An atomic oxygen protective coating for the outer surface of an ultra-low orbit spacecraft and its preparation method
By employing the self-passivation reaction and gradient design of silicon-containing precursor coatings in an atomic oxygen environment, the problems of one-time consumption failure and poor thermal cycling resistance of existing coatings have been solved, achieving long-term protection and reducing aerodynamic drag for ultra-low orbit spacecraft, and making it suitable for large-area complex curved surface components.
Patent Information
- Application Number
- CN202611191108.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing protective coatings are consumed and fail in an atomic oxygen environment, lacking long-term self-replenishment capabilities. Rigid inorganic coatings have poor resistance to thermal cycling, and vacuum processes are difficult to adapt to large-area complex components. Existing technologies have failed to effectively solve the long-term protection problem of ultra-low orbit spacecraft.
A silicon-containing precursor coating is used for self-passivation in an atomic oxygen environment. By controlling the degree of curing, unconverted silicon bonds are retained as an on-orbit self-replenishment reserve. Combined with gradient silicon content design and liquid phase coating process, a dense silicon dioxide passivation layer is formed to achieve dynamic balance protection.
It significantly extends the effective protective life of the coating, reduces aerodynamic drag, adapts to large-area complex curved surface components, reduces manufacturing costs, and improves the coating's flexibility and resistance to thermal cycling.
Smart Images

Figure CN123107422A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of space materials and spacecraft surface protection technology, specifically to a silicon-containing coating for atomic oxygen protection on the exposed surface of a low Earth orbit spacecraft and its liquid-phase preparation method. The coating is capable of undergoing a self-passivation reaction in an atomic oxygen environment and achieves long-term protection by reserving silicon bond reserves that can be replenished in orbit. Background Technology
[0002] Very low Earth orbit (VLEO, 150km-300km) satellites are an important development direction for current low Earth orbit constellations due to their low communication latency and high Earth imaging resolution. However, this orbit presents two major challenges posed by exposed surfaces.
[0003] Challenge 1: Atomic oxygen erosion. The VLEO orbital atmosphere is primarily composed of atomic oxygen (AO), with a flux of approximately 10¹. 4 -10¹ 5 The atomic oxygen erosion rate is approximately 3 × 10⁻² / cm²·s, and it exhibits extremely strong oxidizing activity. Exposed polymer-based spacecraft materials (such as polyimide and Kapton) experience C-C and CN bond breakage under continuous atomic oxygen bombardment, leading to material mass loss, surface morphology degradation, and mechanical property deterioration, severely impacting satellite lifespan. Kapton's atomic oxygen erosion rate is approximately 3 × 10⁻² / cm²·s. 4 The mass loss per centimeter can reach tens of micrograms per square centimeter during a year of service in VLEO orbit.
[0004] Challenge Two: Increased Aerodynamic Drag. In rarefied gas conditions, the drag experienced by a satellite is determined by the momentum exchange during collisions between gas molecules and the surface, typically described by the tangential momentum fit coefficient (TMAC). Atomic oxygen erosion causes surface oxidation and roughening, increasing the momentum fit coefficient, thus increasing the aerodynamic drag coefficient. This leads to increased consumption of orbital maintenance propellant, further shortening the satellite's lifespan.
[0005] The two challenges mentioned above are intrinsically related, but have been treated separately in existing research. Current research on atomic oxygen protection (such as atomic layer deposition of alumina and chemical vapor deposition of silicon nitride coatings) primarily focuses on preventing erosion and mass loss; existing research on silicon-containing coatings (such as POSS-doped polyimide and polysilazane silica conversion coatings) has demonstrated excellent resistance to atomic oxygen. However, existing protective coatings generally suffer from a fundamental problem: the passivation layer on the coating surface is continuously consumed by atomic oxygen, and once depleted, it becomes ineffective, representing "one-time protection" and making it difficult to support long-term on-orbit service. Furthermore, processes such as atomic layer deposition and magnetron sputtering suffer from engineering bottlenecks such as reliance on vacuum equipment and difficulty in adapting to large-area, complex, exposed curved surfaces.
[0006] Existing technologies have reported methods for preparing atomic oxygen-resistant coatings using silicon-containing precursors. Chinese patent CN104592893A discloses a solution composition for atomic oxygen-resistant coatings, primarily composed of a perhydropolysilazane that can be converted to silicon oxide. The prepared coating thickness is between 0.1 μm and 10 μm, and the erosion mass loss is less than 0.05 mg / cm² under an atomic oxygen flux of 1.1 × 10²¹ atoms / cm². International patent WO2019140219A1 discloses a coating material that combines atomic oxygen resistance and low aerodynamic drag, reducing drag through an atomically smooth surface, suitable for spacecraft orbiting at altitudes of approximately 100 km to 350 km. However, the aforementioned existing technologies all have significant shortcomings: CN104592893A does not address the precise control of coating curing degree, typically pursuing full curing to improve mechanical strength, and does not reveal the mechanism of long-term self-replenishment achieved by deliberately retaining unconverted silicon bonds; furthermore, the coating thickness is limited to below 10 μm, and there is no record of thick coating protection required for long-term service in ultra-low Earth orbits. WO2019140219A1 relies on the initial atomically smooth surface of the material to reduce drag, but this surface inevitably develops defects under long-term atomic oxygen bombardment. Once the roughness increases, the drag-reduction performance irreversibly degrades; moreover, its protection scheme is static physical protection, lacking dynamic self-replenishment capability. Furthermore, none of the aforementioned existing technologies propose a gradient structure solution for the problem of thermal cycling cracking in spacecraft orbits, nor do they systematically elucidate the influence mechanism of silicon-containing coatings on surface roughness and aerodynamic properties while providing atomic oxygen protection. Therefore, existing silicon-containing coating technologies still have significant room for improvement in terms of long-term protection life and engineering reliability.
[0007] Therefore, the existing technology has the following technical problems that need to be solved: (1) the passivation layer of the protective coating fails after one-time consumption and lacks long-term protection capability; (2) the rigid inorganic protective coating and the polymer substrate are thermally mismatched and are prone to cracking and falling off under orbital thermal cycling; (3) there is a lack of a suitable, low-cost and long-term effective protective coating preparation method for large-area spacecraft exposed parts. Summary of the Invention
[0008] This invention aims to address the technical problems in existing technologies, such as "one-time consumption and failure of protective coatings, lack of long-term self-replenishment capability, poor thermal cycling resistance of inorganic coatings, and difficulty in adapting vacuum processes to large-area complex components." It provides an atomic oxygen protective coating for the outer surface of ultra-low orbit spacecraft with on-orbit self-replenishment capability, long-term effectiveness, resistance to thermal cycling cracking, and suitability for large-area liquid-phase preparation, along with its preparation method. Furthermore, as a beneficial accompanying effect of the protective function, the silica layer formed in situ on the coating surface under the action of atomic oxygen tends to be smooth, helping to maintain a low tangential momentum adaptation coefficient and positively impacting the reduction of aerodynamic drag.
[0009] The core technical idea of this invention is to select a silicon-containing precursor that can undergo a self-passivation reaction in an atomic oxygen environment as a coating material, and to intentionally retain a certain proportion of unconverted silicon bonds as an "on-orbit self-replenishment" reserve during the curing process.
[0010] Upon bombardment by atomic oxygen, the organic components on the coating surface are oxidized and stripped away, while silicon is oxidized in situ to form a dense, glassy silicon dioxide passivation layer. This is because silicon dioxide has an extremely low erosion rate against atomic oxygen (approximately 10⁻²). 5 The resulting silica layer (on the order of cm³ / atom, about an order of magnitude lower than Kapton) effectively prevents atomic oxygen from further eroding the inner layer material.
[0011] like Figure 1 As shown, the coating of the present invention includes a silicon-containing precursor coating body ③, a silicon dioxide passivation layer ② generated in situ on the coating surface under atomic oxygen bombardment ①, and the silicon content in the coating body is distributed in a gradient (the density of circles increases from bottom to top). The coating is applied to the outer surface substrate ④ of the spacecraft.
[0012] like Figure 2 As shown, the core innovation of this invention, which distinguishes it from existing silicon-containing protective coatings, lies in controlling the degree of curing to retain 5wt%-20wt% of unconverted Si-N bonds and / or Si-H bonds within the coating. The initial state (a) is an organic-inorganic hybrid state, where the silicon-containing precursor (○) and organic components (~) are uniformly mixed. During the initial stage of AO bombardment (b), the surface organic components are oxidized and stripped, and silicon is oxidized in situ to generate SiO2 nanoparticles (●). In the stable state (c), a continuous and dense SiO2 passivation layer (■) is formed on the surface, while the inner layer retains some unconverted silicon bonds (○) as an "on-orbit self-replenishment" reserve, achieving a continuous consumption-regeneration balance. During the spacecraft's on-orbit service, while atomic oxygen continuously consumes the surface silicon dioxide passivation layer, the unconverted silicon bonds retained inside the coating act as a reserve, continuously reacting with atomic oxygen to generate new silicon dioxide in situ, forming a dynamic balance of "surface consumption-internal conversion replenishment." This fundamentally solves the problem of "one-time consumption failure" in existing coatings, significantly extending the effective protective lifespan.
[0013] Furthermore, as a beneficial accompanying effect of the formation of the silica passivation layer, the glassy silica surface is chemically inert and tends to be smooth, which theoretically helps to maintain a low tangential momentum adaptation coefficient, thereby helping to reduce aerodynamic drag; this drag reduction effect is an additional beneficial effect of the present invention and is not a necessary limitation of the core protective function.
[0014] In the coating of this invention, the silicon content, based on the atomic mass fraction of silicon, is 15wt%-40wt%, preferably 20wt%-30wt%; the coating thickness is 5μm-50μm, preferably 10μm-30μm. Within the above preferred range, the silicon content is sufficient to rapidly form a continuous and dense silicon dioxide passivation layer under the action of atomic oxygen, without weakening the coating's flexibility and thermal cycling resistance due to excessive inorganic components; the coating thickness ensures sufficient unconverted silicon bond reserves to support long-term on-orbit self-replenishment, while avoiding the risk of curing stress accumulation and cracking caused by excessive thickness. Therefore, a silicon content of 20wt%-30wt% and a thickness of 10μm-30μm are preferred values that balance protective performance, structural reliability, and reserve life.
[0015] The specific technical solution of the present invention is as described in the foregoing claims, with particular emphasis on the following key technical designs and their principles.
[0016] Traditionally, it is believed that the more fully the silicon-containing precursor coating is cured, the better. This invention takes the opposite approach, deliberately controlling the degree of curing to retain 5wt%-20wt% of unconverted Si-N and / or Si-H bonds in the coating. These retained silicon bonds continuously react with atomic oxygen during in-orbit service, replenishing silicon dioxide in situ, forming a dynamic equilibrium in the protective layer. This ensures that the surface consumption rate does not exceed the internal conversion and replenishment rate, achieving long-term stable protection.
[0017] The degree of curing is precisely controlled by the curing temperature (80℃-250℃, with higher temperatures resulting in more complete conversion) and curing time (0.5h-4h). The curing endpoint is determined by real-time tracking of the Si-N bond characteristic peaks (approximately 830cm⁻¹ and 1175cm⁻¹) using Fourier transform infrared spectroscopy. If the retention content is less than 5wt%, the self-replenishment reserve is insufficient, and the lifespan is limited; if the retention content exceeds 20wt%, the initial crosslinking density of the coating is too low, the mechanical strength is insufficient, and the initial protective response is slow.
[0018] like Figure 5 As shown, polysilazane and polyhedral oligomeric silsesquioxane are compounded at a mass ratio of 3:1 to 1:1: the polysilazane is cured to form an organic-inorganic hybrid continuous matrix ①, providing structural integrity; the polyhedral oligomeric silsesquioxane ② is uniformly dispersed as a nanoscale silicon-rich domain (partial magnified figure ③ shows a POSS cage structure). The silica nanoparticles released after atomic oxygen preferentially attacks its organic substituents serve as crystal nuclei, inducing accelerated transformation in the surrounding area of polysilazane, significantly shortening the induction period for the formation of a dense silica layer, so that the protective function can be quickly established in the initial atomic oxygen exposure stage.
[0019] like Figure 4As shown, the mismatch in thermal expansion coefficients at the inorganic-organic interface is the main reason for the cracking and peeling of the coating during orbital thermal cycling (sunlit side +150℃, shaded side -100℃, approximately 90 minutes per cycle). This invention designs a structure with a gradient of silicon content along the thickness direction—the grayscale of the left cross-section gradually deepens from bottom to top, indicating a low-silicon region (10-20wt%) near the substrate, a high-silicon region (30-40wt%) on the outer surface, and a smooth transition zone in between. The curve on the right shows a smooth upward trend in silicon content from near the substrate to the outer surface. The gradient spans 5wt%-10wt% per layer, prepared through multiple coating layers (2-5 times). During curing, partial interdiffusion occurs between adjacent layers, eliminating obvious delamination interfaces and forming a continuous gradient.
[0020] The dispersion state of polyhedral oligomeric silsesquioxanes directly affects the uniformity of the silica passivation layer. This invention controls the dispersed particle size to no more than 50 nm through two steps: (1) first, ultrasonically disperse the polysilazane alone in a solvent for 30-120 min, then add the polysilazane; (2) control the solution concentration to no more than 10 wt% to avoid collisional agglomeration caused by high concentration. Nanoscale uniform dispersion ensures that silica nucleation sites are evenly distributed across the coating cross-section, achieving a density of 10¹. 6 -10¹ 7 The number of cells per cm³ ensures a continuous and dense passivation layer.
[0021] Moisture curing is the dominant pathway for the conversion of polysilazane to silica, but the degree of curing is difficult to precisely stop within a narrow window of 5wt%-20wt% reserve. This invention introduces 254nm-365nm ultraviolet irradiation as a synergistic means: ultraviolet light initiates the free radical crosslinking reaction of Si-H bonds, increasing the crosslinking density of the coating (by 20%-40%) without further promoting the hydrolysis of Si-N bonds. At the same time, the degree of crosslinking is precisely controlled by the irradiation energy density (1000mJ / cm²-5000mJ / cm²), so that the coating has sufficient initial mechanical strength while retaining the reserve of unconverted silicon bonds within the target range.
[0022] When dibutyl ether is used as a solvent, its moderate evaporation rate and low surface tension allow sufficient time for the liquid phase coating to self-level before curing. The final cured coating surface roughness can reach Ra≤0.5μm, which is better than that of tetrahydrofuran (Ra about 0.8μm) and toluene (Ra about 1.2μm). The low initial roughness is beneficial for the coating to maintain a low momentum fit coefficient in the early stages of service.
[0023] Compared with the prior art, the present invention has the following significant advantages:
[0024] By reserving 5wt%-20wt% of unconverted silicon bonds as an on-orbit reserve through controlled curing, a dynamic balance of "surface consumption - internal conversion replenishment" is formed under continuous atomic oxygen erosion, theoretically achieving a service life of 5-10 years (based on calculations and predictions of VLEO orbital atomic oxygen flux and coating thickness). Existing disposable protective coatings fail after the passivation layer is exhausted; this invention significantly extends the service life through a reserve mechanism.
[0025] By using a gradient silicon content design, the thermal expansion mismatch stress at the inorganic-organic interface is effectively mitigated, and the coating adhesion remains good under thermal cycling from -100℃ to +150℃, while existing homogeneous high-silicon coatings crack after only a few cycles.
[0026] Employing a liquid-phase coating process (immersion / spraying), this method eliminates the need for vacuum equipment and is suitable for large-area, complex curved surface components such as satellite solar panel substrates, antenna reflectors, and outer skin of cabins. The cost is significantly lower than atomic layer deposition and magnetron sputtering. The process temperature does not exceed 250℃, ensuring thermal stability compatibility with commonly used aerospace substrates such as polyimide and Kapton.
[0027] With POSS ultrasonic dispersion control (particle size not exceeding 50nm), silica nucleation sites are uniformly and densely distributed, avoiding local weak areas and stress concentration, resulting in a dense passivation layer.
[0028] By combining moisture curing and ultraviolet irradiation, the crosslinking density (increased by 20%-40%) and the proportion of unconverted silicon bonds (5wt%-20wt%) can be precisely controlled to achieve the dual goals of "high initial strength + sufficient long-term reserves".
[0029] As a beneficial accompanying effect of the atomic oxygen-induced silicide self-passivation mechanism, the glassy silicon dioxide passivation layer exhibits strong chemical inertness and a tendency towards smoothness, which helps maintain a low tangential momentum adaptation factor (TMAC). The coating of this invention was irradiated with atomic oxygen (cumulative dose 2 × 10²). 0 After irradiation (atoms / cm²), the measured surface roughness Ra is 0.62-0.85 μm, which is a significant improvement compared to Ra=3.8 μm for uncoated polyimide under the same irradiation conditions. Preliminary predictions based on rarefied gas dynamics theory and molecular dynamics simulations suggest that the TMAC of a smooth silica surface can be maintained below 0.85, a reduction compared to approximately 0.90-0.95 for uncoated or roughened polymer surfaces. Theoretically, this corresponds to a reduction of approximately 10%-15% in the aerodynamic drag coefficient Cd, which is beneficial for reducing orbital sustaining propellant consumption and extending satellite lifespan. Attached Figure Description
[0030] Figure 1This is a schematic cross-sectional view of the coating structure of the present invention. Wherein: ① represents the direction of atomic oxygen bombardment; ② represents the silicon dioxide passivation layer generated in situ after atomic oxygen bombardment; ③ represents the main body of the silicon-containing precursor coating, with the circle density gradually increasing from bottom to top to indicate a gradient distribution of silicon content; ④ represents the substrate on the outer surface of the spacecraft.
[0031] Figure 2 This diagram illustrates the three stages of atomic oxygen-induced silane self-passivation. (a) represents the initial state, where the coating is an organic-inorganic hybrid, with the silicon precursor and organic components uniformly mixed. (b) represents the initial stage of atomic oxygen bombardment, where the surface organic components are oxidized and stripped, and silicon elements are oxidized in situ to generate silicon dioxide nanoparticles, thus the passivation layer begins to form. (c) represents the stable state, where a continuous and dense silicon dioxide passivation layer forms on the surface, while the inner layer retains some unconverted silicon bonds as an on-orbit self-replenishment reserve, achieving a continuous consumption-regeneration balance. Stages (a) to (c) are arranged from left to right, connected by arrows to indicate the direction of time evolution.
[0032] Figure 3 This is a flowchart of the coating preparation process of the present invention. The process includes, in sequence: substrate cleaning → plasma activation → preparation of silicon-containing precursor solution → liquid phase coating (immersion / spraying / spin coating) → moisture curing (80-250℃, 0.5-4h, RH 40%-80%) → UV-assisted curing (optional, 254-365nm, 1000-5000mJ / cm²). Each step is connected sequentially by a vertical arrow.
[0033] Figure 4 This is a schematic diagram of the silicon content distribution in the gradient coating of the present invention. The left side is a schematic diagram of the coating cross-section filling, with the filling density gradually increasing from bottom to top, indicating that the silicon content increases from the near-substrate side to the outer surface side (10-20wt% near the substrate side, 30-40wt% on the outer surface side); the right side is the corresponding silicon content gradient curve, with the vertical axis representing the silicon content (wt%) and the horizontal axis representing the coating depth direction, and the curve showing a smooth upward trend.
[0034] Figure 5 This is a schematic diagram of the microstructure of the composite system of the present invention. Wherein: ① is the polysilazane organic-inorganic hybrid matrix; ② is the POSS cage structure uniformly dispersed in the matrix; ③ is a magnified view of a portion of the POSS structure, showing its cage-like structure. Detailed Implementation
[0035] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments, but the scope of protection of the present invention is not limited to the following embodiments.
[0036] (1) Substrate preparation A 50mm × 50mm × 0.1mm polyimide film was selected as a simulated sample of the exposed substrate for spacecraft. The film was ultrasonically cleaned sequentially with acetone and isopropanol for 5 minutes each to remove surface oil and adsorbates. After drying with nitrogen, the film was placed in a plasma cleaning device for surface activation, with the following parameters: air atmosphere, 100W power, and 2 minutes. After activation, the surface contact angle of the substrate decreased from approximately 70° to approximately 35°, and the surface energy increased, which is beneficial for coating adhesion.
[0037] (2) Preparation of coating solution Take 10g of polysilazane and dissolve it in 90g of dibutyl ether to prepare a homogeneous solution with a solid content of 10wt%. Stir at room temperature for 30 minutes until completely dissolved, and let stand for 10 minutes to defoam.
[0038] (3) Liquid phase coating The immersion method is used: the treated substrate is completely immersed in the coating solution, left for 10 seconds to allow the solution to fully wet the surface, and then lifted at a uniform speed of 5 cm / min. It is then allowed to air dry at room temperature for 15 minutes to allow the solvent to partially evaporate.
[0039] (4) Moisture curing The coated sample was placed in a temperature and humidity controlled curing device, with the temperature set at 150℃, relative humidity at 60%, and the holding time at 2 hours. Water vapor in the moisture catalyzes the hydrolysis and condensation of the Si-N bonds in the polysilazane into Si-O-Si bonds. The reaction can be simplified as: ≡Si-NH-Si≡ + H₂O → ≡Si-O-Si≡ + NH₃↑.
[0040] During the curing process, samples are taken every 30 minutes for rapid infrared spectroscopy detection to track the intensity changes of Si-N bond characteristic peaks (830cm⁻¹, 1175cm⁻¹). Curing is stopped when the peak intensity drops to 15%-20% of the initial value. At this time, about 10wt%-15wt% of the corresponding unconverted Si-N bonds are retained, which meets the requirements for controllable curing degree.
[0041] After curing, the material is allowed to cool naturally to room temperature, resulting in a transparent coating with a thickness of approximately 18 μm.
[0042] (5) Performance characterization Thickness measurement: The height of the coating step was measured using a step meter, and the average value of the three points was 18.2μm ± 0.8μm.
[0043] Silicon content: X-ray photoelectron spectroscopy full spectrum analysis shows that the percentage of silicon atoms is approximately 22 at% (approximately 25 wt% by mass), which is within the design range.
[0044] Surface roughness: Atomic force microscopy scan of a 5μm×5μm area showed a surface roughness Ra=0.42μm, which meets the low roughness requirement.
[0045] Verification of curing degree: Infrared spectroscopy detection showed that the characteristic peak of Si-N bond (830 cm⁻¹) was still visible but its intensity was significantly reduced (down to about 18% of the initial peak intensity), while the broad peak of Si-O-Si (1000-1100 cm⁻¹) was significantly enhanced, confirming that the curing degree was within the controllable target range and that some unconverted silicon bonds were retained.
[0046] (6) Atomic oxygen irradiation test The prepared coating samples were sent to a ground-based atomic oxygen effect simulation test facility for testing. Atomic oxygen was generated using a plasma source, with irradiation parameters of approximately 5 × 10¹ atomic oxygen flux. 5 atoms / cm²·s, cumulative dose 2×10² 0 atoms / cm² (simulating approximately one year of exposure in orbit). A reference sample of an uncoated substrate was irradiated by synchrotron radiation to calibrate the actual atomic oxygen flux.
[0047] Table 1 shows the performance comparison after irradiation.
[0048] Table 1 Comparison of performance of coated and uncoated substrates after atomic oxygen irradiation in Example 1 Results Analysis: The mass loss rate decreased by approximately 93%, confirming that the coating provides effective protection; although the surface roughness increased, the absolute value remained below 1 μm (Ra=0.85 μm), far superior to the Ra=3.8 μm of the uncoated substrate after atomic oxygen etching; the chemical state depth analysis of silicon showed that the silicon in the outer surface region of the coating was mainly in the Si-O-Si state (corresponding to silicon dioxide), the transition region was in a mixed state, and the inner layer was in the incompletely converted Si-N / Si-H state, confirming the expected mechanism of "atomic oxygen-induced outer layer silicification to form a silicon dioxide passivation layer plus inner layer retention reserve" (e.g., Figure 2 (As shown in c). In addition, the surface roughness Ra after coating irradiation is 0.85 μm, which is significantly lower than Ra = 3.8 μm after irradiation of uncoated polyimide. The surface remains relatively smooth. According to the theory of rarefied gas dynamics, a smooth and inert surface helps to reduce the tangential momentum adaptation coefficient of gas molecules, which in turn helps to reduce aerodynamic drag to a certain extent.
[0049] (7) Thermal cycling test The irradiated coating samples were subjected to thermal cycling tests: -100℃ to +150℃, heating and cooling rate of 5℃ / min, holding at each temperature point for 30min, for 50 cycles. After the test, optical microscopy examination showed no visible cracks on the coating surface; the cross-cut adhesion test (100 1mm×1mm grids) showed 0 grids detached, indicating an adhesion grade of 0.
[0050] This embodiment introduces POSS synergistic enhancement based on embodiment 1.
[0051] (1) The substrate preparation is the same as in Example 1.
[0052] (2) Preparation of POSS solution: Take 3g of octaaminophenyl POSS and dissolve it separately in 30g of dibutyl ether. Disperse it ultrasonically for 60 minutes to ensure that the cage structure is completely dispersed and does not agglomerate. Dynamic light scattering test shows that the peak particle size distribution is about 15nm (meeting the requirement of not exceeding 50nm). Then add 7g of polysilazane (the mass ratio of POSS to polysilazane is about 3:7), add dibutyl ether to make up the total solid content 10wt%, stir magnetically for 30 minutes to mix evenly, and let stand to defoam.
[0053] (3) The coating and curing process is the same as in Example 1. The final coating thickness is about 20 μm and the silicon content is about 28 wt% (slightly higher than that of pure polysilazane coating).
[0054] TEM cross-sectional observation (e.g.) Figure 5 It can be seen that the POSS cage-like structures with a size of about 10-20 nm are uniformly dispersed in the matrix, with a dispersion density of about 5 × 10¹. 6 Individuals / cm³, with no obvious aggregation.
[0055] (4) Comparative test of atomic oxygen irradiation Under the same irradiation conditions (cumulative dose 2×10²) 0 Table 2 compares the results with those of Example 1 (atoms / cm²).
[0056] Table 2 Comparison of coating performance between Example 1 and Example 2 Results analysis: The mass loss rate was further reduced by about 33%, confirming that POSS acts as a nucleation site to accelerate the formation of the silica passivation layer; the surface roughness was lower (0.68 μm), which is speculated to be due to the more dense and uniform growth of silica nucleation induced by POSS; the silica passivation layer thickness increased by about 40%, confirming the improved passivation layer density.
[0057] (5) Thermal cycling test: -100℃ to +150℃, 100 cycles, the coating still has no cracks and the adhesion is grade 0.
[0058] In this embodiment, a three-layer gradient coating is prepared, with the silicon content increasing from the inside to the outside: 15wt%→25wt%→35wt%.
[0059] (1) The substrate preparation is the same as in Example 1.
[0060] (2) Applying and curing in multiple layers First layer (near substrate, low silicon content): Prepare a polysilazane solution with a solid content of 8wt% and a silicon content of about 15wt%; apply by impregnation and cure by moisture (150℃, 60%RH, 1.5h) to obtain a first layer with a thickness of about 8μm.
[0061] The second layer (intermediate transition layer): Prepare a mixed solution of 12g polysilazane, 2g POSS, and 86g dibutyl ether (solid content 14wt%), with a silicon content of approximately 25wt%. Repeat the impregnation and coating process on the first layer, followed by moisture curing, to form a second layer with a thickness of approximately 7μm. During the curing process, interfacial interdiffusion occurs between the first and second layers, eliminating the delamination interface.
[0062] The third layer (outer surface, high silicon content): Prepare a mixed solution of 10g polysilazane, 5g POSS, and 85g dibutyl ether (solid content 15wt%), with a silicon content of approximately 35wt%; apply and cure (150℃, 60%RH, 2h) to form a third layer with a thickness of approximately 8μm. The total coating thickness is approximately 23μm.
[0063] (3) Gradient structure characterization Energy dispersive spectroscopy (EDS) was used to scan the silicon content distribution from the near-substrate side to the outer surface of the coating cross-section: approximately 18 wt% silicon was found in the near-substrate region, approximately 25 wt% in the middle region, and approximately 34 wt% on the outer surface, exhibiting a smooth and continuous gradient distribution (e.g., ...). Figure 4 As shown in the figure, there is no mutation interface, confirming successful hierarchical interdiffusion.
[0064] (4) Thermal cycling enhancement test At -100℃ to +150℃ and 150 cycles (extreme conditions), the coating showed no cracking or peeling (adhesion grade 0). In contrast, the control sample (a single-layer homogeneous high-silicon coating, 35wt% silicon content, 23μm thickness) developed microcracks and a drop in adhesion grade to 3 after 75 cycles (approximately 10%-20% peeling area). These results demonstrate that the gradient structure effectively suppresses thermal cycling cracking by buffering stress through a flexible inner layer, increasing the reliable thermal cycle count by approximately two times.
[0065] (5) Properties after atomic oxygen irradiation At a cumulative dose of 2×10² 0 After irradiation with atoms / cm²: mass loss rate 0.07 mg / cm² (better than Examples 1 and 2, attributed to rapid formation of a thick passivation layer due to high silicon content in the outer layer); surface Ra = 0.62 μm (remains smooth); silicon dioxide layer thickness approximately 280 nm, the thickest among the three examples.
[0066] This embodiment adds an ultraviolet irradiation step to the basic embodiment 1.
[0067] (1) Substrate preparation, coating, and moisture curing are the same as in Example 1 (150℃, 60%RH, 2h) to obtain a preliminary cured coating.
[0068] (2) UV-co-curing: The pre-cured coating was irradiated under a UV irradiation device with a main wavelength of 365 nm and a cumulative irradiation energy density of 3000 mJ / cm². The UV light initiated the free radical cross-linking reaction of the residual Si-H bonds, further increasing the cross-linking density of the coating.
[0069] (3) Comparison of crosslinking density and degree of curing Infrared spectroscopy was used to compare the peak areas of Si-O-Si before and after UV treatment (integrated area of 1000-1100 cm⁻¹): the peak area was approximately 48 after moisture curing (arbitrary unit), and approximately 62 after UV-co-curing (an increase of approximately 29%). Simultaneously, the Si-N bond peak intensity (830 cm⁻¹) decreased from approximately 18% of the initial value after moisture curing to approximately 12% of the initial value, confirming that some Si-N participated in cross-linking under UV induction, but still retained approximately 10wt%-12wt% of unconverted silicon bonds, meeting the requirements for on-orbit storage.
[0070] Nanoindentation testing showed that the coating hardness increased from about 0.8 GPa after moisture curing to about 1.1 GPa after UV curing (an increase of about 38%), and the elastic modulus increased from about 8 GPa to about 11 GPa, confirming that the increased crosslinking density improved the mechanical strength.
[0071] (4) Long-life irradiation test At a higher cumulative dose of 5×10² 0 After irradiation at atoms / cm² (simulating approximately 2.5 years of on-orbit operation): mass loss rate 0.35 mg / cm² (although higher than 2 × 10²). 0 The dose was 0.12, but the loss rate did not accelerate significantly, confirming that the inner layer reserves were continuously converted and replenished; the surface Ra=1.2μm (still relatively smooth); the silica layer thickness was approximately 420nm (compared to 2×10²). 0 The 180nm at the dosage almost doubled, confirming that the passivation layer continued to thicken during long-term service.
[0072] The comparison sample (Example 1, no UV curing) was tested at 5 × 10² 0 Localized erosion pits and a mass loss rate of 0.58 mg / cm² were observed after the dosage was applied, confirming that UV-assisted curing enhances the structural integrity and reserve utilization efficiency of the coating during long-term service by increasing the initial crosslinking density.
[0073] This embodiment verifies the applicability of the coating of the present invention to different exposed substrates of spacecraft, and selects polyvinylidene fluoride flexible film as substrate.
[0074] (1) Substrate preparation: A 50mm×50mm×0.05mm polyvinylidene fluoride film was selected. Due to its low surface energy and strong hydrophobicity, adhesion is difficult. Therefore, the activation treatment was strengthened: first, it was ultrasonically cleaned with anhydrous ethanol for 5 minutes, and then activated by oxygen plasma with the following parameters: oxygen atmosphere, power 150W, and time 3min. After activation, the surface contact angle decreased from about 90° to about 40°, and oxygen-containing polar groups were introduced, which significantly improved the coating adhesion.
[0075] (2) Coating solution preparation and application: The composite system of Example 2 was used (POSS to polysilazane mass ratio 3:7, solid content 10wt%, dibutyl ether solvent, POSS pre-ultrasonic dispersion for 60min). Considering that the flexible substrate is not suitable for long-term high temperature, a spraying method was adopted (low mechanical stress on the film): spray distance 20cm, spraying pressure 0.3MPa, spraying 3 times in succession, with a 30-second interval between each spray to allow the solvent to initially evaporate.
[0076] (3) Low-temperature curing: Due to the limited temperature resistance of polyvinylidene fluoride, the curing temperature was lowered to 120℃ and the curing time was extended to 3 hours to compensate for the conversion rate at low temperature. The humidity was maintained at 60%RH. After curing, infrared detection showed that about 15wt% of Si-N bonds remained (the conversion was slower at low temperature, so the reserve was slightly higher, but still within the target range), and the coating thickness was about 16μm.
[0077] (4) Flexibility test: The coated sample was bent 180° around a 10mm diameter rod and bent repeatedly 100 times. The coating was then examined under an optical microscope and found to be free of cracks and peeling. This is attributed to the flexibility provided by the organic components of the composite coating, as well as the presence of unconverted silicon bonds that result in a moderate crosslinking density and good toughness in the coating.
[0078] (5) Atomic oxygen irradiation test: cumulative dose 2×10² 0 After irradiation with atoms / cm², the mass loss rate was 0.10 mg / cm², the surface Ra increased from 0.5 μm to 0.75 μm (maintaining smoothness), and the adhesion was grade 0.
[0079] The results show that by adjusting the activation parameters and curing temperature, the coating of the present invention can be successfully adapted to various spacecraft exposed substrates such as polyvinylidene fluoride, and has good substrate versatility.
[0080] To further highlight the technical effects of the present invention, the following comparative examples are provided, under the same atomic oxygen irradiation conditions (cumulative dose 2×10²). 0 Comparison with embodiments of the present invention (atoms / cm²)
[0081] Comparative Example 1: Uncoated polyimide film. After irradiation, the mass loss rate was 1.82 mg / cm², and the surface roughness increased sharply from 0.5 μm to 3.8 μm.
[0082] Comparative Example 2: Atomic Layer Deposition of Alumina Coating. A 100 nm alumina coating was deposited on a polyimide film. The mass loss rate after irradiation was 0.15 mg / cm² (the protective performance is comparable to that of this invention), but the surface Ra = 0.9 μm (the rigid coating developed microcracks due to thermal shrinkage of the substrate, and atomic oxygen penetrated along the cracks, forming local coarsening); after 50 thermal cycles, obvious crack mesh appeared, and the adhesion dropped to level 2; the preparation requires vacuum equipment and cannot be adapted to large-area curved surfaces.
[0083] Comparative Example 3: Single-layer homogeneous high-silicon coating (silicon content 35wt%). A single-layer homogeneous coating (thickness 23μm, no gradient) was prepared using the same high-silicon formulation as the outer layer of Example 3. The mass loss rate after irradiation was 0.09mg / cm² (good protection), but microcracks appeared after 75 thermal cycles and the adhesion dropped to level 3, confirming that the high-silicon coating without gradient buffer has poor thermal cycling resistance.
[0084] Comparative Example 4: Fully cured polysilazane coating (no reserve design). The formulation of Example 1 was used, but the curing conditions were intensified to 250°C for 4 hours, allowing for complete conversion of the polysilazane (infrared detection showed almost complete disappearance of Si-N bonds, with less than 2 wt% remaining). At 2 × 10² 0 The mass loss rate at the dose irradiation was 0.13 mg / cm² (similar to Example 1), but at a higher dose of 5 × 10² 0 The mass loss rate reached 0.72 mg / cm² at atoms / cm² (far higher than the 0.35 mg / cm² of the UV-cured sample in Example 4), and obvious erosion pits appeared, confirming that the long-term protective life of the fully cured coating, which lacks on-orbit self-replenishment reserves, was significantly shortened.
[0085] The comprehensive comparison results are shown in Table 3.
[0086] Table 3. Overall performance comparison between the present invention and the comparative example. As can be seen from the comprehensive comparison, the coating of the present invention achieves the best performance in terms of protection, thermal cycling resistance, long life, and large-area preparation. The advantage of long life is due to the on-orbit self-replenishment reserve reserved by the controllable curing degree, which is something that existing disposable protective coatings cannot achieve.
Claims
1. An ultra-low Earth orbit spacecraft outer surface atomic oxygen protection coating, characterized by: The coating is formed by controlled curing of a silicon-containing precursor to form an organic-inorganic hybrid matrix. The silicon content in the coating is 15wt%-40wt% based on the atomic mass fraction of silicon, and the coating thickness is 5μm-50μm. After curing, 5wt%-20wt% of unconverted Si-N bonds and / or Si-H bonds are retained in the coating. In an orbital atomic oxygen environment, the silicon element on the surface of the coating is oxidized in situ to form a dense silicon dioxide passivation layer to achieve protection. At the same time, the unconverted silicon bonds inside the coating continue to react with atomic oxygen to generate new silicon dioxide, forming a dynamic self-replenishment of the consumed passivation layer and extending the effective protective life of the coating.
2. The coating of claim 1, wherein: The silicon-containing precursor is selected from at least one of polysilazane, polyhedral oligomeric silsesquioxane and its modified derivatives, and silicon-containing organic-inorganic hybrid sol-gel precursors.
3. The coating of claim 2, wherein: The silicon-containing precursor is a composite system of polysilazane and polyhedral oligomeric silsesquioxane, with a mass ratio of 3:1 to 1:
1. The polysilazane forms a continuous organic-inorganic hybrid matrix, and the cage structure of the polyhedral oligomeric silsesquioxane provides nanoscale silicon-enriched domains. The residual silica nanoparticles after the atomic oxygen preferentially attacks the cage-shaped organic substituents serve as nucleation sites for the passivation layer, accelerating the formation of a coherent and dense silica passivation layer.
4. The coating according to any one of claims 1-3, characterized in that: The coating has a gradient structure with a silicon content varying along the thickness direction. The silicon content near the substrate is 10wt%-20wt%, and the silicon content on the outer surface is 30wt%-40wt%. In the gradient structure, the low silicon content layer near the substrate alleviates the interfacial stress caused by the mismatch of thermal expansion coefficients at the inorganic-organic interface during thermal cycling from -100℃ to +150℃, while the high silicon content layer on the outer surface preferentially reacts with atomic oxygen to form a silicon dioxide passivation layer to provide initial protection.
5. The coating according to claim 4, characterized in that: The gradient structure is obtained by multiple coatings, each coating using a silicon-containing precursor solution with increasing silicon content, and the number of coatings is 2-5. Each coating is cured independently, and the silicon content increases by 5wt%-10wt% between adjacent coatings.
6. The coating according to any one of claims 1-5, characterized in that: The content of unconverted Si-N bonds and / or Si-H bonds retained in the coating is judged by the criterion that the intensity of the characteristic peak of Si-N bonds at 830 cm⁻¹ measured by Fourier transform infrared spectroscopy decreases to 15%-20% of the initial value before curing.
7. The coating according to claim 3, characterized in that: The polyhedral oligomeric silsesquioxane has a dispersed particle size of not more than 50 nm in the coating; and the distribution density of the silicon dioxide nucleation sites is 10 6 - 1 7 0 1 cm-3 in the cross section of the coating.
8. A method for preparing the coating according to any one of claims 1-7, characterized in that... Includes the following steps: (1) Surface activation of the substrate: The substrate on the outer surface of the spacecraft is ultrasonically cleaned with organic solvent in sequence, and then subjected to plasma activation treatment. The activation parameters are power 50W-200W, time 1min-5min, and atmosphere is air or oxygen; (2) Preparation of silicon-containing precursor solution: The silicon-containing precursor is dissolved in organic solvent to prepare a coating solution with a solid content of 5wt%-20wt%; (3) Liquid phase coating: The coating solution is uniformly coated on the surface of the substrate after step (1) by dip coating, spraying or spin coating process; (4) Controlled curing: The coated substrate is placed in a controlled atmosphere with a relative humidity of 40%-80% and kept at 80℃-250℃ for 0.5h-4h. Water vapor is used to catalyze the hydrolysis and condensation of silicon bonds in the silicon-containing precursor. By controlling the curing temperature and holding time, 5wt%-20wt% of unconverted Si-N bonds and / or Si-H bonds are retained in the cured coating. The intensity of the characteristic peak of Si-N bonds at 830cm⁻¹ is monitored by Fourier transform infrared spectroscopy, and the curing termination criterion is used when the intensity drops to 15%-20% of the initial value before curing.
9. The preparation method according to claim 8, characterized in that: After step (4), an ultraviolet irradiation step is added, with an ultraviolet wavelength of 254nm-365nm and an irradiation energy density of 1000mJ / cm²-5000mJ / cm². The synergistic effect of ultraviolet irradiation and thermal curing increases the crosslinking density of the coating by 20%-40%, while controlling the retention ratio of unconverted silicon bonds within the range of 5wt%-20wt%.
10. The preparation method according to any one of claims 8-9, characterized in that: In step (2), the polyhedral oligomeric silsesquioxane is first ultrasonically dispersed in an organic solvent for 30 min-120 min, and then polysilazane is added and stirred evenly. After standing and defoaming, it is used. The stepwise dispersion process ensures that the particle size of the polyhedral oligomeric silsesquioxane dispersed in the solution does not exceed 50 nm.
Citation Information
Patent Citations
Solution composition for atomic oxygen resistant coating, material containing coating and preparation method of material
CN104592893A
Atomic oxygen-resistant, low drag coatings and materials
WO2019140219A1