Low-absorption, radiation-resistant thermally controlled white paint and coating based on Zn2SiO4@silicon-rich glass core-shell structure, and their preparation methods
By combining a Zn2SiO4@silicon-rich glass core-shell structure with a Ce-modified potassium silicate binder, the problems of weak interfacial bonding between fillers and binders and incomplete radiation protection in spacecraft thermal control coatings were solved, achieving an ultra-low absorptivity and excellent radiation stability. The coating exhibited high adhesion and low radiation degradation in the space environment.
Patent Information
- Application Number
- CN202611138695.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
In existing spacecraft thermal control coatings, the interfacial bonding between fillers and binders is weak, and the radiation protection function is limited to the interior of the fillers. The integrated chemical protection of fillers and binders has not been achieved, resulting in the degradation of coating performance under space irradiation conditions.
A functional filler with a Zn2SiO4@silicon-rich glass core-shell structure and a Ce-modified potassium silicate binder are used to achieve chemical bonding between the filler and the binder through in-situ growth of the core-shell structure. Ce ions are uniformly distributed in the filler shell and the binder matrix to form a dual-channel irradiation protection.
It achieves ultra-low solar absorptivity, excellent radiation resistance and high adhesion. The coating shows little change in solar absorptivity after vacuum ultraviolet irradiation and no cracking during thermal cycling, which significantly improves the space environment stability of the coating.
Smart Images

Figure CN123107428A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of spacecraft thermal control coating materials technology, specifically relating to a low-absorption, radiation-resistant thermal control white paint, coating, and preparation method based on a Zn2SiO4@silicon-rich glass core-shell structure. Background Technology
[0002] During spacecraft operation in orbit, solar irradiation is the primary external heat source for their surface thermal balance. Thermal control coatings maintain a low solar absorptivity (α). s Surface absorptivity (SA) is a core component of thermal control systems, used to regulate surface temperature. Coating-type thermal control coatings consist of white inorganic fillers and binders, with the solar absorptivity of the fillers directly determining the coating's thermal control performance. Traditional white fillers are mainly metal oxides such as zinc oxide (ZnO) and zinc titanate (ZnTiO3). However, under combined space proton, electron, and ultraviolet irradiation conditions, defects such as oxygen vacancies and zinc interstitials easily form in the ZnO lattice, resulting in color centers and a significant increase in solar absorptivity. Developing novel white fillers that combine ultra-low initial solar absorptivity with excellent space irradiation stability is an urgent need in this field.
[0003] Zinc silicate (α-Zn₂SiO₄) has become a key focus for next-generation thermally controlled fillers due to its wide bandgap (approximately 5.5 eV). Its fundamental absorption edge is located at approximately 225 nm, and it does not exhibit intrinsic absorption in the main energy band of the solar spectrum (300-2500 nm). Microcrystalline glass technology provides a novel approach for preparing high-performance Zn₂SiO₄ fillers. Through a melt-quench-controlled crystallization process, α-Zn₂SiO₄ crystals can be precipitated in situ from the glass matrix, spontaneously forming a silicon-rich glassy shell around the grains. A continuous glassy phase transition interface exists between the shell and the crystal nucleus. This shell is rich in Si-OH active groups, providing unique surface chemical conditions for chemical bonding with potassium silicate binders. Furthermore, Ce ion doping is an effective means to improve the radiation resistance of materials. 3+ / Ce 4+ Variable valence cycles can trap electrons and holes generated by irradiation. However, existing studies either only introduce Ce into the filler or only focus on optimizing the performance of the filler itself, without achieving the synergistic design of in-situ grown core-shell structure fillers and functionalized binders, resulting in insufficient interface protection.
[0004] In summary, the existing technologies mainly have the following problems: (1) In the existing potassium silicate thermal control coatings, the filler and binder are physically embedded, resulting in weak interfacial bonding: In the existing inorganic thermal control coatings, the filler and potassium silicate binder are physically embedded. The filler particles are mechanically wrapped by the potassium silicate gel. After curing, no chemical bond is formed between the two. Under the thermal cycling (-130 to 150°C) conditions experienced by the spacecraft in orbit, the filler and binder are prone to interfacial microcracks due to the difference in thermal expansion coefficients, which leads to a decrease in coating adhesion (usually ≥1 level in cross-cut test) and causes degradation of optical performance. At the same time, the abrupt change in refractive index between the filler particles and the binder significantly increases the interfacial scattering loss, making the solar absorptivity of the coating generally higher than the inherent absorption level of the filler powder itself; (2) In the existing thermal control coatings, the radiation protection function of Ce is limited to the inside of the filler, and the binder matrix lacks radiation protection capability: Ce exists in the form of doped ions inside the filler particles. The potassium silicate binder matrix does not contain Ce ions. The electron-hole pairs generated by irradiation cannot be blocked by Ce in the binder area between the filler particles. 3+ / Ce 4+ The variable valence cycle effectively captures and annihilates, and the filler / binder interface becomes a weak link in radiation protection. The radiation protection of the full coating has the defect of incomplete spatial coverage; (3) The surface chemical characteristics of the in-situ grown core-shell structure filler have not been used to construct the filler-binder integrated protection system: The surface of the in-situ grown core-shell structure Zn2SiO4@SiO2 microcrystalline glass filler is a continuous silicon-rich glass phase shell layer, which is rich in Si-OH active groups. This unique surface chemical characteristic enables it to have the conditions to chemically bond with potassium silicate binder. The Si-OH on the filler surface can co-condense with the Si-OH of potassium silicate to form Si-O-Si covalent bonds during the curing process. However, the existing technology only focuses on the preparation and performance of the filler itself, without involving the matching design of this surface chemical characteristic with functionalized binder to construct a chemically integrated coating structure of filler-binder. Summary of the Invention
[0005] To address the aforementioned technical problems, the present invention aims to provide a low-absorption, radiation-resistant thermally controlled white paint, coating, and preparation method thereof based on a Zn2SiO4@silicon-rich glass core-shell structure.
[0006] In a first aspect, the present invention provides a low-absorption, radiation-resistant thermal control white paint based on a Zn2SiO4@silicon-rich glass core-shell structure, wherein the components of the low-absorption, radiation-resistant thermal control white paint based on a Zn2SiO4@silicon-rich glass core-shell structure include: functional fillers and radiation-resistant modified binders. The functional filler includes in-situ precipitated core-shell structured Zn2SiO4@SiO2 microcrystalline glass; The radiation-resistant modified binder includes a Ce-modified potassium silicate aqueous solution.
[0007] Preferably, the core-shell structured Zn2SiO4@SiO2 microcrystalline glass uses Zn2SiO4 as the crystal nucleus and a silicon-rich glassy SiO2 phase as the shell, with a continuous glassy phase transition interface between the shell and the crystal nucleus; preferably, the shell is enriched with Ce. 3+ and Ce 4+ Ce ions in mixed valence states.
[0008] Preferably, the particle size D50 of the core-shell structure Zn2SiO4@SiO2 microcrystalline glass filler is 1-5 μm; more preferably, the particle size of the crystal nucleus is 50-200 nm, and the thickness of the silicon-rich glass SiO2 phase shell is 100-300 nm. Preferably, in the Ce-modified potassium silicate aqueous solution, CeO2 accounts for 0.5-1.5 wt% of the potassium silicate solid content.
[0009] Preferably, the mass ratio of the functional filler to the radiation-resistant modified binder is 1:0.5-1.2.
[0010] Secondly, the present invention provides a method for preparing the above-mentioned low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure, the preparation method comprising the following steps: (1) Weigh the raw materials according to the functional filler group distribution ratio and mix them to obtain a mixture. Then melt, cast, anneal and cool to obtain a precursor glass. Next, nucleate and crystallize the precursor glass to obtain a microcrystalline glass block. After crushing, obtain functional filler powder. (2) Low modulus potassium silicate and silica sol are stirred and reacted to obtain high modulus potassium silicate solution, and then soluble cerium salt is added and mixed evenly to obtain radiation-resistant modified binder; (3) The functional filler powder is mixed evenly with the radiation-resistant modified binder to obtain a low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure.
[0011] Preferably, in step (1), the raw materials of the functional filler include the following components by molar percentage: ZnO 34-40%, SiO2 42-50%, Al2O3 8-12%, K2O 4-8%, CeO2 0.1-0.5%, nucleating agent 0.5-1.5%, and the sum of the molar percentages of each component is 100%. Preferably, the molar ratio of ZnO to SiO2 is 0.75-0.82, and the nucleating agent is selected from at least one of ZrO2, SnO2, and Y2O3.
[0012] Preferably, in step (1), the melting temperature is 1450-1550℃ and the holding time is 1-3 hours; Preferably, the annealing temperature is 500-550℃, and the holding time is 1-2 hours.
[0013] Preferably, the nucleation treatment temperature is 30-60°C higher than the initial glass transition temperature (Tg) of the precursor glass, the treatment time is 1-2 hours, and the heating rate is 5-10°C / minute; more preferably, the Tg is 630-700°C. The crystallization treatment temperature is 20-50°C lower than the peak temperature Tp of the exothermic crystallization peak of the precursor glass, the time is 2-8 hours, and the heating rate is 2-5°C / minute; preferably, the Tp is 800-850°C.
[0014] Preferably, in step (2), the modulus of low-modulus potassium silicate is 2.0-3.0, the temperature of the stirring reaction is 40-60℃, the time is 2-6 hours, and the modulus of high-modulus potassium silicate is 4.5-6.0; Preferably, the soluble cerium salt includes at least one of cerium nitrate, cerium acetate, or cerium chloride.
[0015] Thirdly, the present invention also provides a method for preparing a thermal control coating using the above-mentioned low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure. The preparation method includes the following steps: spraying the low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure onto the surface of a substrate, and curing it to obtain the low-absorption, radiation-resistant thermal control coating based on the Zn2SiO4@silicon-rich glass core-shell structure.
[0016] Beneficial effects (1) Ultra-low solar absorptivity – achieved through integrated chemical bonding of filler and binder: The solar absorptivity α of the coating of this invention s ≤0.08, this effect stems from the chemical bonding mechanism described in Improvement Point 1. During curing, the Si-OH groups of the silica-rich glassy shell on the filler surface co-condense with the Si-OH groups of potassium silicate to form Si-O-Si covalent bonds. The filler is upgraded from "physical embedding" to chemical anchoring within the three-dimensional network of the coating. This bonding significantly reduces abrupt changes in interfacial refractive index and scattering losses, ensuring that the solar absorptivity of the coating remains essentially consistent with the inherent absorptivity of the filler powder. This completely solves the problem of α-reflection in physically embedded coatings. s Generally higher than filler powder α s The core defect; (2) Excellent vacuum ultraviolet irradiation resistance – achieved through the dual-channel spatial distribution of the Ce full coating: after 5000 equivalent solar hours of vacuum ultraviolet irradiation, the change in solar absorptivity Δα of the coating of the present invention is as follows. s≤+0.06, this effect originates from the dual-channel Ce distribution described in improvement point two. Ce ions in the filler shell and Ce ions in the binder matrix spatially and synergistically capture electron-hole pairs generated by irradiation, thereby achieving this effect through Ce... 3+ ←→Ce 4+ The variable valence cycle annihilates it in a non-radiative recombination manner, suppressing the formation of color centers at the source. Compared with coatings containing only Ce as filler, the dual-channel design of this invention further reduces irradiation degradation, demonstrating the innovative value of spatial synergistic gain. (3) Excellent adhesion and thermal cycling resistance – achieved through the synergy of chemical bonding interface and in-situ grown core-shell structure: The adhesion of the coating of this invention is grade 1 according to the cross-cut test, and there is no cracking or peeling after 150 thermal cycles at (-130~150℃); This effect is mainly due to the following reasons: On the one hand, the filler is firmly anchored in the coating network through Si-O-Si covalent bonds, and the interface bonding strength is far greater than that of physically embedded coatings; On the other hand, the continuous glass phase transition interface between the shell and the crystal nucleus in the in-situ grown core-shell structure ensures the matching of thermal expansion coefficients, effectively avoiding the problem of interface microcracks generated by traditional core-shell structures during thermal cycling. Attached Figure Description
[0017] Figure 1 This is an exemplary process flow diagram for the preparation of low-absorption, radiation-resistant thermally controlled white paint and coating based on Zn2SiO4@silicon-rich glass core-shell structure provided by the present invention. Figure 2 The image shows the X-ray diffraction pattern of the functional filler powder prepared in Example 1. Figure 3 Scanning electron micrograph of the functional filler powder prepared in Example 1; Figure 4 This is a comparison of the UV-Vis-NIR diffuse reflectance spectra of the coatings prepared in Example 1; Figure 5 The image shows a surface scanning electron microscope image of the coating prepared in Example 1; Figure 6 The image shows an adhesion test photograph of the coating prepared in Example 1. Detailed Implementation
[0018] The present invention will be further illustrated by the following embodiments. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the present invention.
[0019] First, this invention provides a low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure. The components of this Zn2SiO4@silicon-rich glass core-shell structure low-absorption, radiation-resistant thermally controlled white paint may include: functional fillers and radiation-resistant modified binders; the functional fillers may include in-situ precipitated core-shell structure Zn2SiO4@SiO2 microcrystalline glass, and the radiation-resistant modified binder may include Ce-modified potassium silicate aqueous solution.
[0020] In some embodiments, the core-shell structured Zn2SiO4@SiO2 glass-ceramics uses Zn2SiO4 as the crystal nucleus and a silicon-rich glassy SiO2 phase as the shell, with a continuous glassy phase transition interface between the shell and the crystal nucleus; preferably, the shell is enriched with Ce. 3+ and Ce 4+ Ce ions in mixed valence states.
[0021] In some embodiments, the particle size D50 of the core-shell structure Zn2SiO4@SiO2 microcrystalline glass filler can be 1-5 μm; preferably, the particle size of the crystal nucleus is 50-200 nm, and the thickness of the silicon-rich glass SiO2 phase shell is 100-300 nm.
[0022] The above dimensional parameters are the result of synergistic optimization after comprehensively considering optical scattering efficiency, intrinsic transparency, and interfacial chemical bonding requirements: the overall particle size D50 of the filler is controlled at 1-5 μm, making it close to the main energy band of the solar spectrum (300-2500 nm). Maximizing the diffuse reflectance of near-infrared radiation according to Mie scattering theory is key to achieving an ultra-low solar absorptivity. The crystal nucleus size is controlled at 50-200 nm, much smaller than the wavelength of visible light, which avoids scattering of visible light and maintains the optical transparency of the Zn2SiO4 wide bandgap material outside the intrinsic absorption edge (about 225 nm), while ensuring that the grains do not grow abnormally during the controllable crystallization process of the glass-ceramic. The shell thickness is designed to be 100-300 nm. On the one hand, this is sufficient to form a refractive index gradient transition layer to mitigate abrupt refractive index changes between the core and shell, and between the filler and the binder, reducing interfacial scattering losses. On the other hand, the shell surface is rich in Si-OH active groups, and this thickness provides ample chemical bonding sites to ensure sufficient co-condensation with the potassium silicate binder to form Si-O-Si covalent bonds. The synergistic effect of these three factors gives the filler efficient light scattering, intrinsic transparency, and chemical anchoring functions, jointly ensuring the coating's ultra-low solar absorptivity and excellent space environment stability.
[0023] In some embodiments, Ce is introduced into the Ce-modified potassium silicate aqueous solution in the form of a soluble cerium salt; preferably, CeO2 accounts for 0.5-1.5 wt% of the solid content of potassium silicate.
[0024] This ratio is an optimized result that balances radiation protection efficiency and coating optical properties. If the content is too low, the Ce content in the binder matrix will be insufficient. 3+ / Ce 4+ Insufficient density of active sites makes it impossible to effectively capture electron-hole pairs generated by irradiation in the binder region between fillers, making this region a weak point in the protection. The synergistic gain of the dual channels cannot be fully realized, resulting in a change in the solar absorptivity (Δα) after irradiation. s The content will exceed expectations; if the content is too high, the cerium-rich segregating phase may introduce additional absorption centers, reducing the initial solar absorptivity (α) of the coating. s The increase in concentration weakens the ultra-low absorption characteristics imparted by Zn2SiO4.
[0025] In some embodiments, the mass ratio of the functional filler to the radiation-resistant modified binder can be 1:0.5-1.2. This achieves an optimal balance between optical and mechanical properties. If the binder is insufficient, it cannot adequately coat the filler particles, resulting in decreased coating density and adhesion; if the filler is insufficient, the coating's diffuse reflectance of the solar spectrum will significantly decrease, failing to achieve the ultra-low absorption target.
[0026] This invention uses Ce 3+ / Ce 4+ Mixed valence ions are enriched in the silica-rich glassy shell on the filler surface, and Ce ions of the same valence are introduced into the binder, constructing a chemical bonding system between the filler and the binder, which significantly enhances radiation stability.
[0027] The following, combined with Figure 1 This document exemplifies a method for preparing a low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure. The preparation method may include the following steps: (1) Weigh the raw materials according to the functional filler group distribution ratio and mix them to obtain a mixture. Then melt, cast, anneal and cool to obtain a precursor glass. Next, nucleate and crystallize the precursor glass to obtain a microcrystalline glass block. After crushing, obtain functional filler powder. (2) Low modulus potassium silicate and silica sol are stirred and reacted to obtain high modulus potassium silicate solution, and then soluble cerium salt is added and mixed evenly to obtain radiation-resistant modified binder; (3) The functional filler powder is mixed evenly with the radiation-resistant modified binder to obtain a low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure.
[0028] In some embodiments, in step (1), the raw materials of the functional filler include the following components by molar percentage: ZnO 34-40%, SiO2 42-50%, Al2O3 8-12%, K2O 4-8%, CeO2 0.1-0.5%, and nucleating agent 0.5-1.5%, with the sum of the molar percentages of each component being 100%; preferably, the molar ratio of ZnO to SiO2 is 0.75-0.82, and the nucleating agent is selected from at least one of ZrO2, SnO2, and Y2O3. This ensures the stable formation of the α-Zn2SiO4 crystal phase.
[0029] In some embodiments, in step (1), the raw materials for the functional filler are mixed by ball milling at a speed of 250-500 r / min for 1-4 hours; preferably, the mixture is obtained by passing it through an 80-100 mesh sieve after ball milling.
[0030] In some embodiments, in step (1), the melting temperature is 1450-1550°C and the holding time is 1-3 hours.
[0031] If the melting temperature is too low, the glass batch will not melt sufficiently, resulting in high melt viscosity and inadequate component diffusion. This leads to uneven composition and unmelted particles, causing uneven nucleation and an incomplete core-shell structure during subsequent crystallization. If the temperature is too high, the volatilization of ZnO and K2O will be accelerated, causing the actual glass composition to deviate from the designed ratio, affecting the purity of the crystalline phase and the thickness of the shell. If the holding time is too short, the melt will not clarify sufficiently, leaving bubbles and streaks, resulting in poor glass uniformity. If the holding time is too long, it will also accelerate the volatilization of ZnO and K2O, and the high temperature will exacerbate the corrosion of the crucible, potentially introducing Al2O3 contamination. Controlling an appropriate melting regime can achieve an optimal window that balances sufficient melting and homogenization with suppressing component volatilization.
[0032] In some embodiments, in step (1), the annealing temperature is 500-550°C and the holding time is 1-2 hours.
[0033] If the annealing temperature is too low, atomic migration is insufficient, and the internal thermal stress of the glass cannot be fully released, making it prone to uneven crystallization or even cracking during subsequent crystallization. If the annealing temperature is too high, approaching the glass transition temperature, uncontrollable nucleation or phase separation may occur prematurely, interfering with subsequent controllable crystallization. If the holding time is too short, stress relief is insufficient; if the holding time is too long, prolonged holding at temperatures close to the glass transition temperature (Tg) also carries the risk of uncontrollable crystallization. Controlling the appropriate annealing regime can achieve an optimal window for both sufficient stress relief and prevention of premature crystallization.
[0034] In some implementations, in step (1), the cooling method can be slow cooling with the furnace.
[0035] In some embodiments, in step (1), the temperature of the nucleation treatment is 30-60°C higher than the initial temperature Tg of the precursor glass during glass transition, the time is 1-2 hours, and the heating rate is 5-10°C / minute; preferably, the Tg is 630-700°C.
[0036] The nucleation process was designed based on the kinetic requirements of controllable nucleation in glass-ceramics, and was determined after comprehensively considering nucleation density, phase selectivity, and grain size distribution. The nucleation temperature was set 30-60℃ above Tg. This range is in the supercooled liquid phase region with moderate viscosity, providing sufficient atomic mobility to achieve high-density uniform nucleation without causing a decrease in the nucleation rate or premature nucleus growth. Below this range, the viscosity is too high, resulting in insufficient nucleation; above it, the nucleation rate is too high and prone to runaway growth. The nucleation time of 1-2 hours aims to achieve saturated nucleus density. Too short a time results in insufficient nucleation, while too long a time leads to nucleus coarsening or phase transformation. The heating rate of 5-10℃ / min is used to quickly pass through the low-temperature region to avoid uncontrollable structural relaxation or precipitation of impurity phases, while ensuring a uniform temperature field to prevent thermal stress cracking. Glass systems with a Tg of 630-700℃ can obtain ideal number density and uniformly distributed crystal nuclei after being treated by this process, laying the foundation for subsequent crystallization treatment to form Zn2SiO4 grains of 50-200nm.
[0037] In some embodiments, in step (1), the temperature of the crystallization treatment is 20-50°C lower than the peak temperature Tp of the exothermic crystallization peak of the precursor glass (the crystallization peak temperature range determined by DSC test), the time is 2-8 hours, and the heating rate is 2-5°C / minute; preferably, the Tp is 800-850°C.
[0038] The crystallization process is designed to precisely control the growth kinetics and final size distribution of Zn₂SiO₄ grains. The crystallization temperature is set 20-50℃ below Tp, at the low-temperature side of the crystallization peak. At this temperature, the crystal growth driving force is moderate, effectively avoiding abnormal grain growth and size inhomogeneity near Tp due to excessively rapid growth rates. Too low a temperature hinders crystallization kinetics, while too high a temperature leads to grain coarsening, compromising nucleus transparency and core-shell structure integrity. A holding time of 2-8 hours ensures that the Zn₂SiO₄ phase is fully precipitated to the expected proportion. Too short a time results in incomplete crystallization and excessive residual glass phase, while too long a time can cause secondary crystallization or grain merging. The heating rate of 2-5℃ / min is gentler than during the nucleation stage, ensuring uniform thermal history within the large glass bulk and preventing localized overheating and thermal stress cracking caused by thermal hysteresis. Glass components with a Tp of 800-850℃, after being treated by this process, can obtain Zn2SiO4 crystal nuclei with a grain size of 50-200nm, uniformly distributed, and a shell structure with controllable thickness.
[0039] In some embodiments, in step (2), the modulus of low-modulus potassium silicate can be 2.0-3.0, the temperature of the stirring reaction can be 40-60℃, the time can be 2-6 hours, and the modulus of high-modulus potassium silicate can be 4.5-6.0.
[0040] In some embodiments, in step (2), the soluble cerium salt may include at least one of cerium nitrate, cerium acetate, or cerium chloride.
[0041] Furthermore, this invention also provides a method for preparing a thermal control coating using the aforementioned low-absorption, radiation-resistant thermal control white paint based on a Zn2SiO4@silicon-rich glass core-shell structure. Wherein, as... Figure 1 As shown, the preparation method may include the following steps: spraying the low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure onto the surface of the substrate, and curing it to obtain the low-absorption, radiation-resistant thermal control coating based on the Zn2SiO4@silicon-rich glass core-shell structure.
[0042] In some embodiments, the substrate may include aluminum alloy or stainless steel.
[0043] In some embodiments, before spraying the low-absorption, radiation-resistant thermally controlled white paint based on the Zn2SiO4@silicon-rich glass core-shell structure, distilled water can be added to adjust the viscosity of the Forte 4 cup to 30-40 seconds and then passed through a 200-mesh sieve.
[0044] In some embodiments, the spraying pressure is 0.2-0.3 MPa, and the spraying is performed in 3-6 applications, with each application spaced at least 30 minutes apart for surface drying.
[0045] In some embodiments, the curing may include room temperature static curing and heat curing; preferably, the room temperature static curing time may be 12-24 hours, and the heat curing temperature may be 80-120°C, and the time may be 2-12 hours.
[0046] In some embodiments, the thickness of the coating is controlled to be 120-200 μm.
[0047] The preparation method provided by this invention results in a cured coating in which the silicon-rich glassy phase shell on the surface of the functional filler is chemically bonded to the potassium silicate matrix via Si-O-Si covalent bonds.
[0048] In some embodiments, the coating adhesion is rated as Grade 1 according to the cross-cut adhesion test, and shows no cracking or peeling after 150 thermal cycles at -150 to +150°C; the coating has a solar absorptivity α in the visible light band of 250-2500 nm. s ≤0.06, the change in solar absorptivity Δα after 5000 equivalent solar hours (ESH) of vacuum ultraviolet irradiation.s ≤+0.04.
[0049] In summary, this invention has the following significant advancements compared to existing technologies: 1. Using in-situ grown core-shell Zn2SiO4@SiO2 microcrystalline glass as a functional filler, and utilizing the chemical affinity between its surface silicon-rich glassy shell and potassium silicate, the filler and binder are chemically bonded together: This invention uses in-situ grown core-shell Zn2SiO4@SiO2 microcrystalline glass as a functional filler. Compared to traditional externally coated core-shell fillers, the silicon-rich glassy shell of this filler is spontaneously formed during crystallization due to thermodynamically driven component differentiation. The growth of Zn2SiO4 crystals consumes Zn from the surrounding matrix. 2+ This process automatically enriches SiO2 in the crystal front region, forming a silicon-rich glassy phase that tightly encapsulates the grain surface. The shell and crystal nucleus form a continuous glassy phase transition interface with chemical bonding, without any physical abrupt boundary. This fundamentally solves the problem of weak bonding between the shell and crystal nucleus interface in external coating schemes. More importantly, the surface of this filler's silicon-rich glassy phase shell is rich in Si-OH active groups, giving it unique surface chemical conditions for chemical bonding with potassium silicate binder. This is unlike existing ZnO fillers (without Si-OH on the surface), solid-phase Zn2SiO4 fillers (with exposed crystal faces), and externally coated core-shell fillers (shell surface...). Unlike existing physically embedded coatings, this invention utilizes the surface chemical properties of in-situ grown core-shell fillers to achieve chemical bonding between the filler and binder. This process involves a co-condensation reaction between the Si-OH groups on the filler surface and the Si-OH groups of potassium silicate during coating curing, forming Si-O-Si covalent bonds. This elevates the filler from traditional "physical embedding" to "chemical anchoring" within the three-dimensional network of the coating. This invention is the first to utilize the surface chemical properties of in-situ grown core-shell fillers to achieve chemical bonding between the filler and binder. Unlike existing physically embedded coatings, this invention eliminates optical discontinuities at the interface due to chemical bonding. The solar absorptivity of the coating is essentially consistent with that of the filler powder, and the α-coating characteristic of traditional physically embedded coatings is absent. s Significantly higher than the α of the filler powder s The phenomenon of... 2. Simultaneously introducing Ce into both the filler shell and the binder matrix to achieve a dual-channel spatial distribution of the full coating with radiation protection function: This invention introduces soluble cerium salt into the binder, so that the cured potassium silicate matrix also contains Ce. 3+ / Ce 4+The variable-valence ions, combined with the Ce ions already enriched in the filler shell, form a dual-channel spatial synergistic distribution system of "Ce in the filler shell (first line of defense) + Ce in the binder matrix (second line of defense)". The Ce in the filler shell captures electrons and holes generated by irradiation at a position close to the Zn2SiO4 crystal nucleus, while the Ce in the binder matrix provides continuous supplementary protection in the binder region between filler particles. The two lines of defense are spatially continuous and completely eliminate the "vacuum zone" of irradiation protection at the filler / binder interface region in the traditional scheme. This invention achieves for the first time a uniform spatial distribution of Ce in the entire coating (filler shell + binder matrix), and the irradiation protection effect has a synergistic gain. The ultraviolet irradiation degradation of the dual-channel Ce distribution coating is significantly lower than that of the coating containing only Ce in the filler.
[0050] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections within the range based on the description herein, and are not intended to be limited to the specific values in the examples below. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.
[0051] Example 1 The method for preparing low-absorption, radiation-resistant thermally controlled white paint / coating based on Zn2SiO4@silicon-rich glass core-shell structure provided in this embodiment includes the following steps: (1) Preparation of functional fillers: The precursor glass was prepared according to the following molar percentages: ZnO 37.0%, SiO2 46.0%, Al2O3 10.0%, K2O 5.5%, CeO2 0.3%, ZrO2 1.2%, with the sum of each component being 100% and the ZnO / SiO2 molar ratio being 0.804. After conversion by mass percentage, the raw materials were weighed as follows: zinc oxide (ZnO, AR, ≥99.0%), silicon dioxide (SiO2, 200 mesh, AR, ≥99.5%), aluminum hydroxide (Al(OH)3, AR, ≥99.0%), anhydrous potassium carbonate (K2CO3, AR, ≥99.0%), cerium oxide (CeO2, 99.9%), and zirconium dioxide (ZrO2, AR, ≥99.0%). All raw materials were added to a zirconium oxide ball mill jar with a ball-to-material ratio of 3:1 and milled at 250°C. Dry ball milling at rpm for 4 hours, and passing through a 100-mesh sieve to obtain a mixture; the mixture is loaded into an alumina crucible (pre-fired at 1100℃ for 2 hours to remove gas), melted at 1480℃ for 2.5 hours, and after the melt is cooled to 1360℃, it is poured into a graphite mold preheated to 250℃, and quickly transferred to a muffle furnace at 520℃ for annealing for 2 hours, and slowly cooled to room temperature with the furnace at a rate of 2℃ / min to obtain the precursor glass; The precursor glass powder was subjected to DSC analysis at 10℃ / min. The DSC curve showed that Tg = 642℃, Tp = 838℃, the nucleation temperature was set to Tg+53℃=695℃, and the crystallization temperature was set to Tp-28℃=810℃. The temperature was increased to 695℃ at 5℃ / min and held for 1.5 hours, then increased to 810℃ at 3℃ / min and held for 4 hours. The mixture was then cooled to room temperature in the furnace to obtain the microcrystalline glass bulk. Microcrystalline glass blocks were coarsely crushed to <5 mm, wet-milled in anhydrous ethanol for 6 hours (350 rpm), and dried at 80°C for 12 hours to obtain the functional filler. This filler exhibits a solar absorbance ratio α... s =0.05, Ce is enriched in the shell. 3+ / Ce 4+ Mixed valence ions; (2) Preparation of modified binder: 50 g of low-modulus potassium silicate solution (modulus 2.8, solid content 30 wt%) was added to the reactor, and 25 g of silica sol (SiO2 content 30 wt%) was slowly added under stirring. The reaction was carried out at 50℃ for 2 hours to obtain a high-modulus potassium silicate solution with a modulus of about 5.2. 0.35 g of cerium nitrate (Ce(NO3)3·6H2O, accounting for about 1.5 wt% of the potassium silicate solid content based on CeO2) was added and stirred until dissolved evenly to obtain a Ce-containing binder. 3+ / Ce 4+ Modified potassium silicate aqueous solution; (3) White paint preparation and coating preparation: 30 g of functional filler powder was added to distilled water and ultrasonically dispersed for 10 minutes. 25 g of modified binder solution was added and stirred for 15 minutes (the mass ratio of filler to binder is about 1:0.8) to obtain a low-absorption, radiation-resistant heat-controlled white paint based on Zn2SiO4@silicon-rich glass core-shell structure. Distilled water was added to adjust the viscosity of the Forte 4 cup to 30-40 seconds, and the mixture was passed through a 200-mesh sieve to obtain a thermally controlled white paint slurry. An aluminum alloy substrate (50×50×1 mm, pre-cleaned with acetone and sandblasted) was fixed on a spraying table, and the slurry was sprayed evenly onto the substrate surface at a pressure of 0.3 MPa. The slurry was sprayed in 6 coats, with a 30-minute interval between each coat. After spraying, the coating was allowed to cure at room temperature for 24 hours, and then heated at 80℃ for 12 hours. The coating thickness was controlled at 120-150 μm to obtain the low-absorption, radiation-resistant thermally controlled coating based on the Zn2SiO4@silicon-rich glass core-shell structure.
[0052] Example 2 The preparation method of the low-absorption, radiation-resistant thermally controlled white paint and coating based on Zn2SiO4@silicon-rich glass core-shell structure provided in this embodiment is the same as in Example 1, with the main difference being: In step (1), the nucleating agent is replaced by SnO2 instead of ZrO2.
[0053] Comparative Example 1 The preparation methods for the white paint and coating provided in this comparative example are the same as in Example 1, with the main difference being: In step (1), the precursor glass composition of the functional filler does not contain CeO2 and is prepared with ZnO 37.0%, SiO2 46.0%, Al2O3 10.3%, K2O 5.5%, and ZrO2 1.2%. In step (2), cerium nitrate is not added to the modified binder.
[0054] Comparative Example 2 The preparation methods for the white paint and coating provided in this comparative example are the same as in Example 1, with the main difference being: In step (2), cerium nitrate is not added to the modified binder.
[0055] Comparative Example 3 The preparation methods for the white paint and coating provided in this comparative example are the same as in Example 1, with the main difference being: In step (1), the precursor glass composition of the functional filler does not contain CeO2 and is prepared with ZnO 37.0%, SiO2 46.0%, Al2O3 10.3%, K2O 5.5%, and ZrO2 1.2%.
[0056] Comparative Example 4 The preparation methods for the white paint and coating provided in this comparative example are the same as in Example 1, with the main difference being: In step (1), Zn2SiO4 powder synthesized by solid-state method (ZnO and SiO2 calcined at 1050℃ for 3 hours in a molar ratio of 2:1 and ball-milled to D50≈2.5μm) is used as filler; In step (2), the adhesive used is a common high-modulus potassium silicate solution without Ce modification (modulus 5.2 but without cerium nitrate).
[0057] Table 1 below compares the performance test results of the coatings prepared in Examples 1 and 2 with those in Comparative Examples 1-4: .
[0058] As can be seen from Table 1 above, the effectiveness and synergistic necessity of the three major technical features of this invention have been systematically verified. Regarding Ce dual-channel protection, after 5000 ESH ultraviolet irradiation, Δα in Examples 1-2... s Only 0.03-0.04, while the Δα of Comparative Example 1 (no Ce), Comparative Example 2 (filler only containing Ce), and Comparative Example 3 (binder only containing Ce) was much higher. s The values were 0.05, 0.05, and 0.05 respectively, all significantly worse than the example, demonstrating that the single-channel Ce protection is insufficient due to incomplete coverage of the irradiated area. Only a dual-channel spatially coordinated distribution can achieve efficient annihilation of electron-hole pairs across the entire coating area. Regarding the core-shell structure and chemical bonding interface, the initial α of the example... s As low as 0.06, with an absorption ratio of 0.066, while Comparative Example 4 (solid-phase Zn2SiO4 ordinary filler combined with unmodified binder, without core-shell structure and chemical bonding) had an initial α s The Si-O-Si covalent bonds, reaching 0.10 and an absorption ratio of 0.111, demonstrate that the Si-O-Si covalent bonds effectively eliminate interfacial scattering losses in the physical embedding mode. Regarding interfacial bonding strength, the example showed no cracking or peeling after 150 thermal cycles, with adhesion at grade 1, while Comparative Example 4 exhibited microcracks and adhesion decreased to grade 2. This indicates that the continuous transition interface of the core-shell structure and chemical bonding together provide excellent thermal expansion matching and thermal shock resistance. After eliminating any channel of the Ce dual-channel in Comparative Examples 1-3, the irradiation stability decreased. In Comparative Example 4, after eliminating both the core-shell structure and chemical bonding, the optical and mechanical properties deteriorated comprehensively. Both positive and negative examples demonstrate that each core technical feature of this invention is indispensable for achieving an ultra-low absorption, radiation-resistant, and highly reliable thermally controlled coating.
[0059] Figure 2The image shows the X-ray diffraction pattern of the functional filler powder prepared in Example 1. As can be seen from the image, the positions of the diffraction peaks in the XRD pattern of the functional filler prepared in Example 1 match the Zn2SiO4 standard card (PDF#37-1485), and no diffraction peaks of other crystalline phases (such as ZnO, SiO2, or CeO2) were detected. This indicates that after controlled crystallization treatment, the precursor glass has been fully precipitated with a pure α-Zn2SiO4 crystalline phase, demonstrating good phase selectivity.
[0060] Figure 3 The images show scanning electron micrographs of the functional filler powder prepared in Example 1. As can be seen from the images, the scanning electron microscope clearly reveals a complete core-shell structure: the internal structure consists of Zn₂SiO₄ crystal nuclei, with an outer silicon-rich glass shell transitioning through a continuous interface. The core-shell boundaries are clear and complete, without cracks or peeling, and the size distribution is uniform, with no abnormal growth or particle adhesion observed. This microstructure confirms the precise control of nucleation density and crystal growth by the controlled crystallization process.
[0061] Figure 4 This is a comparison of the UV-Vis-NIR diffuse reflectance spectra of the coating prepared in Example 1. As can be seen from the figure, the coating exhibits extremely high diffuse reflectance across the entire main energy band of the solar spectrum (250-2500 nm), with a reflectance exceeding 90% in the ultraviolet band (250-380 nm). Based on the ASTM E490 standard solar spectrum weighted integral, the solar absorptivity α... s It is only 0.06.
[0062] Figure 5 The image shows a scanning electron microscope (SEM) image of the coating prepared in Example 1. As can be seen from the image, the coating surface is smooth and dense, the filler particles are uniformly dispersed in the binder matrix without agglomeration, the particles are tightly packed together, and there are very few microscopic defects such as pores and cracks. The interface between the filler particles and the potassium silicate binder is blurred with no obvious gaps, providing direct experimental evidence at the microstructural level for the coating to achieve ultra-low solar absorptivity, excellent adhesion, and resistance to thermal cycling cracking.
[0063] Figure 6 The image shows an adhesion test photograph of the coating prepared in Example 1. As can be seen from the image, a small amount of coating peeled off at the intersection of the coating cuts, with the affected area ≤5%. The edges of the cuts are basically smooth but not completely free of peeling. The coating adhesion is judged to be level 1.
[0064] Although the present invention has been described in detail through the preferred embodiments above, it should be understood that the above description should not be considered as a limitation of the present invention. Various modifications and substitutions to the present invention will be apparent to those skilled in the art after reading the above description. Therefore, the scope of protection of the present invention should be defined by the appended claims.
Claims
1. A low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure, characterized in that, The components of the low-absorption, radiation-resistant thermally controlled white paint based on Zn2SiO4@silicon-rich glass core-shell structure include: functional fillers and radiation-resistant modified binders. The functional filler includes in-situ precipitated core-shell structured Zn2SiO4@SiO2 microcrystalline glass; The radiation-resistant modified binder includes a Ce-modified potassium silicate aqueous solution.
2. The low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure according to claim 1, characterized in that, The core-shell structured Zn2SiO4@SiO2 microcrystalline glass uses Zn2SiO4 as the crystal nucleus and a silicon-rich glassy SiO2 phase as the shell, with a continuous glassy phase transition interface between the shell and the crystal nucleus; preferably, the shell is enriched with Ce. 3+ and Ce 4+ Ce ions in mixed valence states.
3. The low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure according to claim 1 or 2, characterized in that, The particle size D50 of the core-shell structured Zn2SiO4@SiO2 microcrystalline glass filler is 1-5 μm; preferably, the particle size of the crystal nucleus is 50-200 nm, and the thickness of the silicon-rich glass SiO2 phase shell is 100-300 nm. Preferably, in the Ce-modified potassium silicate aqueous solution, CeO2 accounts for 0.5-1.5 wt% of the potassium silicate solid content.
4. The low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure according to any one of claims 1-3, characterized in that, The mass ratio of the functional filler to the radiation-resistant modified binder is 1:0.5-1.
2.
5. A method for preparing a low-absorption, radiation-resistant thermally controlled white paint based on a Zn2SiO4@silicon-rich glass core-shell structure as described in any one of claims 1-4, characterized in that, The preparation method includes the following steps: (1) Weigh the raw materials according to the functional filler group distribution ratio and mix them to obtain a mixture. Then melt, cast, anneal and cool to obtain a precursor glass. Next, nucleate and crystallize the precursor glass to obtain a microcrystalline glass block. After crushing, obtain functional filler powder. (2) Low modulus potassium silicate and silica sol are stirred and reacted to obtain high modulus potassium silicate solution, and then soluble cerium salt is added and mixed evenly to obtain radiation-resistant modified binder; (3) The functional filler powder is mixed evenly with the radiation-resistant modified binder to obtain a low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure.
6. The preparation method according to claim 5, characterized in that, In step (1), the raw materials of the functional filler include the following components by molar percentage: ZnO 34-40%, SiO2 42-50%, Al2O3 8-12%, K2O 4-8%, CeO2 0.1-0.5%, nucleating agent 0.5-1.5%, and the sum of the molar percentages of each component is 100%. Preferably, the molar ratio of ZnO to SiO2 is 0.75-0.82, and the nucleating agent is selected from at least one of ZrO2, SnO2, and Y2O3.
7. The preparation method according to claim 5 or 6, characterized in that, In step (1), the melting temperature is 1450-1550℃, and the holding time is 1-3 hours; Preferably, the annealing temperature is 500-550℃, and the holding time is 1-2 hours.
8. The preparation method according to any one of claims 5-7, characterized in that, The nucleation treatment temperature is 30-60°C higher than the initial glass transition temperature (Tg) of the precursor glass, the treatment time is 1-2 hours, and the heating rate is 5-10°C / minute; preferably, the Tg is 630-700°C. The crystallization treatment temperature is 20-50°C lower than the peak temperature Tp of the exothermic crystallization peak of the precursor glass, the time is 2-8 hours, and the heating rate is 2-5°C / minute; preferably, the Tp is 800-850°C.
9. The preparation method according to any one of claims 5-8, characterized in that, In step (2), the modulus of low-modulus potassium silicate is 2.0-3.0, the temperature of the stirring reaction is 40-60℃, the time is 2-6 hours, and the modulus of high-modulus potassium silicate is 4.5-6.
0. Preferably, the soluble cerium salt includes at least one of cerium nitrate, cerium acetate, or cerium chloride.
10. A method for preparing a thermal control coating using a low-absorption, radiation-resistant thermal control white paint based on a Zn2SiO4@silicon-rich glass core-shell structure as described in any one of claims 1-4, characterized in that, The preparation method includes the following steps: spraying the low-absorption, radiation-resistant thermal control white paint based on the Zn2SiO4@silicon-rich glass core-shell structure onto the surface of the substrate, and curing it to obtain the low-absorption, radiation-resistant thermal control coating based on the Zn2SiO4@silicon-rich glass core-shell structure.