A water-based antistatic coating composition for single-walled carbon nanotubes and its preparation method
By using a one-step high-pressure microfluidic equipment for circulating homogenization and controlling the timing of resin addition, the problems of low dispersion efficiency and stability of waterborne antistatic coatings based on single-walled carbon nanotubes were solved, achieving efficient and stable coating preparation, reducing production costs and improving antistatic performance.
Patent Information
- Application Number
- CN202611165685.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing waterborne antistatic coatings made from single-walled carbon nanotubes suffer from problems such as long process routes, cumbersome steps, low dispersion efficiency, and easy agglomeration of carbon nanotubes, resulting in unstable antistatic performance of the coating.
A one-step method is adopted to simultaneously disperse single-walled carbon nanotubes and compound coatings. High-pressure microfluidic equipment is used for circulating homogenization, and the timing of resin addition is controlled within the range of 30-70% of the total circulation. This ensures the deagglomeration of carbon nanotubes and resin adsorption, and avoids the increase in coating resistance caused by adding too early or too late.
It achieves efficient dispersion of single-walled carbon nanotubes, reduces production costs and energy consumption, improves the storage stability and antistatic properties of coatings, reduces coating resistivity by 3 orders of magnitude, ensures uniform dispersion of the coating system, and shows no significant sedimentation after 7 days of storage at 50℃.
Smart Images

Figure SMS_14
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional coatings, specifically to a water-based antistatic coating composition of single-walled carbon nanotubes and its preparation method. Background Technology
[0002] Static electricity buildup can cause equipment damage, data errors, and even serious safety accidents such as fires and explosions in fields such as electronics, precision instruments, petrochemicals, and medical devices. Using antistatic coatings is one of the effective means to eliminate the hazards of static electricity.
[0003] Carbon nanotubes, especially single-walled carbon nanotubes, are considered ideal conductive fillers due to their excellent electrical conductivity, high aspect ratio, and superior mechanical properties. However, single-walled carbon nanotubes exhibit extremely strong van der Waals forces, making them prone to aggregation and difficult to disperse uniformly and stably in aqueous systems.
[0004] Currently, the preparation of waterborne antistatic coatings for single-walled carbon nanotubes generally adopts a two-step method. First, a high proportion of dispersant needs to be added, and high-intensity energy dispersion treatment is used to prepare a pre-dispersion liquid or concentrated masterbatch of single-walled carbon nanotubes. Then, this dispersion liquid is mixed and compounded with waterborne resin, other additives, etc., to obtain the finished coating. This two-step method has problems such as long process route, complicated steps, low dispersion efficiency, and carbon nanotubes are prone to secondary agglomeration during the compounding stage, resulting in unstable antistatic performance and poor appearance quality of the final coating.
[0005] Therefore, there is an urgent need to develop an efficient preparation method for waterborne antistatic coatings made from single-walled carbon nanotubes. Summary of the Invention
[0006] To overcome the above-mentioned technical problems, the present invention aims to provide a water-based antistatic coating composition of single-walled carbon nanotubes and its preparation method. For the first time, a one-step method is proposed to simultaneously achieve the dispersion of single-walled carbon nanotubes and coating compounding, and to solve the problem that carbon nanotubes are prematurely encapsulated or excessively sheared by resin and the coating resistance increases due to improper feeding sequence and timing in the one-step process.
[0007] The objective of this invention can be achieved through the following technical solutions: In a first aspect, this application provides a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step 1: Weigh out 0.05-1 parts by weight of single-walled carbon nanotubes, 3-30 parts by weight of water-based resin, 0.1-5 parts by weight of ionic dispersant, 55-65 parts by weight of deionized water, and 0.01-2.2 parts by weight of additives, and set aside. Step 2: Add the ionic dispersant to deionized water and stir at 300-500 rpm for 10-15 minutes at room temperature. Add single-walled carbon nanotubes and pre-disperse at 800-1200 rpm for 10-30 minutes at room temperature. Then, send the mixture to a high-pressure microfluidic device for homogenization. Set the total number of cycles to N, where N is 10-25 times, and the homogenization pressure to 1000-1500 bar. When the number of homogenization cycles reaches N, continue the homogenization process. When the content reaches 30-70%, pause the equipment, add water-based resin and additives, and stir and mix at a speed of 500-800 r / min for 5-10 min. Then restart the equipment and continue to complete the remaining homogenization cycle. After all homogenization cycles are completed, release the material, filter it with a 200-500 mesh filter to remove impurities, and then transfer it to a vacuum degassing tank. Degas it for 5-15 min at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube water-based antistatic coating.
[0008] In a preferred embodiment of the present invention, the single-walled carbon nanotubes have an average diameter of 1.6 nm and a length distribution of 5-30 μm, and are manufactured by OCSiAl. series.
[0009] In a preferred embodiment of the present invention, the waterborne resin is one or more selected from waterborne polyurethane, waterborne acrylic resin, waterborne epoxy resin, and waterborne polyester resin; wherein the waterborne polyurethane is an anionic or nonionic polyurethane dispersion, such as the Covestro Bayhydrol® U series; and the waterborne acrylic resin is a latex-type or secondary dispersion type, such as the BASF Joncryl® series and Dow... Series products; model of waterborne epoxy resin is 3510-W-60A; the waterborne polyester resin is from the Toyobo Vylon® series.
[0010] In a preferred embodiment of the present invention, the ionic dispersant is an anionic dispersant or a cationic dispersant; the anionic dispersant is one or more of sodium dodecylbenzenesulfonate, sodium lignosulfonate, sodium polycarboxylate, and alkylnaphthalene sulfonate; the cationic dispersant is one or more of hexadecyltrimethylammonium bromide and polyethyleneimine.
[0011] In a preferred embodiment of the present invention, the additive is one or more of the following: defoamer, wetting agent, leveling agent, film-forming aid, pH adjuster, and thickener.
[0012] Secondly, this application provides a water-based antistatic coating composition for single-walled carbon nanotubes, which is prepared according to the preparation method of the water-based antistatic coating composition for single-walled carbon nanotubes in the first aspect above.
[0013] The beneficial effects of this invention are: This invention discloses a water-based antistatic coating composition for single-walled carbon nanotubes and its preparation method. The method involves adding an ionic dispersant to deionized water and stirring to obtain an aqueous dispersant solution. Single-walled carbon nanotubes are then added to the aqueous dispersant solution to pre-disperse the carbon nanotubes, resulting in a pre-dispersed slurry. This pre-dispersed slurry is then fed into a high-pressure microfluidic jet device for cyclic homogenization. The total number of cycles is set to N, and the homogenization pressure is set. The device is paused, and aqueous resin and additives are added and stirred. The device is then restarted to complete the remaining homogenization cycles. After all homogenization cycles are completed, the material is discharged, filtered, and then degassed to obtain the water-based antistatic coating for single-walled carbon nanotubes. In the first half of the homogenization process, the system contains only carbon nanotubes, dispersant, and deionized water, without resin molecule encapsulation or obstruction. The high-intensity shearing, collision impact, and cavitation effects generated by the high-pressure microfluidic jet efficiently disintegrate the aggregates and bundles of carbon nanotubes, ultimately achieving complete unbundling and homogeneous dispersion of the carbon nanotubes. When aqueous resin is added during the 30-70% range of the total homogenization cycle, the resin molecules adsorb onto the surface of carbon nanotubes. On the one hand, this provides steric hindrance protection during the latter half of the homogenization process, preventing excessive breakage of carbon nanotubes under continuous strong shear, maintaining their high aspect ratio, and ensuring the integrity of the conductive network. On the other hand, the adsorption of resin prevents the dispersed carbon nanotubes from re-agglomerating, improving the storage stability of the coating system. If the resin is added too early (before 30% of the total cycle), the carbon nanotubes have not yet been fully unbundled and deagglomerated, and the resin will quickly coat the surface of the agglomerates, hindering the shear force from disintegrating the agglomerates. At the same time, an insulating layer is formed on the surface of the carbon nanotubes, leading to an increase in coating resistivity. If the resin is added too late (after 70% of the total cycle), the carbon nanotubes undergo excessive shearing without protection, resulting in a significant reduction in length and aspect ratio, and the conductive network is destroyed. This also leads to an increase in resistivity, and the short carbon nanotubes are prone to sedimentation, resulting in poor coating stability.
[0014] This invention achieves a one-step preparation method for waterborne antistatic coatings using single-walled carbon nanotubes (SHU). The one-step method involves the continuous completion of SHU deagglomeration and dispersion, along with the stabilization of the waterborne resin, within the same high-pressure homogenization process. This eliminates the need for separate preparation and transfer of the SHU pre-dispersion intermediate, significantly improving production efficiency and reducing costs compared to the traditional two-step method. Through a systematic study of the impact of resin addition timing during homogenization on SHU dispersion, length retention, and coating conductivity, a process strategy of initial deagglomeration, mid-stage resin addition, and final stage stabilization is proposed. This strategy precisely controls the addition of waterborne resin within the 30-70% range of the total high-pressure homogenization cycle, effectively solving the dilemma in one-step SHU conductive coating preparation where early resin addition leads to SHU coating and insulation, while late resin addition results in excessive shearing and breakage of the SHU. This achieves an optimal balance between SHU dispersion and length retention. Under the same SHU addition amount, the prepared coating surface resistivity can reach [value missing]. The coating strength is reduced by more than three orders of magnitude compared to the traditional two-step and simple one-step methods. Simultaneously, the coating system exhibits uniform dispersion, shows no significant sedimentation after 7 days of storage at 50°C, and produces a smooth, particle-free coating with significantly improved performance consistency and stability. This process eliminates the traditional two-step process of separately preparing a carbon nanotube pre-dispersion intermediate and then compounding it with resin to form a paint. It removes the pre-dispersion preparation, storage, and transfer steps, shortening production time and significantly reducing energy consumption, labor, and management costs. Furthermore, it requires no additional dedicated production equipment; the technology can be upgraded simply by adjusting the feeding sequence of the existing high-pressure microjet production line. The process parameters are highly controllable, facilitating rapid industrialization and large-scale production. Detailed Implementation
[0015] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0016] Example 1: This embodiment describes a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The material is pre-dispersed at 800 rpm for 10 minutes at room temperature, then fed into a high-pressure microfluidic device for homogenization. The total number of cycles is set to N, which is 10 times, and the homogenization pressure is 1000 bar. When the number of homogenization cycles reaches 50% of the total number of cycles N, the device is stopped, and waterborne resin (waterborne polyurethane, model Covestro Bayhydrol® U series) and additives (defoamer and wetting agent, model BYK-024 for defoamer and model BYK-348 for wetting agent) are added. The mixture is stirred at 500 rpm for 5 minutes, then the device is restarted to complete the remaining homogenization cycle. After all homogenization cycles are completed, the material is discharged, filtered through a 200-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. Degassing is performed for 5 minutes at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0017] Example 2: This embodiment describes a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.5 parts by weight of single-walled carbon nanotubes, 28 parts by weight of water-based resin, 3 parts by weight of ionic dispersant, 60 parts by weight of deionized water, 2 parts by weight of film-forming aid and 0.2 parts by weight of leveling agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium lignosulfonate) to deionized water and stir at 400 rpm for 12 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The mixture was pre-dispersed at 1000 rpm for 20 minutes at room temperature, and then fed into a high-pressure microfluidic device for homogenization. The total number of cycles was set to N, which was 15 times, and the homogenization pressure was 1200 bar. When the number of homogenization cycles reached 47% of the total number of cycles N, the device was stopped, and water-based resin (water-based acrylic resin, BASF Joncryl® series) and additives (film-forming aid and leveling agent, the film-forming aid being dipropylene glycol butyl ether, and the leveling agent being Tego® Glide 450) were added. The mixture was stirred and mixed at 600 rpm for 7 minutes, and then the device was restarted to continue the remaining homogenization cycles. After all homogenization cycles were completed, the material was discharged, filtered through a 300-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. The material was degassed for 10 minutes at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube water-based antistatic coating.
[0018] Example 3: This embodiment describes a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 1 part single-walled carbon nanotubes, 20 parts water-based resin, 5 parts ionic dispersant, 55 parts deionized water, 0.5 parts defoamer, and 0.3 parts thickener according to the weight ratio, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium lignosulfonate) to deionized water and stir at 500 rpm for 15 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). (Series), pre-dispersed at room temperature at 1200 r / min for 30 min, then fed into a high-pressure microfluidic device for circulating homogenization. The total number of cycles was set to N, which was 25 times, and the homogenization pressure was 1500 bar. When the number of homogenization cycles reached 48% of the total number of cycles N, the equipment was stopped, and water-based resin (water-based epoxy resin, model number) was added. The mixture was stirred and mixed with additives (defoamer and thickener, defoamer model BYK-024 and thickener model RM-8W) at 800 r / min for 10 min. The equipment was then restarted to continue the remaining homogenization cycle. After all homogenization cycles were completed, the material was discharged, filtered through a 500-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. The material was degassed for 15 min at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0019] Example 4: This embodiment describes a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The material is pre-dispersed at 800 rpm for 10 minutes at room temperature, then fed into a high-pressure microfluidic device for homogenization. The total number of cycles is set to N, which is 10 times, and the homogenization pressure is 1000 bar. When the number of homogenization cycles reaches 30% of the total number of cycles N, the device is stopped, and waterborne resin (waterborne polyurethane, model Covestro Bayhydrol® U series) and additives (defoamer and wetting agent, model BYK-024 for defoamer and model BYK-348 for wetting agent) are added. The mixture is stirred at 500 rpm for 5 minutes, then the device is restarted to complete the remaining homogenization cycle. After all homogenization cycles are completed, the material is discharged, filtered through a 200-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. Degassing is performed for 5 minutes at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0020] Example 5: This embodiment describes a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The material is pre-dispersed at 800 rpm for 10 minutes at room temperature, then fed into a high-pressure microfluidic device for homogenization. The total number of cycles is set to N, which is 10 times, and the homogenization pressure is 1000 bar. When the number of homogenization cycles reaches 70% of the total number of cycles N, the device is stopped, and waterborne resin (waterborne polyurethane, model Covestro Bayhydrol® U series) and additives (defoamer and wetting agent, model BYK-024 for defoamer and model BYK-348 for wetting agent) are added. The mixture is stirred at 500 rpm for 5 minutes, then the device is restarted to complete the remaining homogenization cycle. After all homogenization cycles are completed, the material is discharged, filtered through a 200-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. Under the conditions of room temperature and a vacuum degree of -0.1 MPa, the material is degassed for 5 minutes to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0021] Comparative Example 1: This comparative example illustrates a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The mixture consisted of a series of waterborne polyurethane resins (model: Covestro Bayhydrol® U series) and additives (defoamer and wetting agent; defoamer model: BYK-024, wetting agent model: BYK-348). The mixture was pre-dispersed at 800 rpm for 10 minutes at room temperature, then fed into a high-pressure microfluidic device for homogenization. The total number of cycles was set to N, which was 10 cycles, and the homogenization pressure was 1000 bar. After all homogenization cycles were completed, the material was discharged, filtered through a 200-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. Degassing was performed for 5 minutes at room temperature and a vacuum of -0.1 MPa to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0022] Comparative Example 2: This comparative example illustrates a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The material is pre-dispersed at 800 rpm for 10 minutes at room temperature, then fed into a high-pressure microfluidic device for homogenization. The total number of cycles is set to N, which is 10 times, and the homogenization pressure is 1000 bar. When the number of homogenization cycles reaches 20% of the total number of cycles N, the device is stopped, and waterborne resin (waterborne polyurethane, model Covestro Bayhydrol® U series) and additives (additives are defoamer and wetting agent, model BYK-024 for defoamer and model BYK-348 for wetting agent) are added. The mixture is stirred at 500 rpm for 5 minutes, then the device is restarted to complete the remaining homogenization cycle. After all homogenization cycles are completed, the material is discharged, filtered through a 200-mesh filter to remove impurities, and then transferred to a vacuum degassing tank. Under the conditions of room temperature and a vacuum degree of -0.1 MPa, the material is degassed for 5 minutes to obtain a single-walled carbon nanotube waterborne antistatic coating.
[0023] Comparative Example 3: This comparative example illustrates a method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, comprising the following steps: Step S1: Weigh out 0.3 parts by weight of single-walled carbon nanotubes, 25 parts by weight of water-based resin, 2.5 parts by weight of ionic dispersant, 65 parts by weight of deionized water, 0.2 parts by weight of defoamer and 0.3 parts by weight of wetting agent, and set aside. Step S2: Add the ionic dispersant (an anionic dispersant, sodium dodecylbenzenesulfonate) to deionized water and stir at 300 rpm for 10 minutes at room temperature. Then add single-walled carbon nanotubes (the average diameter of the single-walled carbon nanotubes is 1.6 nm, the length distribution is 5-30 μm, and the product is from OCSiAl). The material was pre-dispersed at 800 rpm for 10 minutes at room temperature, and then fed into a high-pressure microfluidic device for circulating homogenization. The total number of cycles was set to N, which is 10 times, and the homogenization pressure was 1000 bar. After all homogenization cycles were completed, the material was discharged, and water-based resin (water-based polyurethane, model Covestro Bayhydrol® U series) and additives (defoamer and wetting agent, model BYK-024 for defoamer and model BYK-348 for wetting agent) were added to the material. The mixture was stirred at 500 rpm for 5 minutes, and then filtered through a 200-mesh filter to remove impurities. The mixture was then transferred to a vacuum degassing tank and degassed for 5 minutes at room temperature and a vacuum degree of -0.1 MPa to obtain a single-walled carbon nanotube water-based antistatic coating.
[0024] Performance testing The single-walled carbon nanotube waterborne antistatic coatings of Examples 1-5 and Comparative Examples 1-3 were coated on a clean PET film, and the dry film thickness was controlled to be 20 μm. After drying, the film was tested according to the following method. The timing of resin addition during homogenization is calculated using the following formula: Timing of addition = Number of completions / Total number of completions.
[0025] Surface resistivity test: The test was conducted in accordance with GB / T 31838.3-2019 "Dielectric and resistive properties of solid insulating materials - Part 3: Resistive properties (DC method) - Surface resistance and surface resistivity". The test environment temperature was 23℃, the relative humidity was 50%, the test DC voltage was 100V, and the stable value was read after 1 minute of power-on. Five different locations were tested for each group of samples, and the arithmetic mean was taken as the final surface resistivity result.
[0026] Carbon nanotube average length test: Using an atomic force microscope, a small amount of the coating to be tested was taken and diluted with deionized water to a carbon nanotube mass concentration of 0.001%. After ultrasonic dispersion for 5 min, 10 μL of the diluted solution was dropped onto the surface of a freshly cleaved mica sheet and allowed to air dry at room temperature for later use. Twenty fields of view were randomly selected, and the lengths of independently dispersed single-walled carbon nanotubes in the fields of view were counted. Obviously aggregated carbon nanotube bundles were removed, and finally the arithmetic mean length of all counted carbon nanotubes was calculated.
[0027] Storage stability test: A thermally accelerated storage test was adopted. 200g of the coating to be tested was sealed in a glass container with a lid and placed in a constant temperature test chamber at 50℃ for 7 consecutive days. After the expiration, the sample was taken out and placed at room temperature for 2 hours to observe the state of the system. The system was classified according to the degree of sedimentation: No sedimentation: The system is uniform and consistent, with no stratification and no bottom sedimentation; Slight sedimentation: There is a small amount of soft sediment at the bottom, which can be redispersed evenly by gently stirring with a glass rod; Severe sedimentation: There is a large amount of hard sediment at the bottom, which cannot be completely redispersed after stirring, and the system shows obvious stratification.
[0028] The test results are shown in Table 1:
[0029] Referring to Table 1, based on the comparison between Examples 1-5 and Comparative Examples 1-3, it can be seen that the one-step process of adding water-based resin in the range of 30-70% of the total high-pressure homogenization cycle can effectively balance the degree of deagglomeration and length retention of single-walled carbon nanotubes. Compared with the schemes of adding the resin in full before homogenization, adding it too early, or adding it after homogenization, it can reduce the surface resistivity of the coating and improve the storage stability of the coating.
[0030] Examples 1-3 respectively employed waterborne polyurethane, waterborne acrylic, and waterborne epoxy resin systems, with the amount of single-walled carbon nanotubes added increasing progressively. The resin addition timing was within the 30-70% homogeneous range specified in this invention. The resulting coatings from all three systems exhibited uniform carbon nanotube dispersion, showed no sedimentation after 7 days of storage at 50°C, and demonstrated high surface resistivity. With an Ω / sq rating, it exhibits excellent antistatic properties.
[0031] Examples 1, 4, and 5 used identical formulations and homogenization parameters, adjusting only the timing of resin addition to correspond to the lower limit (30%), optimal value (50%), and upper limit (70%) of the process range, respectively. Single-variable verification validated the effectiveness of the process range, with all three coatings exhibiting resistivity within the specified range. The excellent antistatic range of Ω / sq fully demonstrates that 30-70% is a stable and effective process window.
[0032] Comparative Example 1: All resin was added before homogenization. The carbon nanotubes were insulated and coated with resin, and the coating resistivity exceeded [a certain value]. Ω / sq, completely losing its anti-static function.
[0033] In Comparative Example 2, the resin was added too early (20% node). The resin hindered the deagglomeration process of carbon nanotubes and formed a partial insulating coating. The coating resistivity increased by about four orders of magnitude compared with Example 1.
[0034] In Comparative Example 3, resin was added after all homogenization was completed. The carbon nanotubes were excessively sheared without protection, with an average length of only 0.4 μm. The conductive network was severely damaged, the resistivity increased significantly, and the coating had extremely poor storage stability, with severe sedimentation occurring after only 7 days.
[0035] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0036] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a water-based antistatic coating composition using single-walled carbon nanotubes, characterized in that, Includes the following steps: Step 1: Weigh out 0.05-1 parts by weight of single-walled carbon nanotubes, 3-30 parts by weight of water-based resin, 0.1-5 parts by weight of ionic dispersant, 55-65 parts by weight of deionized water, and 0.01-2.2 parts by weight of additives, and set aside. Step 2: Add the ionic dispersant to deionized water and stir. Add single-walled carbon nanotubes and pre-disperse. Then perform cyclic homogenization treatment, set the total number of cycles to N, set the homogenization pressure, pause the equipment, add water-based resin and additives, stir and mix, then restart the equipment and continue to complete the remaining homogenization cycle. After all homogenization cycles are completed, release the material, filter, and then degas to obtain a single-walled carbon nanotube water-based antistatic coating.
2. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The total number of cycles N in step two is 10-25 times; the homogenization pressure is 1000-1500 bar.
3. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The aqueous resin in step two is added at 30-70% of the total number of cycles N.
4. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The filtration in step two uses a 200-500 mesh filter.
5. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The single-walled carbon nanotubes have an average diameter of 1.6 nm and a length distribution of 5-30 μm.
6. The method for preparing a water-based antistatic coating composition of single-walled carbon nanotubes according to claim 1, characterized in that, The waterborne resin is one or more of waterborne polyurethane, waterborne acrylic resin, waterborne epoxy resin, and waterborne polyester resin; wherein the waterborne polyurethane is an anionic or nonionic polyurethane dispersion; and the waterborne acrylic resin is a latex or secondary dispersion.
7. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The ionic dispersant is an anionic or cationic dispersant; the anionic dispersant is one or more of sodium dodecylbenzene sulfonate, sodium lignosulfonate, sodium polycarboxylate, and alkylnaphthalene sulfonate; the cationic dispersant is one or more of hexadecyltrimethylammonium bromide and polyethyleneimine.
8. The method for preparing a water-based antistatic coating composition for single-walled carbon nanotubes according to claim 1, characterized in that, The additives are one or more of the following: defoamers, wetting agents, leveling agents, film-forming aids, pH adjusters, and thickeners.
9. A water-based antistatic coating composition for single-walled carbon nanotubes, characterized in that, The single-walled carbon nanotube waterborne antistatic coating composition is prepared by the method described in any one of claims 1-8.