4.
[0026] Example 5 The thermally conductive gel was prepared according to the method of Example 1, except that zinc oxide was replaced with aluminum nitride in the same weight proportions, and the other conditions were the same as in Example 1. The resulting thermally conductive gel was denoted as DSi-5.
[0027] Example 6 The thermally conductive gel was prepared according to the method of Example 1, except that aluminum nitride, single-crystal alumina and zinc oxide were all replaced with diamond (manufacturer: Henan Power Diamond Co., Ltd., grade LD340 30 / 40, particle size D90 of 40 μm) in the same weight proportions. The other conditions were the same as in Example 1, and the resulting thermally conductive gel was designated DSi-7.
[0028] Example 7 The thermally conductive gel was prepared according to the method of Example 7, except that the diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 110 / 120, particle size D90 of 120 μm, sphericity of 0.75) was replaced with the same weight of diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 30 / 40, particle size D90 of 40 μm, sphericity of 0.65). The other conditions were the same as in Example 1, and the resulting thermally conductive gel was designated DSi-8.
[0029] Comparative Example 1 The thermally conductive gel was prepared according to the method in Example 1, except that the same weight parts of alkoxy-terminated polydimethylsiloxane (manufacturer: Yunnan Zhonghe Silicon-based New Materials Co., Ltd., brand name JZH-203B, number average molecular weight 2000, molecular formula: (CH3O)3Si-O-[Si(CH3)2-O) was used as the siloxane-containing silicone oil treatment agent. n The reference thermally conductive gel was obtained by substituting -Si(CH3)2-(OCH3)3 and using the same conditions as in Example 1, and denoted as DDSi-1.
[0030] Comparative Example 2 The thermally conductive gel was prepared according to the method of Example 1, except that the diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 110 / 120, particle size D90 of 120 μm, sphericity of 0.75) and diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 30 / 40, particle size D90 of 40 μm, sphericity of 0.75) were replaced with the same weight parts of diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD90, particle size D90 of 130 μm, sphericity of 0.5). The other conditions were the same as in Example 1, and a reference thermally conductive gel was obtained, denoted as DDSi-2.
[0031] Comparative Example 3 The thermally conductive gel was prepared according to the method of Example 1, except that the diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 110 / 120, particle size D90 of 120 μm, sphericity of 0.75) and diamond (manufacturer: Henan Lili Diamond Co., Ltd., grade LD340 30 / 40, particle size D90 of 40 μm, sphericity of 0.75) were replaced with the same weight parts of diamond (manufacturer: Henan Houde Diamond Technology Co., Ltd., grade HD9890 120 / 140, particle size D90 of 40 μm, sphericity of 0.80). The other conditions were the same as in Example 1, and a reference thermally conductive gel was obtained, denoted as DDSi-3.
[0032] Comparative Example 4 The thermally conductive gel was prepared according to the method of Example 1, except that the diamond (manufacturer: Henan Houde Diamond Technology Co., Ltd., grade LD340 110 / 120, particle size D90 of 120 μm, sphericity of 0.75) and diamond (manufacturer: Henan Houde Diamond Technology Co., Ltd., grade LD340 30 / 40, particle size D90 of 40 μm, sphericity of 0.75) were replaced with the same weight parts of diamond (manufacturer: Henan Houde Diamond Technology Co., Ltd., grade HD98960, particle size D90 of 300 μm, sphericity of 0.80). The other conditions were the same as in Example 1, and a reference thermally conductive gel was obtained, denoted as DDSi-4.
[0033] Test case (1) Interface thickness: The interface thickness of the thermally conductive gels obtained in the above embodiments and comparative examples was measured and calculated according to the method disclosed in ASTM D5470. Specifically, the total thermal resistance R of the thermally conductive gels obtained in the above embodiments and comparative examples with thicknesses of 1 mm, 2 mm and 3 mm were measured according to the method disclosed in ASTM D5470. total The testing instrument was purchased from Ruiling (model LW-9389). The testing pressure was 40 psi and the testing temperature was 80℃. A linear fit was performed with sample thickness as the x-axis and total thermal resistance as the y-axis. The slope of the fitted curve was 1 / k, where k is the thermal conductivity (W / (m·K)) and the intercept is the contact thermal resistance Rc (K·m² / W). According to the formula R... TIM =R total -R c Calculate the thermal resistance R of the thermally conductive gel layer TIM Then, according to BLT=k×R TIM The interface thickness (BLT) was calculated. The results are shown in Table 1.
[0034] (2) Thermal conductivity: The thermal conductivity of the thermally conductive gels obtained in the above examples and comparative examples was determined according to the method disclosed in ASTM D5470. The total thermal resistance R of the three samples with thicknesses of 1 mm, 2 mm and 3 mm was measured. total The testing instrument was purchased from Ruiling (model LW-9389). The test pressure was 40 psi and the test temperature was 80 ℃. A linear fit was performed with the sample thickness as the abscissa and the total thermal resistance as the ordinate. The slope of the fitted curve was 1 / k, where k is the thermal conductivity (W / (m·K)). The results are shown in Table 1.
[0035] (3) Initial viscosity: The viscosity of the thermally conductive gels obtained in the above examples and comparative examples was measured by a rotational viscometer (Brookfield DV2T) according to the rotational method disclosed in GB / T 2794-2022. The test temperature was 25℃, the rotation speed was 10rpm, and the rotor model was SC4-14. The results are shown in Table 1.
[0036] Table 1
[0037] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention.
Claims
1. A thermally conductive gel, characterized in that, The thermally conductive gel contains vinyl silicone oil, hydrogen-containing silicone oil, a single-component platinum catalyst, a powder treatment agent, and thermally conductive powder. The powder treatment agent has a silicon-oxygen chain main chain and single-ended alkoxy end caps. The thermally conductive powder contains more than 50 wt% of diamond, which is a single-crystal diamond with a sphericity of 0.7 or higher. The diamond contains large-diameter diamond and small-diameter diamond in a mass ratio of 1:(0.1~0.7). The large-diameter diamond has a particle size D90 of 100 μm to 150 μm, and the small-diameter diamond has a particle size D90 of 40 μm to 95 μm.
2. The thermally conductive gel according to claim 1, characterized in that, The thermally conductive gel satisfies at least one of the following conditions: (1) The mass ratio of the vinyl silicone oil to the hydrogen-containing silicone oil is 1:(0.01~1); (2) The mass ratio of the vinyl silicone oil to the single-component platinum catalyst is 1:(0.0001~0.01); (3) The mass ratio of the powder treatment agent to the thermally conductive powder is 1:(20~650); (4) The ratio of the content of the powder treatment agent to the total content of vinyl silicone oil, hydrogen-containing silicone oil, single-component platinum catalyst and thermally conductive powder is 1:(30~500).
3. The thermally conductive gel according to claim 1, characterized in that, The vinyl silicone oil is selected from at least one of double-ended vinyl silicone oil, single-ended vinyl silicone oil, side-ended vinyl silicone oil, and end-side vinyl silicone oil; Preferably, the viscosity of the vinyl silicone oil at 25°C is 10 cps to 200 cps; Preferably, the vinyl content in the vinyl silicone oil is 0.05% to 3%.
4. The thermally conductive gel according to claim 1, characterized in that, The hydrogen-containing silicone oil is selected from at least one of double-ended hydrogen-containing silicone oil, single-ended hydrogen-containing silicone oil, side-ended hydrogen-containing silicone oil, and end-side hydrogen-containing silicone oil. Preferably, the hydrogen content in the hydrogen-containing silicone oil is 0.05% to 1.5%.
5. The thermally conductive gel according to claim 1, characterized in that, The single-component platinum catalyst is a phase change wax-coated platinum catalyst. Preferably, the content of platinum catalyst in the phase change wax-coated platinum catalyst is 1000ppm~10000ppm.
6. The thermally conductive gel according to claim 1, characterized in that, The number average molecular weight of the powder treatment agent is 1000~20000; the number of carbon atoms of the alkoxy group in the powder treatment agent is 1~10.
7. The thermally conductive gel according to claim 1, characterized in that, The thermally conductive powder contains 50wt%~100wt% diamond and 0wt%~50wt% other thermally conductive powders. Preferably, the other thermally conductive powder is selected from at least one of alumina, zinc oxide, aluminum nitride, boron nitride, carbon fiber, silicon carbide, graphene, aluminum powder, and silver powder; Preferably, the thermally conductive powder is composed of diamond, aluminum nitride, aluminum oxide, and zinc oxide; Preferably, the mass ratio of diamond, aluminum nitride, aluminum oxide and zinc oxide in the thermally conductive powder is 1:(0.2~0.8):(0.1~0.5):(0.05~0.4), more preferably 1:(0.3~0.6):(0.2~0.4):(0.1~0.3); Preferably, the aluminum nitride has a particle size D90 of 0.5 μm to 50 μm; Preferably, the particle size D90 of the alumina is 0.2 μm to 10 μm; Preferably, the zinc oxide has a particle size D90 of 0.1 μm to 1 μm.
8. A method for preparing the thermally conductive gel according to any one of claims 1 to 7, characterized in that, The method involves uniformly mixing vinyl silicone oil, hydrogen-containing silicone oil, a single-component platinum catalyst, a powder treatment agent, and a thermally conductive powder.
9. The method for preparing the thermally conductive gel according to claim 8, characterized in that, The method for achieving uniform mixing includes premixing vinyl silicone oil, hydrogen-containing silicone oil, powder treatment agent and thermally conductive powder, and then deeply mixing the resulting semi-finished product with a single-component platinum catalyst. Preferably, the premixing method includes stirring for 60s to 180s at a stirring speed of 1000rpm to 2000rpm and a pressure below -0.1MPa, and then placing the resulting mixture at 40℃ to 120℃ for 2h to 24h before cooling to room temperature; Preferably, the conditions for deep mixing include a stirring speed of 600 rpm to 1500 rpm, a pressure below -0.1 MPa, and a stirring time of 60 s to 300 s.
10. The application of the thermally conductive gel according to any one of claims 1-7 in electronic components.