Preparation method of high-temperature-resistant fireproof heat-preservation heat-insulation coating of oil storage tank

By introducing a variety of components and modification treatments into the petroleum storage tank coating, the problem of coating aging and uniform coating difficulty is solved, high durability and uniformity are achieved, and fire resistance, insulation and thermal insulation performance is significantly improved.

CN118978820APending Publication Date: 2024-11-19SICHUAN FIRE RES INST OF MEM

Patent Information

Application Number
CN202411346715.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing high-temperature, fire-resistant, thermal insulation coatings are prone to aging and cracking in harsh environments, which are difficult to construct and have great challenges in uniform coating, especially in complex structural storage tanks.

Method used

Using components such as inorganic silicate binder, alumina nanoparticles, hollow glass microbeads, magnesium hydroxide, silicone resin, shape memory polymer, graphene composite materials and ceramic fibers, etc., through modification and layer-by-layer Construction, form a high-performance fireproof, thermal insulation coating to enhance the durability and uniformity of the coating.

Benefits of technology

It significantly improves the durability and protection of the coating, enhances high-temperature resistance, impact resistance and mechanical strength, ensures the uniformity and thermal insulation of the coating, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978820A_ABST
    Figure CN118978820A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-temperature-resistant fireproof heat-preservation heat-insulation coating of an oil storage tank, and relates to the field of fireproof heat-preservation heat-insulation coatings. The high-temperature-resistant fireproof thermal-insulation coating based on the oil storage tank comprises 25-35% of an inorganic silicate binder used for forming a tough base layer and remarkably enhancing the durability of the coating, and the binder comprises a mixture of potassium silicate and lithium silicate so as to further improve the chemical corrosion resistance of the coating. Various components such as the inorganic silicate binder, the aluminum oxide nanoparticles, the shape memory polymer and the ceramic fibers are introduced into the coating, the durability and the protection capacity of the coating are remarkably improved, the inorganic silicate binder is composed of a mixture of potassium silicate and lithium silicate, a tough base layer is formed, and the durability and the protection capacity of the coating are improved. The chemical corrosion resistance is excellent; after the aluminum oxide nanoparticles are modified, the compatibility of the aluminum oxide nanoparticles and the organic silicon resin is enhanced, and excellent high-temperature tolerance and impact resistance are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fireproof heat-insulating coatings, and in particular to a method for preparing a high-temperature resistant fireproof heat-insulating coating for a petroleum storage tank. Background Art

[0002] Oil storage tanks play a key role in the petrochemical industry. In order to ensure their safety in extreme environments, fireproof and heat-insulating coatings are essential. The coatings can not only effectively prevent high-temperature flames from directly damaging the tank structure, but also reduce heat conduction, thereby extending the tank's endurance time in a fire and providing valuable rescue time. In addition, these coatings also have a heat-insulating effect, which can keep the internal temperature of the tank relatively stable in an environment with extreme temperature changes, reducing energy loss.

[0003] Although the existing high temperature resistant fireproof thermal insulation coatings have played an important role in practical applications, there are still some defects that cannot be ignored. The durability of the coating. After being exposed to harsh environments for a long time, the coating may age and crack, resulting in a decrease in the protective effect. The construction is difficult, especially on storage tanks with complex structures, and uniform coating is challenging. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-temperature resistant, fireproof, thermal insulation coating for petroleum storage tanks, which solves the problem of durability of the coating and the challenge of uniform coating.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A high temperature resistant fireproof thermal insulation coating for a petroleum storage tank, comprising:

[0006] Inorganic silicate binder: 25-35%, used to form a strong base layer, significantly enhancing the durability of the coating. The binder includes a mixture of potassium silicate and lithium silicate to further improve the coating's resistance to chemical corrosion;

[0007] Alumina nanoparticles: 15-25%. The ultrafine particle design provides excellent high temperature resistance and improves the impact resistance of the coating. The surface of the alumina nanoparticles is modified to enhance its compatibility with silicone resin, thereby improving the overall performance of the coating.

[0008] Hollow glass microspheres: 10-20%, which improve the thermal insulation effect of the coating by reducing the density and thermal conductivity of the coating and make the coating process more uniform;

[0009] Magnesium hydroxide: 8-12%, its highly effective flame retardancy ensures the coating’s ability to protect itself in a fire while reducing the release of harmful gases;

[0010] Silicone resin: 7-10%, with excellent flexibility and adhesion, enabling the coating to adapt to the thermal expansion and contraction of the tank in extreme environments, preventing cracking and falling off;

[0011] Shape memory polymers: 3-7%, which can undergo phase change under high temperature conditions, thereby forming an additional protective layer on the surface of the tank, enhancing fire resistance, and autonomously adjust their shape under high temperature conditions to ensure optimal protection at different temperatures;

[0012] Graphene composite material: 1-3%, enhances the conductivity and UV resistance of the coating, extends the service life of the coating, and gives the coating a certain antistatic function, thereby reducing the risk of fire in flammable environments;

[0013] Ceramic fiber: 2-5%, provides additional mechanical strength, enables the coating to withstand external impact and wear, and prolongs service life.

[0014] Preferably, the inorganic silicate binder comprises a mixture of potassium silicate and lithium silicate, and the surface of the aluminum oxide nanoparticles is modified to enhance their compatibility with the silicone resin.

[0015] Preferably, the coating further comprises 0.5-2% of nano titanium dioxide to improve the UV resistance and self-cleaning performance of the coating.

[0016] A method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank comprises the following steps:

[0017] S1. Weigh potassium silicate and lithium silicate in a weight percentage of 25-35%, and mix them evenly to form a binder base solution;

[0018] S2, weighing 15-25% of aluminum oxide nanoparticles by weight, soaking them in a surface modifier solution to ensure that the surface of the particles is evenly coated, and then drying them, weighing 10-20% of hollow glass microspheres by weight, and ensuring that there are no impurities on the surface of the microspheres to ensure the uniformity and thermal insulation performance of the coating, weighing 8-12% of magnesium hydroxide by weight, and mixing it with an appropriate amount of water, and stirring until it is evenly dispersed;

[0019] S3, weigh 7-10% by weight of organic silicon resin, add appropriate amount of solvent, and stir until uniform;

[0020] S4, weighing 3-7% of the shape memory polymer by weight and mixing it with the silicone resin solution to ensure the adjustability of the coating at high temperature;

[0021] S5, weighing 1-3% of the graphene composite material by weight, mixing it with the silicone resin, and stirring evenly;

[0022] S6. Weigh 2-5% of the ceramic fiber by weight and ensure that its length is moderate to enhance the mechanical strength of the coating;

[0023] S7, adding an inorganic silicate binder, aluminum oxide nanoparticles, hollow glass microspheres, magnesium hydroxide, a silicone resin solution, a shape memory polymer, a graphene composite material and ceramic fibers to a stirring tank in sequence, and stirring evenly until a homogeneous coating mixture is formed;

[0024] S8, weighing 0.5-2% by weight of nano titanium dioxide, slowly adding it to the mixed solution, and continuing to stir to enhance the UV resistance and self-cleaning performance of the coating;

[0025] S9. Use spraying, brushing or rolling to evenly apply the coating on the surface of the oil storage tank, control the thickness of the coating, ensure uniform coverage, and perform high-temperature curing treatment on the coated tank in an environment of 200°C to further enhance the durability, fire resistance and mechanical strength of the coating.

[0026] Preferably, the surface modification of the aluminum oxide nanoparticles is completed by using a silane coupling agent to further enhance the bonding force between the particles and the binder, the particle size of the hollow glass microspheres is 30-100 microns to ensure the best thermal insulation effect and coating uniformity, and the mixing ratio of the magnesium hydroxide to water is 1:2 to ensure the best dispersibility and flame retardant effect of the flame retardant.

[0027] Preferably, the length of the ceramic fibers is controlled within a range of 2-5 mm to ensure their dispersion and reinforcement in the coating, and the thickness of the coating is controlled within a range of 1-3 mm to ensure optimal protective performance.

[0028] Preferably, the high temperature curing time of the coating is 1-2 hours to ensure that the coating is fully cured and achieves optimal performance.

[0029] Preferably, the coating is subjected to an ultraviolet aging test to verify its anti-aging properties.

[0030] The present invention provides a method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank. It has the following beneficial effects:

[0031] The present invention significantly improves the durability and protective ability of the coating by introducing multiple components such as inorganic silicate binder, aluminum oxide nanoparticles, shape memory polymer and ceramic fiber into the coating. The inorganic silicate binder is composed of a mixture of potassium silicate and lithium silicate, forming a strong base layer and having excellent resistance to chemical corrosion; after the aluminum oxide nanoparticles are modified, their compatibility with silicone resin is enhanced, providing excellent high temperature tolerance and impact resistance; the shape memory polymer can undergo phase change under high temperature conditions to form an additional protective layer and enhance the fire resistance; the addition of ceramic fiber significantly improves the mechanical strength of the coating, enabling it to better withstand external impact and wear, thereby extending the service life of the coating.

[0032] The technical solution of the present invention pays special attention to the uniform coating problem. By introducing hollow glass microspheres, nano-titanium dioxide and other optimization treatment methods, the density and fluidity of the coating are effectively improved, thereby improving the uniformity during the coating process. The hollow glass microspheres reduce the density of the coating, improve the heat insulation effect, and ensure the uniformity of coverage during coating; the addition of nano-titanium dioxide not only enhances the UV resistance and self-cleaning performance of the coating, but also makes the coating easier to apply evenly. In addition, by strictly controlling the coating process, such as layer-by-layer construction and high-temperature curing treatment, the uniformity and overall performance of the coating are further ensured. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] like Figure 1 As shown, an embodiment of the present invention provides a high temperature resistant fireproof heat insulation coating for a petroleum storage tank, comprising: an inorganic silicate binder: 25-35%, used to form a tough base layer, significantly enhancing the durability of the coating, the binder comprises a mixture of potassium silicate and lithium silicate to further improve the chemical corrosion resistance of the coating, the inorganic silicate binder comprises a mixture of potassium silicate and lithium silicate, and the surface of the aluminum oxide nanoparticles is modified to enhance its compatibility with the silicone resin;

[0036] Alumina nanoparticles: 15-25%. The ultrafine particle design provides excellent high temperature resistance and improves the impact resistance of the coating. The surface of the alumina nanoparticles is modified to enhance its compatibility with silicone resin, thereby improving the overall performance of the coating.

[0037] Hollow glass microspheres: 10-20%, which improve the thermal insulation effect of the coating by reducing the density and thermal conductivity of the coating and make the coating process more uniform;

[0038] Magnesium hydroxide: 8-12%, its highly effective flame retardancy ensures the coating’s ability to protect itself in a fire while reducing the release of harmful gases;

[0039] Silicone resin: 7-10%, with excellent flexibility and adhesion, enabling the coating to adapt to the thermal expansion and contraction of the tank in extreme environments, preventing cracking and falling off;

[0040] Shape memory polymers: 3-7%, which can undergo phase change under high temperature conditions, thereby forming an additional protective layer on the surface of the tank, enhancing fire resistance, and autonomously adjust their shape under high temperature conditions to ensure optimal protection at different temperatures;

[0041] Graphene composite material: 1-3%, enhances the conductivity and UV resistance of the coating, extends the service life of the coating, and gives the coating a certain antistatic function, thereby reducing the risk of fire in flammable environments;

[0042] Ceramic fiber: 2-5%, provides additional mechanical strength, enables the coating to withstand external impact and wear, and prolongs its service life. The coating also includes 0.5-2% nano titanium dioxide to improve the coating's UV resistance and self-cleaning properties.

[0043] A method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank comprises the following steps:

[0044] S1. Weigh potassium silicate and lithium silicate in a weight percentage of 25-35%, and mix them evenly to form a binder base solution;

[0045] S2, weighing 15-25% of aluminum oxide nanoparticles by weight, soaking them in a surface modifier solution to ensure that the surface of the particles is evenly coated, and then drying them, weighing 10-20% of hollow glass microspheres by weight, and ensuring that there are no impurities on the surface of the microspheres to ensure the uniformity and thermal insulation performance of the coating, weighing 8-12% of magnesium hydroxide by weight, and mixing it with an appropriate amount of water, stirring until it is evenly dispersed, and the surface modification of the aluminum oxide nanoparticles is completed by using a silane coupling agent to further enhance the bonding force between the particles and the binder;

[0046] S3, weigh 7-10% by weight of organic silicon resin, add appropriate amount of solvent, and stir until uniform;

[0047] S4, weighing 3-7% of the shape memory polymer by weight and mixing it with the silicone resin solution to ensure the adjustability of the coating at high temperature;

[0048] S5, weighing 1-3% of the graphene composite material by weight, mixing it with the silicone resin, and stirring evenly;

[0049] S6. Weigh ceramic fibers at a weight percentage of 2-5%, and ensure that the length is moderate to enhance the mechanical strength of the coating. The length of the ceramic fibers is controlled at 2-5 mm to ensure their dispersion and reinforcement in the coating;

[0050] S7. Add inorganic silicate binder, alumina nanoparticles, hollow glass microspheres, magnesium hydroxide, silicone resin solution, shape memory polymer, graphene composite material and ceramic fiber into a stirring tank in sequence, and stir evenly until a homogeneous coating mixture is formed. The particle size of the hollow glass microspheres is 30-100 microns to ensure the best thermal insulation effect and coating uniformity. The mixing ratio of magnesium hydroxide to water is 1:2 to ensure the best dispersibility and flame retardant effect of the flame retardant.

[0051] S8, weighing 0.5-2% by weight of nano titanium dioxide, slowly adding it to the mixed solution, and continuing to stir to enhance the UV resistance and self-cleaning performance of the coating;

[0052] S9. Use spraying, brushing or rolling to evenly apply the coating on the surface of the oil storage tank, control the thickness of the coating to ensure uniform coverage, and perform high-temperature curing treatment on the coated tank in an environment of 200°C to further enhance the durability, fire resistance and mechanical strength of the coating. The coating thickness is controlled at 1-3 mm to ensure the best protective performance. The high-temperature curing time of the coating is 1-2 hours to ensure that the coating is fully cured and achieves the best performance. The coating is subjected to UV aging test to verify its anti-aging performance.

[0053] Table 1: Data comparison table

[0054]

[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high temperature resistant fireproof thermal insulation coating for petroleum storage tanks, characterized in that: include: Inorganic silicate binder: 25-35%, used to form a strong base layer; Alumina nanoparticles: 15-25%, its ultra-fine particle design can provide excellent high temperature resistance performance; Hollow glass microspheres: 10-20%, by reducing the density and thermal conductivity of the coating; Magnesium hydroxide: 8-12%, its highly effective flame retardancy ensures the coating’s ability to protect itself in a fire while reducing the release of harmful gases; Silicone resin: 7-10%, with excellent flexibility and adhesion, enabling the coating to adapt to the thermal expansion and contraction of the tank in extreme environments, preventing cracking and falling off; Shape memory polymers: 3-7%, which can undergo phase changes under high temperature conditions to form an additional protective layer on the tank surface; Graphene composites: 1-3%, enhancing the conductivity and UV resistance of the coating; Ceramic fiber: 2-5%, provides additional mechanical strength, enabling the coating to withstand external impact and abrasion.

2. The high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 1, characterized in that: The inorganic silicate binder comprises a mixture of potassium silicate and lithium silicate, and the surface of the aluminum oxide nanoparticles is modified to enhance the compatibility with the organic silicone resin.

3. The high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 1, characterized in that: The coating also includes 0.5-2% of nano titanium dioxide to improve the coating's UV resistance and self-cleaning properties.

4. A method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank, characterized in that: The following steps are involved: S1. Weigh potassium silicate and lithium silicate in a weight percentage of 25-35%, and mix them evenly to form a binder base solution; S2. Weigh 15-25% of aluminum oxide nanoparticles by weight, soak them in a surface modifier solution to ensure that the surface of the particles is evenly coated, and then dry them. Weigh 10-20% of hollow glass microspheres by weight, and ensure that there are no impurities on the surface of the microspheres to ensure the uniformity and thermal insulation performance of the coating. Weigh 8-12% of magnesium hydroxide by weight, mix it with an appropriate amount of water, and stir until it is evenly dispersed. S3, weigh 7-10% by weight of organic silicon resin, add appropriate amount of solvent, and stir until uniform; S4, weighing 3-7% of the shape memory polymer by weight and mixing it with the silicone resin solution to ensure the adjustability of the coating at high temperature; S5, weighing 1-3% of the graphene composite material by weight, mixing it with the silicone resin, and stirring evenly; S6. Weigh 2-5% of the ceramic fiber by weight and ensure that its length is moderate to enhance the mechanical strength of the coating; S7, adding an inorganic silicate binder, aluminum oxide nanoparticles, hollow glass microspheres, magnesium hydroxide, a silicone resin solution, a shape memory polymer, a graphene composite material and ceramic fibers to a stirring tank in sequence, and stirring evenly until a homogeneous coating mixture is formed; S8, weighing 0.5-2% by weight of nano titanium dioxide, slowly adding it to the mixed solution, and continuing to stir to enhance the UV resistance and self-cleaning performance of the coating; S9. Use spraying, brushing or rolling to evenly apply the coating on the surface of the oil storage tank, control the thickness of the coating, ensure uniform coverage, and perform high-temperature curing treatment on the coated tank in an environment of 200°C to further enhance the durability, fire resistance and mechanical strength of the coating.

5. The method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 4, characterized in that: The surface modification of the aluminum oxide nanoparticles is completed by using a silane coupling agent to further enhance the bonding force between the particles and the binder. The particle size of the hollow glass microspheres is 30-100 microns to ensure the best thermal insulation effect and coating uniformity. The mixing ratio of the magnesium hydroxide to water is 1:2 to ensure the best dispersibility and flame retardant effect of the flame retardant.

6. The method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 4, characterized in that: The length of the ceramic fiber is controlled within 2-5 mm to ensure its dispersion and reinforcement in the coating, and the thickness of the coating is controlled within 1-3 mm to ensure optimal protective performance.

7. The method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 4, characterized in that: The high temperature curing time of the coating is 1-2 hours to ensure that the coating is fully cured and achieves optimal performance.

8. The method for preparing a high temperature resistant fireproof thermal insulation coating for a petroleum storage tank according to claim 4, characterized in that: The coating was subjected to UV aging test to verify its anti-aging performance.

Citation Information

Patent Citations

  • Total-effect gel heat insulation coating and preparation method thereof

    CN117363060A

  • Heat insulation coating with high temperature resistance and low heat conductivity coefficient and preparation method thereof

    CN117363139A

Cited By

  • High-temperature-resistant sealing coating and preparation method thereof

    CN120795661A