A method for preparing highly resilient biodegradable containers using mixed crop straw
By combining the compound of crop straw and glycerol activation treatment, and using citric acid-crosslinked oxidized starch-polyvinyl alcohol adhesive, the problem of weak interfacial bonding in mixed fiber containers was solved, and a high-toughness biodegradable container was prepared, achieving efficient utilization and environmentally friendly production.
Patent Information
- Application Number
- CN202611278647.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively utilize mixed crop straw to prepare high-toughness biodegradable containers, facing technical bottlenecks such as the difficulty in balancing the environmental friendliness of adhesives, bonding strength and economic cost, weak interfacial bonding between fibers and the matrix, and prominent interfacial debonding issues.
By using a blend of corn straw, rice straw, and wheat straw, and through glycerol surface activation treatment, combined with a citric acid-crosslinked oxidized starch-polyvinyl alcohol fully degradable adhesive system, a composite material route combining multi-fiber synergistic reinforcement and interfacial chemical bonding was constructed.
The prepared containers have excellent mechanical properties, water resistance and surface smoothness, and a biodegradability rate of over 91% after 180 days. Free formaldehyde was not detected, realizing the high-value utilization of agricultural straw and the large-scale production of environmentally friendly containers.
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of agricultural waste resource utilization, specifically relating to a method for preparing highly resilient biodegradable containers using mixed crop straw. Background Technology
[0002] With the deepening of global "plastic ban / restriction" policies, the demand for fully biodegradable and environmentally friendly container materials is growing. The proportion of crop straw used in high-end molded containers is extremely low; a large amount of straw is still mainly disposed of through low-value return to the field or incineration, resulting in resource waste and environmental pollution. Currently, various technical routes have been developed for container molding using plant fibers and adhesives, but many technical bottlenecks remain. First, it is difficult to balance environmental friendliness, bonding strength, and economic cost in adhesive systems. Formaldehyde-containing adhesives have the problem of releasing free formaldehyde, petroleum-based hot melt adhesives are non-degradable, and single natural adhesives (such as native starch) have poor water resistance and insufficient adhesion, resulting in product strength far below usage standards. Second, existing technologies mostly use single straw varieties or random mixtures, lacking interfacial compatibilization methods for mixed fibers, leading to weak interfacial bonding between fibers and the matrix, and poor overall mechanical properties of the products. Third, the surface of straw fibers is rich in waxy layers and inert groups, resulting in poor wettability with hydrophilic adhesives. Existing technologies have not systematically controlled the polarity of the fiber surface, leading to prominent interfacial debonding problems. Summary of the Invention
[0003] To address the above problems, the present invention aims to provide a method for preparing highly resilient biodegradable containers using mixed crop straw.
[0004] The technical content of this invention is as follows: This invention provides a method for preparing a highly resilient biodegradable container using mixed crop straw, comprising the following steps: 1) Preparation of straw powder Remove impurities from corn stalks, rice stalks, and wheat stalks, cut them into small pieces, dry them separately until the moisture content is less than 8%, grind them into powder, sieve them through a 30-60 mesh, and mix them evenly to obtain straw powder; The mixing mass ratio of corn straw powder, rice straw powder and wheat straw powder is (1~3):(1~2):(1~2); Spray the surface of the straw powder with a glycerol aqueous solution accounting for 1-2% of its mass, and stir at high speed at 60-80℃ to carry out activation treatment; The volume ratio of glycerol to water in the glycerol aqueous solution is 1:(3~5); After activation, dry at low temperature until the moisture content is below 6%.
[0005] The corn stalks used have long fibers and high cellulose content, providing skeletal reinforcement; the rice stalks are rich in a silica layer, which helps improve the surface smoothness of the product; the wheat stalks have a high hemicellulose content, which can partially melt under hot pressing conditions, resulting in in-situ thickening; and the glycerol used in the surface activation treatment is a polyol that can form a hydrophilic active layer on the surface of the straw fibers, forming a dense hydrogen bond network with the hydroxyl groups in the subsequent starch-PVA adhesive.
[0006] 2) Preparation of biodegradable adhesives The raw materials used include plant starch, polyvinyl alcohol, hydrogen peroxide, polyethylene glycol, anhydrous citric acid, sodium hypophosphite, and deionized water; By weight, the plant starch accounts for 20-30 parts, polyvinyl alcohol accounts for 15-20 parts, hydrogen peroxide accounts for 1.5-3 parts, polyethylene glycol accounts for 4-6 parts, anhydrous citric acid accounts for 1-2 parts, sodium hypophosphite accounts for 0.3-0.8 parts, and deionized water accounts for 45-55 parts. a) Mix plant starch and deionized water and stir. Heat the mixture to 88-92°C at a rate of 2°C / min and maintain the temperature for 35-45 minutes until the starch is completely gelatinized and becomes transparent and viscoelastic. Then cool the mixture to 62-68°C and adjust the pH to 3.5-4.2 with dilute hydrochloric acid (0.5 mol / L). Slowly add hydrogen peroxide solution and maintain the temperature for 50-80 minutes for oxidation. After the reaction is complete, adjust the pH to 6.5-7.5 to obtain oxidized starch colloid. Then heat the mixture to 70-75°C and maintain the temperature for later use (preferably 72°C). The carboxyl content of the oxidized starch colloid was determined by titration to be 0.3%~0.6% (relative to dry starch). b) Heat deionized water to 93~97℃, slowly add PVA powder while stirring continuously, keep warm and stir until completely dissolved to obtain a clear and transparent PVA solution, then cool to 70~75℃ for later use. c) While stirring, slowly add the heat-insulated oxidized starch colloid to the PVA solution, continuing to stir to ensure that the molecular chains of the two are fully entangled and miscible; then add the polyethylene glycol plasticizer and stir evenly, and finally add anhydrous citric acid and sodium hypophosphite catalyst in sequence (both are dissolved in a small amount of 60°C warm water before adding), and keep it at 70~75°C for 40~60 minutes for pre-reaction to ensure that the components are fully miscible and partially pre-crosslinked (esterification conversion rate ≤10%, the remaining deep crosslinking will be completed in the subsequent high-temperature molding stage), thus obtaining a uniform, milky white viscous adhesive product. After cooling to room temperature, the rotational viscosity is 6000~12000 mPa·s and the solid content is 28%~34%.
[0007] The plant starch used provides film-forming properties and adhesive strength, but its water resistance is poor. Therefore, active carboxyl groups are introduced by hydrogen peroxide to improve its compatibility with PVA and fibers. PVA, as a toughening segment, has flexible long chains that interpenetrate and entangle with oxidized starch to form a "rigid and flexible" physical cross-linking network, which solves the problem of high brittleness of pure starch glue. Citric acid / sodium hypophosphite constitutes a green cross-linking system, which initiates esterification cross-linking in the subsequent high-temperature molding stage, transforming linear molecular chains into a three-dimensional network structure, thereby significantly improving water resistance and mechanical strength.
[0008] 3) Preparation of high-toughness biodegradable containers Mix straw powder and adhesive at a mass ratio of 10:(1.5~3), first stir at a low speed of 30~40 rpm, then stir at a high speed of 90~110 rpm, control the moisture content to 20~25%, and keep the temperature below 40℃; Finally, the mixture is heated at 120~160℃ and under a pressure of 100~150 kg / cm². 2 Under certain conditions, a high-toughness biodegradable container is obtained by compression molding.
[0009] The beneficial effects of this invention are as follows: This invention provides a method for preparing high-toughness biodegradable containers using mixed crop straws. The method involves compounding corn straw, rice straw, and wheat straw, followed by glycerol surface activation treatment, and then using a citric acid-crosslinked oxidized starch-polyvinyl alcohol (PVA) fully biodegradable adhesive system. The optimal mixing temperature was determined through orthogonal experiments, constructing a composite material preparation route combining multi-fiber synergistic reinforcement and interfacial chemical bonding. Specifically, glycerol activation introduces active hydroxyl groups on the fiber surface, forming a dense hydrogen bond network with the adhesive, effectively enhancing interfacial bonding. Hydrogen peroxide oxidation introduces active carboxyl groups, improving the compatibility of starch with PVA and fibers. The flexible long chains of PVA interpenetrate and entangle with oxidized starch, forming a "rigid-flexible" physical crosslinked network. Citric acid initiates esterification crosslinking during the high-temperature molding stage, transforming the container into a three-dimensional network structure. The container products prepared by this invention exhibit excellent mechanical properties, water resistance, and surface smoothness, with a biodegradability rate exceeding 91% after 180 days. Free formaldehyde was not detected, resulting in an overall improvement in product performance. All raw materials used are bio-based or biodegradable, with wide availability and controllable costs. This provides a practical and feasible technical solution for the high-value utilization of agricultural straw waste and the large-scale production of environmentally friendly containers, and has good application prospects. Detailed Implementation
[0010] The present invention will be further described in detail below through specific implementation examples. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. After reading the present invention, any modifications of the present invention in various equivalent forms by those skilled in the art fall within the scope of the appended claims.
[0011] Unless otherwise specified, all raw materials and reagents used in this invention are from the conventional market.
[0012] Example 1 A method for preparing highly resilient biodegradable containers using mixed crop straw
[0013] 1) Preparation of straw powder After removing impurities and cutting the corn stalks, rice stalks, and wheat stalks into small pieces, they are dried at 80-105℃ until the moisture content is less than 8%, ground through a 40-mesh sieve, and mixed evenly at a mass ratio of 2:1:1 to obtain mixed straw powder. The straw powder was placed in a high-speed mixer and a glycerol aqueous solution (glycerol:water = 1:4, volume ratio) of 1.2% by weight of the straw powder was sprayed evenly. The mixture was then activated by high-speed stirring at 70°C for 18 minutes, followed by low-temperature drying until the moisture content was less than 6% for later use.
[0014] 2) Preparation of biodegradable adhesives a) Mix 25 parts corn starch with 30 parts deionized water and add them to the reactor. Heat the mixture to 90°C at 2°C / min and keep it at this temperature for 40 min until it becomes transparent and viscoelastic. Cool the mixture to 65°C and adjust the pH to 3.8 with dilute hydrochloric acid (0.5 mol / L). Slowly add 2.2 parts hydrogen peroxide (30% concentration) and maintain the temperature for 65 min for oxidation. After the reaction, neutralize the mixture to pH=7.0 to obtain oxidized starch colloid. The carboxyl content was determined by titration to be 0.45% (relative to dry starch). Then, raise the reactor temperature to 72°C and keep it at this temperature for later use. b) Heat 18 parts of deionized water to 95°C, slowly add 17 parts of PVA (type 1788) powder while stirring, keep warm and dissolve until clear and transparent to obtain PVA solution, then cool to 72°C for later use. c) While stirring, slowly add the oxidized starch colloid, which is kept at 72℃, to the PVA solution at the same temperature, and continue stirring for 25 minutes to ensure that the two are fully miscible; add 5 parts of polyethylene glycol (PEG-400) and stir well; finally, add 1.5 parts of anhydrous citric acid and 0.5 parts of sodium hypophosphite pre-dissolved in warm water, and keep at 72℃ for pre-reaction for 50 minutes to obtain the adhesive product, which has a rotational viscosity (GB / T10247-2008, NDJ-1 type rotational viscometer, 12 rpm, 25℃) of 8500 mPa·s and a solid content of 31%.
[0015] 3) Preparation of high-toughness biodegradable containers The straw powder and adhesive were mixed at a mass ratio of 10:2.2. The mixture was first stirred at a low speed of 35 rpm for 6 minutes, and then stirred at a high speed of 100 rpm for 15 minutes. The temperature was controlled at ≤45℃ throughout the process using a jacket cooling system. The final moisture content of the material was controlled at 22%. Finally, the mixture is quantitatively poured into the mold and heated at 140℃ and 100 kg / cm². 2 Under certain conditions, hot pressing molding is used to obtain biodegradable container products.
[0016] Example 2 A method for preparing highly resilient biodegradable containers using mixed crop straw
[0017] 1) Preparation of straw powder After removing impurities and cutting the corn stalks, rice stalks, and wheat stalks into small pieces, they are dried until the moisture content is less than 8%, ground through a 50-mesh sieve, and mixed evenly in a mass ratio of 3:1:1 to obtain mixed straw powder. Place the straw powder into a high-speed mixer, and spray it evenly with a glycerol aqueous solution (glycerol:water = 1:3, volume ratio) accounting for 1.5% of the mass of the straw powder. Activate the mixture at high speed at 75°C for 15 minutes, and then dry it at low temperature until the moisture content is less than 6% for later use.
[0018] 2) Preparation of biodegradable adhesives a) Mix 28 parts of cassava starch with 30 parts of deionized water and add them to a reaction vessel. Heat the mixture to 92°C at 2°C / min and keep it at this temperature for 35 min until it becomes transparent and viscoelastic. Cool the mixture to 68°C, adjust the pH to 4.0 with dilute hydrochloric acid (0.5 mol / L), slowly add 2.8 parts of hydrogen peroxide, and maintain the temperature for 75 min for oxidation. After the reaction is complete, neutralize the mixture to pH=7.2 to obtain oxidized starch colloid. The carboxyl content was determined to be 0.52% by titration. Then, raise the temperature of the vessel to 72°C and keep it at this temperature for later use. b) Heat 20 parts of deionized water to 97°C, slowly add 15 parts of PVA (type 1788) powder while stirring, keep warm and dissolve until clear and transparent to obtain PVA solution, then cool to 72°C for later use;
[0019] c) While stirring, slowly add the oxidized starch colloid, which is kept at 72℃, to the PVA solution at the same temperature, and continue stirring for 20 minutes to ensure that the two are fully miscible; add 4 parts of polyethylene glycol (PEG-400) and stir well; finally, add 1.8 parts of anhydrous citric acid and 0.6 parts of sodium hypophosphite pre-dissolved in warm water, and keep at 72℃ for 45 minutes for pre-reaction to obtain the adhesive product, which has a rotational viscosity of 10200 mPa·s and a solid content of 33%.
[0020] 3) Preparation of high-toughness biodegradable containers The straw powder and adhesive were mixed at a mass ratio of 10:2.5. The mixture was first stirred at a low speed of 30 rpm for 8 minutes, and then stirred at a high speed of 110 rpm for 12 minutes. The temperature was controlled at ≤45℃ throughout the process by jacket cooling. The final moisture content of the material was controlled at 24%. Finally, the mixture is quantitatively poured into the mold and heated at 150℃ and a pressure of 110 kg / cm².2 Under certain conditions, hot pressing molding is used to obtain biodegradable container products.
[0021] Example 3 A method for preparing highly resilient biodegradable containers using mixed crop straw
[0022] 1) Preparation of straw powder After removing impurities and cutting the corn stalks, rice stalks, and wheat stalks into small pieces, they are dried until the moisture content is less than 8%, ground through a 30-mesh sieve, and mixed evenly in a mass ratio of 1:1:1 to obtain mixed straw powder. Place the straw powder into a high-speed mixer, and spray it evenly with a glycerol aqueous solution (glycerol:water = 1:5, volume ratio) accounting for 1.0% of the mass of the straw powder. Activate the mixture by high-speed stirring at 65℃ for 20 minutes, and then dry it at low temperature until the moisture content is less than 6% for later use.
[0023] 2) Preparation of biodegradable adhesives a) Mix 22 parts corn starch with 28 parts deionized water and add them to a reaction vessel. Heat the mixture to 88°C at 2°C / min and keep it at this temperature for 45 min until it becomes transparent and viscoelastic. Cool the mixture to 62°C and adjust the pH to 3.6 with dilute hydrochloric acid (0.5 mol / L). Slowly add 1.8 parts hydrogen peroxide and maintain the temperature for 55 min for oxidation. After the reaction is complete, neutralize the mixture to pH=6.8 to obtain oxidized starch colloid. The carboxyl content was determined to be 0.38% by titration. Then, raise the temperature of the vessel to 72°C and keep it at this temperature for later use. b) Heat 18 parts of deionized water to 93°C, slowly add 18 parts of PVA (type 1788) powder while stirring, keep warm and dissolve until clear and transparent to obtain PVA solution, then cool to 72°C for later use. c) While stirring, slowly add the oxidized starch colloid, which is kept at 72℃, to the PVA solution at the same temperature, and continue stirring for 30 minutes to ensure that the two are fully miscible; add 6 parts of polyethylene glycol (PEG-400) and stir well; finally, add 1.2 parts of anhydrous citric acid and 0.4 parts of sodium hypophosphite pre-dissolved in warm water, and keep at 72℃ for pre-reaction for 55 minutes to obtain the adhesive product, which has a rotational viscosity of 7200 mPa·s and a solid content of 29%.
[0024] 3) Preparation of high-toughness biodegradable containers The straw powder and adhesive were mixed at a mass ratio of 10:1.8. The mixture was first stirred at a low speed of 40 rpm for 5 minutes, and then stirred at a high speed of 90 rpm for 18 minutes. The temperature was controlled at ≤45℃ throughout the process using a jacket cooling system. The final moisture content of the material was controlled at 20%. Finally, the mixture is quantitatively poured into the mold and heated at 130℃ and a pressure of 80 kg / cm². 2 Under certain conditions, hot pressing molding is used to obtain biodegradable container products.
[0025] Example 4 A method for preparing highly resilient biodegradable containers using mixed crop straw
[0026] 1) Preparation of straw powder After removing impurities and cutting the corn stalks, rice stalks, and wheat stalks into small pieces, they are dried until the moisture content is less than 8%, ground through a 60-mesh sieve, and mixed evenly in a mass ratio of 2:2:1 to obtain mixed straw powder. Place the straw powder into a high-speed mixer, and spray it evenly with a glycerol aqueous solution (glycerol:water = 1:4, volume ratio) accounting for 1.8% of the mass of the straw powder. Activate the mixture by high-speed stirring at 78°C for 15 minutes, and then dry it at low temperature until the moisture content is less than 6% for later use.
[0027] 2) Preparation of biodegradable adhesives a) Mix 30 parts corn starch with 32 parts deionized water and add them to a reaction vessel. Heat the mixture to 90°C at 2°C / min and keep it at this temperature for 40 min until it becomes transparent and viscoelastic. Cool the mixture to 65°C and adjust the pH to 4.2 with dilute hydrochloric acid (0.5 mol / L). Slowly add 3 parts hydrogen peroxide and maintain the temperature for 80 min for oxidation. After the reaction is complete, neutralize the mixture to pH=7.0 to obtain oxidized starch colloid. The carboxyl content was determined to be 0.58% by titration. Then, raise the temperature of the vessel to 72°C and keep it at this temperature for later use. b) Heat 20 parts of deionized water to 95°C, slowly add 20 parts of PVA (type 1788) powder while stirring, keep warm and dissolve until clear and transparent to obtain PVA solution, then cool to 72°C for later use; c) While stirring, slowly add the oxidized starch colloid, which is kept at 72℃, to the PVA solution at the same temperature, and continue stirring for 25 minutes to ensure that the two are fully miscible; add 5 parts of polyethylene glycol (PEG-400) and stir well; finally, add 2 parts of anhydrous citric acid and 0.7 parts of sodium hypophosphite pre-dissolved in warm water, and keep at 72℃ for 60 minutes for pre-reaction to obtain the adhesive product, which has a rotational viscosity of 11500 mPa·s and a solid content of 34%.
[0028] 3) Preparation of high-toughness biodegradable containers The straw powder and adhesive were mixed at a mass ratio of 10:2.8. The mixture was first stirred at a low speed of 35 rpm for 7 minutes, and then stirred at a high speed of 100 rpm for 15 minutes. The temperature was controlled at ≤45℃ throughout the process using a jacket cooling system. The final moisture content of the material was controlled at 23%. Finally, the mixture is quantitatively poured into the mold and heated at 155℃ and a pressure of 120 kg / cm². 2 Under certain conditions, hot pressing molding is used to obtain biodegradable container products.
[0029] Comparative Example 1 The difference from Example 1 is that: in the preparation of straw powder, no glycerol aqueous solution is sprayed for surface activation treatment; instead, the dried and ground mixed straw powder is directly mixed with the adhesive. Otherwise, it is the same as Example 1.
[0030] Comparative Example 2 The difference from Example 1 is that: during the preparation of the adhesive, anhydrous citric acid and sodium hypophosphite and subsequent heat preservation pre-reaction operations are not added. The oxidized starch colloid is simply mixed with PVA solution and polyethylene glycol to obtain the finished adhesive product. The rest is the same as in Example 1.
[0031] Comparative Example 3 The difference from Example 1 is that the straw powder uses only corn straw of a single variety, ground to the same fineness (40 mesh), and is otherwise the same as in Example 1.
[0032] Comparative Example 4 The difference from Example 1 is that in step c, the oxidized starch colloid is cooled to 62°C and kept at that temperature, and the PVA solution is also cooled to 62°C before mixing. The rest is the same as in Example 1.
[0033] The adhesive and finished product prepared according to this invention were subjected to relevant tests, as follows: 1. Relevant tests for adhesives The adhesive was sealed and placed in a 60℃ constant temperature chamber for 7 days, and the viscosity change rate before and after was tested.
[0034] Table 1. Storage stability of adhesives Test Project Viscosity change rate after storage (%) Test Project Viscosity change rate after storage (%) Example 1 3.2 Comparative Example 1 3.5 Example 2 3.5 Comparative Example 2 5.8 Example 3 2.8 Comparative Example 3 3.3 Example 4 3.8 Comparative Example 4 — Note: Comparative Example 4 did not undergo storage stability testing because PVA had already undergone severe cold-induced gelation when mixed at 62℃, resulting in an uneven system and an inability to obtain a representative sample.
[0035] After standing at 60°C for 7 days, the viscosity of the adhesives in each embodiment increased by only 2.8% to 3.8%, indicating that the citric acid crosslinking agent only underwent trace pre-crosslinking (esterification conversion rate ≤10%) during the pre-reaction stage at 70-75°C, and the adhesives have good shelf life and industrial applicability. Comparative Example 2 (without crosslinking agent) showed a slightly higher change rate (+5.8%), presumably related to the difference in pH and ionic strength of the system without crosslinking agent, but its absolute change value remained within a controllable range.
[0036] 2. In the adhesive compounding and formulation step of this invention, the mixing temperature of oxidized starch colloid and PVA solution is a key process parameter determining the microstructure uniformity of the adhesive and the mechanical properties of the final product. To determine the optimal mixing temperature, orthogonal experiments were conducted, and the results are as follows: Table 2 Comparison of overall performance at different mixing temperatures Mixing temperature (°C) Mixing uniformity (%) Storage viscosity change rate (%) Flexural strength of the specimen (MPa) 65 86.3 gelation 13.9 68 92.7 8.6 14.8 72 98.6 3.2 15.8 75 97.8 9.6 15.2 80 97.1 14.2 14.5 As shown in Table 2, 72℃ is the optimal mixing and compounding temperature, resulting in superior performance indicators. This ensures uniform dispersion at the molecular level while minimizing premature cross-linking of citric acid, thus balancing adhesive quality and storage stability. Therefore, in step c of all embodiments, the oxidized starch colloid and PVA solution are mixed at 72℃.
[0037] Among them, the 65℃ group: the PVA solution is close to the critical temperature for cold gelation (about 68℃) at this temperature. The viscosity of the system increases sharply when mixed, and the uniformity and strength of the test piece decrease. Furthermore, gelation occurs during storage, making it unusable. The 68℃ group: although it can be mixed with difficulty, the mixing uniformity and storage stability are significantly worse than those of the 72℃ group, and the strength of the test piece is also lower. The 75℃ and 80℃ groups: the mixing uniformity is acceptable, but the storage stability deteriorates significantly, indicating that citric acid has already begun to initiate significant cross-linking at this temperature, and the pot life of the adhesive is greatly shortened.
[0038] 3. Standard specimens were prepared from the mixtures of each embodiment and the comparative example under the same molding conditions, and their physical and mechanical properties were tested: Bending strength: Tested according to GB / T 9341-2008; Impact toughness: Tested according to GB / T 1043.1-2008 (simply supported beam, no notch); Water immersion strength retention rate: The standard bending test specimen is immersed in distilled water at 25℃ for 2 hours. After being removed and the surface moisture is wiped off, the bending strength is immediately tested according to GB / T 9341-2008. The strength is expressed as the percentage of the strength after immersion to the strength in the dry state. Interfacial shear strength: Using the micro-debonding method, a single straw fiber (length ≥ 10 mm) was cut from the product, embedded with adhesive microdroplets, and then pulled out at a loading speed of 1 mm / min. The maximum load was recorded and divided by the interfacial area. Surface finish Ra: Tested according to GB / T 3505-2009; Dimensional tolerance: After molding, place the product horizontally at room temperature for 24 hours, measure the outer diameter of the product with vernier calipers, and calculate the deviation from the nominal value of the mold (the number of measurement points is ≥6, and the maximum deviation value is taken).
[0039] The results are as follows: Table 3 Physical properties of biodegradable container molded products Test Project Flexural strength (MPa) <![CDATA[Impact toughness (kJ / m 2 )]]> Strength retention rate after immersion in water for 2 hours (%) Interfacial shear strength (MPa) Surface finish Ra (μm) Dimensional tolerances (mm) Example 1 15.2 18.5 66.3 4.8 2.5 ±0.12 Example 2 14.6 17.2 63.8 4.5 2.7 ±0.14 Example 3 14 16.8 62.1 4.2 2.9 ±0.15 Example 4 16.8 20.1 68.5 5.1 2.3 ±0.11 Comparative Example 1 10.8 14.6 58.2 3.1 3.8 ±0.28 Comparative Example 2 6.5 19.2 31.6 4.6 2.6 ±0.13 Comparative Example 3 12.1 13.8 64.5 3.9 4.5 ±0.32 Comparative Example 4 12.5 15.3 62.8 4.3 2.8 ±0.18
[0040] As can be seen from Table 3: Effects of glycerol activation treatment (Example 1 and Comparative Example 1): Comparative Example 1, without glycerol activation treatment, showed a decrease in interfacial shear strength of approximately 35.4% compared to Example 1, along with a significant reduction in flexural strength and surface smoothness. This indicates that glycerol forms a hydrophilic active layer on the surface of the straw fibers, creating a dense hydrogen bond network with the hydroxyl groups in the adhesive, effectively enhancing interfacial bonding. The decrease in surface smoothness from Ra 3.8 μm to 2.5 μm is related to the more uniform wetting and coating of the siliceous layer on the rice straw surface by the adhesive after activation.
[0041] The effect of citric acid crosslinking (Example 1 and Comparative Example 2): Comparative Example 2, without the addition of the citric acid / sodium hypophosphite crosslinking system, exhibited higher impact toughness due to the greater flexibility of the uncrosslinked molecular chains. However, its strength retention rate after 2 hours of immersion in water decreased by 52.4% compared to Example 1, and its dry flexural strength was also significantly lower than that of Example 1. This indicates that the esterification crosslinking reaction initiated by citric acid during the high-temperature molding stage transforms linear molecular chains into a three-dimensional chemical network structure, which is a key means of imparting water resistance and high-strength mechanical properties to the product.
[0042] The synergistic effect of the three types of straw (Example 1 and Comparative Example 3): Comparative Example 3 used only corn straw. Although the bending strength was acceptable, the surface smoothness and dimensional tolerance were significantly worse than those of Example 1, and the impact toughness was also lower. This indicates that the surface siliceous layer of rice straw improved the smoothness, the in-situ thickening effect of wheat straw hemicellulose under hot pressing, and the skeletal strengthening effect of corn straw effectively complemented each other.
[0043] The hazards of mixing temperatures below 68°C (Example 1 and Comparative Example 4): In Comparative Example 4, the flexural strength, interfacial shear strength, and dimensional tolerances of the mixed oxidized starch colloid and PVA solution at 62°C were significantly worse than those of Example 1. This may be because the PVA solution is close to its cold-induced gelation critical temperature at 62°C, causing a sharp increase in the viscosity of the mixed system. This prevents the starch and PVA from achieving molecular-level miscibility, resulting in poor adhesive uniformity and consequently affecting the mechanical properties and dimensional stability of the product.
[0044] 4. The biodegradation rate and free formaldehyde release of the finished products from each embodiment and comparative example were tested: Biodegradation rate is referenced to GB / T 41010-2021: composting conditions (58±2℃, humidity ≥70%, inoculum activity ≥30%), cycle 180 days; The free formaldehyde release was determined according to GB 31604.1-2015: spectrophotometric method after immersion in simulated solution.
[0045] The results are as follows: Table 4. Tests on biodegradation rate and free formaldehyde release. Test Project 180-day biodegradation rate (%) Free formaldehyde release (mg / L) Example 1 92.5 Not detected Example 2 91.8 Not detected Example 3 91.2 Not detected Example 4 93.0 Not detected Comparative Example 1 92.1 Not detected Comparative Example 2 93.5 Not detected Comparative Example 3 91.5 Not detected Comparative Example 4 91.8 Not detected As can be seen from Table 4: Biodegradability: All examples achieved a biodegradability rate of over 91% after 180 days, meeting the requirements of GB / T 41010-2021 standard. Comparative Example 2 (without crosslinking agent) showed a slightly higher degradation rate, which is related to its lower crosslinking density and looser network structure, but its mechanical properties were insufficient (see Table 3), rendering it without practical value. The degradation rates of all examples fluctuated within a reasonable range, indicating that the adhesive system of this invention did not compromise the overall biodegradability of the product while ensuring crosslinking density. All raw materials used (starch, PVA, citric acid, polyethylene glycol, and glycerin) are bio-based or biodegradable materials.
[0046] Hygiene and safety (free formaldehyde): The free formaldehyde release in each example and comparative example was not detected (detection limit 0.05 mg / L). This is because the raw materials used in this invention do not contain formaldehyde, and no formaldehyde byproducts are generated under the high temperature molding conditions.
[0047] This invention utilizes a synergistic approach involving straw compounding, glycerol surface activation, and citric acid crosslinking modification of a starch-PVA adhesive system. Through orthogonal experiments to determine the optimal mixing temperature, the storage stability of the adhesive is significantly improved, and the mixing uniformity is greatly enhanced. The products from the examples exhibit excellent performance in flexural strength, impact toughness, water immersion strength retention, surface smoothness, and dimensional accuracy. Furthermore, the biodegradability rate exceeds 91% after 180 days, and free formaldehyde was undetectable. This invention simultaneously improves overall performance while ensuring biodegradability and food safety, providing a technical solution with industrially viable value for the high-value utilization of straw.
[0048] Furthermore, those skilled in the art can combine and integrate the different embodiments or examples described herein, as well as the features of those embodiments or examples, without contradiction. Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions, and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for preparing high-toughness degradable containers using mixed crop stalks, characterized by, Includes the following steps: 1) Preparation of straw powder Remove impurities from corn stalks, rice stalks, and wheat stalks, cut them into small pieces, dry them separately until the moisture content is less than 8%, grind them into powder, sieve them through a 30-60 mesh, and mix them evenly to obtain straw powder; Spray the surface of the straw powder with a glycerol aqueous solution accounting for 1-2% of its mass, and stir at high speed at 60-80℃ to carry out activation treatment; After activation, dry at low temperature until the moisture content is below 6%; 2) Preparation of biodegradable adhesives The raw materials used include plant starch, polyvinyl alcohol, hydrogen peroxide, polyethylene glycol, anhydrous citric acid, sodium hypophosphite, and deionized water; a) Mix plant starch and deionized water and stir. Heat the mixture to 88-92°C at a rate of 2°C / min and keep it at this temperature for 35-45 minutes until the starch is completely gelatinized and becomes transparent and viscoelastic. Then cool the mixture to 62-68°C, adjust the pH to 3.5-4.2, slowly add hydrogen peroxide solution, and maintain the temperature for 50-80 minutes for oxidation. After the reaction is complete, adjust the pH to 6.5-7.5 to obtain oxidized starch colloid. Then heat the mixture to 70-75°C and keep it at this temperature for later use. b) Heat deionized water to 93~97℃, slowly add PVA powder while stirring continuously, keep warm and stir until completely dissolved to obtain a clear and transparent PVA solution, then cool to 70~75℃ for later use. c) While stirring, slowly add the heat-insulated oxidized starch colloid to the PVA solution and continue stirring. Then add the polyethylene glycol plasticizer and stir until uniform. Finally, add anhydrous citric acid and sodium hypophosphite catalyst in sequence and heat at 70~75℃ for 40~60 minutes to allow the components to fully dissolve and partially cross-link, thus obtaining a uniform, milky white viscous adhesive product. 3) Preparation of highly resilient biodegradable containers.
2. The method of claim 1, wherein the mixed crop straw is used to prepare the high-toughness degradable container. The mixing mass ratio of corn straw powder, rice straw powder and wheat straw powder is (1~3):(1~2):(1~2).
3. The method of claim 1, wherein the mixed crop straw is used to prepare the high-toughness degradable container. The volume ratio of glycerol to water in the glycerol aqueous solution is 1:(3~5).
4. The method for preparing a highly resilient biodegradable container using mixed crop straw according to claim 1, characterized in that, The biodegradable adhesive comprises, by weight, 20-30 parts plant starch, 15-20 parts polyvinyl alcohol, 1.5-3 parts hydrogen peroxide, 4-6 parts polyethylene glycol, 1-2 parts anhydrous citric acid, 0.3-0.8 parts sodium hypophosphite, and 45-55 parts deionized water.
5. The method of claim 1, wherein the mixed crop straw is used to prepare the high-toughness degradable container. The anhydrous citric acid and sodium hypophosphite catalyst are dissolved in warm water before use.
6. The method for preparing a high-toughness biodegradable container using mixed crop straw according to claim 1, characterized in that, In step 3), the straw powder and adhesive are mixed at a mass ratio of 10:(1.5~3). First, the mixture is stirred at a low speed of 30~40 rpm, and then stirred at a high speed of 90~110 rpm. The moisture content is controlled at 20~25%, and the temperature is kept below 40℃.
7. The method of claim 1, wherein the mixed crop straw is used to prepare the high-toughness degradable container. In step 3), the mixture is finally heated at 120~160℃ and under a pressure of 100~150 kg / cm². 2 Under certain conditions, a high-toughness biodegradable container is obtained by compression molding.