Sapphire substrate pad printing ink and its preparation method, and preparation method of sapphire structural parts.

By chemically bonding a modified polyester resin and modified acrylic resin compound system with a coupling agent, the problem of poor ink adhesion on sapphire inert surfaces was solved, resulting in inks with high adhesion and hardness, simplifying the process and reducing costs.

CN123107451APending Publication Date: 2026-11-17HUIZHOU BESTER CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611540020.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve high adhesion, hardness, and durability of pad printing inks on inert sapphire surfaces, and plasma cleaning equipment requires significant investment, is sensitive to process parameters, and has unstable yield rates.

Method used

A modified polyester resin and modified acrylic resin compound system is adopted. Through the cross-linking network of the modified polyester resin and modified acrylic resin and the chemical bonding of the coupling agent, a double cross-linking effect is formed, which improves the adhesion of ink to sapphire substrate and simplifies the process.

Benefits of technology

Achieving high adhesion and hardness on inert sapphire surfaces simplifies the process, reduces costs, improves production yield, and meets the high precision and high reliability requirements of sapphire structural components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107451A_ABST
    Figure CN123107451A_ABST
Patent Text Reader

Abstract

This application provides a sapphire substrate pad printing ink and its preparation method, as well as a method for preparing sapphire structural parts. The aforementioned sapphire substrate pad printing ink includes component A and component B. Component A comprises the following components by weight: 30-40 parts modified polyester resin; 15-25 parts modified acrylic resin; 5-10 parts filler; 15-25 parts carbon black; 1-3 parts coupling agent; 1-4 parts additives; and 10-20 parts diluent. Component B is an isocyanate curing agent. The mass ratio of component A to component B is 100:(8-20). The modified polyester resin and modified acrylic resin are compounded to improve wetting and spreading on the sapphire substrate surface, while also considering adhesion and hardness. The coupling agent chemically bonds with the sapphire substrate and integrates into the polyurethane crosslinking network, forming a double crosslinking that enhances adhesion. High adhesion can be achieved on the inert surface of sapphire without plasma cleaning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the technical field of coatings, and in particular to a sapphire substrate pad printing ink and its preparation method, as well as a method for preparing sapphire structural components. Background Technology

[0002] Sapphire glass (monocrystalline alumina, Al2O3) has become a core substrate for smartphone camera covers, smartwatch crystals, AR / VR lenses, and fingerprint recognition modules due to its Mohs hardness of 9, visible light transmittance of ≥92%, and excellent chemical inertness. Pad printing technology uses a silicone pad to transfer ink patterns from an etched steel plate to the surface of sapphire glass, enabling high-precision pattern transfer on curved and irregular surfaces. Pad printing inks are widely used for surface decoration of precision components such as watch dials and consumer electronics panels.

[0003] However, sapphire glass substrates face significant adhesion challenges in pad printing processes. The surface energy of untreated sapphire glass is 30mN / m-40mN / m. Sapphire glass has extremely low surface energy, stable chemical bonding, and a lack of active functional groups, resulting in poor adhesion and easy detachment of conventional pad printing inks.

[0004] Moreover, existing technologies mostly rely on pre-processing activation techniques such as plasma treatment to improve the surface energy of sapphire substrates. Plasma cleaning requires a high vacuum or specific gas environment, and the equipment includes a vacuum chamber, radio frequency power supply, gas control system, etc., which increases costs due to high equipment investment. The surface polar groups induced by plasma treatment are not permanently stable, and the activation effect is time-sensitive, which poses a rigid constraint on the production cycle. Plasma treatment also carries the risk of damaging the sapphire substrate, and the process parameters are sensitive, making it difficult to guarantee the stability of yield.

[0005] For example, prior art document CN202410898628.1 discloses a 3D mobile phone back cover pad printing ink, its preparation method, and its application, comprising: 50-70 parts acrylic resin, 10-20 parts pigment, 10-20 parts filler, 1-3 parts adhesion agent, 5-15 parts curing agent, 1-10 parts dispersant, and 1-5 parts additives. The combination of polyester-modified acrylic resin and polyester-modified hydroxyl acrylic resin improves the adhesion of 3D glass pad printing, enhances the printing effect, and produces neat and uniform printing edges without burrs. The combination of talc and matting powder as filler improves printing resolution and enhances the printing effect. The resulting ink exhibits strong aging resistance and solvent resistance, is not easily peeled off after application to 3D glass surfaces, and has excellent gloss. The polyester-modified acrylic resin and polyester-modified hydroxyl acrylic resin used in this scheme are chemically both polyester-acrylic acid graft copolymers. In this system, the ratio of polyester to acrylic segments is determined by the grafting rate during the synthesis stage. Once the graft copolymer is synthesized, the polyester to acrylic ratio is fixed, and ink formulators cannot independently adjust the polyester content during the formulation stage. Furthermore, the resin system is predominantly acrylic resin, with polyester existing only as a modified form on the acrylic resin molecular chain. The polyester segment content is constrained by the grafting rate, making it difficult to fully utilize the wetting and adhesion functions of polyester resin on inert substrates. This solution targets 3D glass as the substrate, whose surface energy is typically in the range of 45 mN / m-55 mN / m. Sapphire, however, has a surface energy below 40 mN / m, exhibits far greater chemical inertness than 3D glass, and has an extremely low surface hydroxyl density. Therefore, when directly applied to sapphire substrates, the adhesion is insufficient to meet the requirements of sapphire products.

[0006] There is an urgent need for a pad printing ink that can achieve high adhesion, high hardness, and high durability on inert sapphire surfaces without relying on pre-activation processes such as plasma cleaning. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a sapphire substrate pad printing ink that can achieve high adhesion on the inert surface of sapphire without relying on plasma cleaning, as well as a method for preparing the same and a method for preparing sapphire structural parts.

[0008] The objective of this invention is achieved through the following technical solution: A sapphire substrate pad printing ink includes component A and component B, wherein component A has the following components by weight: 30-40 parts of modified polyester resin; 15-25 parts of modified acrylic resin; 5-10 parts of filler; 15-25 parts carbon black; 1-3 parts coupling agent; 1-4 parts of auxiliary agent; 10-20 parts diluent; Component B is an isocyanate curing agent; The mass ratio of component A to component B is 100:(8-20).

[0009] In one embodiment, the coupling agent is γ-glycidoxypropyltrimethoxysilane.

[0010] In one embodiment, the modified polyester resin is an amorphous copolyester resin.

[0011] In one embodiment, the hydroxyl value of the amorphous copolyester resin is 3mgKOH / g-12mgKOH / g, and the acid value of the amorphous copolyester resin is ≤5mgKOH / g.

[0012] In one embodiment, the diluent is at least one of isophor, propylene glycol methyl ether acetate, and cyclohexanone.

[0013] In one embodiment, the filler is fumed silica.

[0014] In one embodiment, the additives include a superdispersant, a defoamer, and a leveling agent; and / or, the mass ratio of the superdispersant, the defoamer, and the leveling agent is (1-3):(0.5-1.5):(0.5-1.5).

[0015] In one embodiment, the isocyanate curing agent is HDI biuret.

[0016] A method for preparing a sapphire substrate pad printing ink, used to prepare the sapphire substrate pad printing ink as described in any of the above embodiments, includes the following steps: Pre-dispersion treatment involves mixing and dispersing modified polyester resin, modified acrylic resin, dispersant, and a portion of diluent at a speed of 300 r / min-500 r / min for 5 min-10 min to obtain a premix. For the filler dispersion treatment, carbon black and filler are added sequentially to the premix, the dispersion speed is increased to 800 r / min-1200 r / min, and the dispersion time is 10 min-15 min to obtain a dispersed mixture; The dispersion mixture is ground to a fineness of ≤8μm to obtain a ground mixture. Additive dispersion treatment: Coupling agent, leveling agent, defoamer and remaining diluent are added to the grinding mixture. The speed is 300r / min-500 and the dispersion time is 5min-10min. After uniform mixing, component A is obtained. The mixing process involves uniformly mixing component A and component B at a mass ratio of 100:8 to 100:20, wherein component B is an isocyanate curing agent, to obtain sapphire substrate pad printing ink.

[0017] A method for preparing a sapphire structural component, using the sapphire substrate pad printing ink prepared in any of the above embodiments, includes the following steps: Ink pad printing, the sapphire substrate is not plasma cleaned before pad printing. The pad printing equipment is used to transfer pad printing ink onto the sapphire substrate to form an ink pad printing layer, thereby obtaining a pad printing substrate; Baking and curing: The pad printing substrate is baked and cured at a temperature of 120℃-150℃ for 20min-40min. After the pad printing layer is cured, an ink curing layer is obtained to obtain a sapphire cured part. Cooling treatment is performed to cool the sapphire cured part to room temperature to obtain a sapphire structural part.

[0018] Compared with the prior art, the present invention has at least the following advantages: The aforementioned sapphire substrate pad printing ink employs a modified polyester resin and modified acrylic resin compound system, with the modified polyester resin as the dominant component. Its polar ester bonds and hydroxyl groups improve wetting and spreading on the low surface energy surface of the sapphire substrate, while the modified acrylic resin provides hardness and abrasion resistance. The polyester resin first reacts with the curing agent to rapidly establish a cross-linked framework and provide interfacial adhesion. The acrylic resin gradually participates in the reaction during the subsequent high-temperature curing stage, thereby forming a differentiated curing cross-linked network, ensuring that the cured ink balances adhesion and hardness. Through the inorganic end of the coupling agent chemically bonding with the sapphire substrate surface, and the organic end of the coupling agent reacting with the hydroxyl and carboxyl groups of the modified polyester and modified acrylic resins to integrate into the polyurethane cross-linked network, a dual cross-linking effect is formed with the cured cross-linked network, further enhancing the adhesion to the sapphire substrate. The sapphire substrate pad printing ink can achieve high adhesion on the inert surface of the sapphire substrate without plasma cleaning, thereby simplifying the process, reducing costs, and improving yield. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 The following is a flowchart of the preparation method of sapphire substrate pad printing ink according to an embodiment of the present invention; Figure 2This is a flowchart illustrating the steps of a method for preparing a sapphire structural component according to an embodiment of the present invention. Figure 3 This is a physical image of a sapphire structural component according to an embodiment of the present invention; Figure 4 This is another physical image of a sapphire structural component according to one embodiment of the present invention. Detailed Implementation

[0021] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0023] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0024] In this invention, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous, and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to directly listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.

[0025] Unless otherwise specified, the temperature parameters in this invention can be either constant temperature treatment or variations within a certain temperature range. It should be understood that the constant temperature treatment allows temperature fluctuations within the precision range controlled by the instrument. Fluctuations are permitted within ranges such as ±5℃, ±4℃, ±3℃, ±2℃, and ±1℃.

[0026] This application provides a sapphire substrate pad printing ink, comprising component A and component B. Component A has the following components by weight: 30-40 parts modified polyester resin; 15-25 parts modified acrylic resin; 5-10 parts filler; 15-25 parts carbon black; 1-3 parts coupling agent; 1-4 parts additives; and 10-20 parts diluent. Component B is an isocyanate curing agent. The mass ratio of component A to component B is 100:8-100:20.

[0027] To better understand this application, the following further explanation is provided: One embodiment of the sapphire substrate pad printing ink includes component A and component B, wherein component A has the following components by weight: 30-40 parts of modified polyester resin; 15-25 parts of modified acrylic resin; 5-10 parts of filler; 15-25 parts carbon black; 1-3 parts coupling agent; 1-4 parts of auxiliary agent; 10-20 parts diluent; Component B is an isocyanate curing agent; The mass ratio of component A to component B is 100:(8-20).

[0028] It is understandable that the modified polyester resin and modified acrylic resin exist as independent molecular chains in the ink, and cross-linking is achieved through the isocyanate curing agent during the curing process. The hydroxyl groups of the modified polyester resin are mainly primary hydroxyl groups, with low steric hindrance and high reactivity with isocyanate groups. The hydroxyl groups of the modified acrylic resin are mostly secondary hydroxyl groups, and their reactivity is relatively low due to the steric hindrance of the polymer chain segments. After mixing, the curing agent preferentially reacts with the polyester resin to quickly establish a cross-linked skeleton. The acrylic resin gradually participates in the reaction during the subsequent high-temperature curing stage, forming a gradient cross-linking. The modified acrylic resin forms a high cross-linking density, thereby providing cohesive strength and interfacial adhesion. The cross-linking of the modified acrylic resin provides hardness, abrasion resistance, and flexibility. The modified acrylic resin itself has excellent UV resistance and aging resistance. The polyurethane network formed by the cross-linking of the isocyanate curing agent and the resin hydroxyl groups is dense and stable, which can effectively block solvent penetration, thereby improving alcohol resistance.

[0029] Understandably, the inorganic end of the coupling agent hydrolyzes to generate silanol groups, which can undergo a condensation reaction with the trace amounts of hydroxyl groups remaining on the sapphire surface to form Si-O-Al chemical bonds; the organic end of the coupling agent, such as epoxy groups, can undergo a ring-opening reaction with the hydroxyl and carboxyl groups of the modified polyester resin and modified acrylic resin, directly integrating the coupling agent into the polyurethane crosslinking network.

[0030] The aforementioned sapphire substrate pad printing ink employs a modified polyester resin and modified acrylic resin compound system, with the modified polyester resin as the dominant component. Its polar ester bonds and hydroxyl groups improve wetting and spreading on the low surface energy surface of the sapphire substrate, while the modified acrylic resin provides hardness and abrasion resistance. The polyester resin first reacts with the curing agent to rapidly establish a cross-linked framework and provide interfacial adhesion. The acrylic resin gradually participates in the reaction during the subsequent high-temperature curing stage, thereby forming a differentiated curing cross-linked network, ensuring that the cured ink balances adhesion and hardness. Through the inorganic end of the coupling agent chemically bonding with the sapphire substrate surface, and the organic end of the coupling agent reacting with the hydroxyl and carboxyl groups of the modified polyester and modified acrylic resins to integrate into the polyurethane cross-linked network, a dual cross-linking effect is formed with the cured cross-linked network, further enhancing the adhesion to the sapphire substrate. The sapphire substrate pad printing ink can achieve high adhesion on the inert surface of the sapphire substrate without plasma cleaning, thereby simplifying the process, reducing costs, and improving yield.

[0031] In one embodiment, the coupling agent is γ-glycidoxypropyltrimethoxysilane. In this embodiment, γ-glycidoxypropyltrimethoxysilane is an epoxy silane coupling agent with a bifunctional molecular structure. The methoxy group at one end of γ-glycidoxypropyltrimethoxysilane hydrolyzes to generate a highly reactive silanol group, which then undergoes a condensation reaction with the hydroxyl groups on the sapphire substrate surface to form a stable Al-O-Si covalent bond. The epoxy group at the other end of γ-glycidoxypropyltrimethoxysilane can undergo a ring-opening reaction with the hydroxyl and carboxyl groups in the organic resin system, thereby constructing a strong chemical bond between the sapphire substrate and the organic ink. Understandably, amino groups have extremely high reactivity with isocyanate groups. If an amino-type coupling agent is used, its amino group will react rapidly with the isocyanate curing agent during the ink mixing stage, significantly shortening the ink's pot life. Silane coupling agents containing epoxy groups are suitable for unsaturated polyester resin and acrylic resin systems. The epoxy group of γ-glycidoxypropyltrimethoxysilane can simultaneously undergo ring-opening reactions with the carboxyl / hydroxyl groups of modified polyester resin and the hydroxyl groups of modified acrylic resin, allowing the coupling agent to directly integrate into the polyurethane crosslinking network.

[0032] In one embodiment, the modified polyester resin is an amorphous copolyester resin. In this embodiment, the molecular chains of the amorphous copolyester resin are randomly arranged, allowing polar groups such as ester bonds, hydroxyl groups, and carboxyl groups to be fully exposed and freely spread on the sapphire substrate surface. Compared with crystalline polyester, the amorphous copolyester resin has better wettability on the sapphire surface and a larger effective contact area. The amorphous copolyester resin is blended with the modified acrylic resin in an independent molecular form, ensuring that the polar groups are not spatially blocked by the acrylic chain segments, thereby allowing for full contact with the sapphire surface.

[0033] In one embodiment, the hydroxyl value of the amorphous copolyester resin is 3 mgKOH / g-12 mgKOH / g, and the acid value of the amorphous copolyester resin is ≤5 mgKOH / g. In this embodiment, the hydroxyl value of the amorphous copolyester resin is 3 mgKOH / g-12 mgKOH / g, which gives the amorphous copolyester resin an appropriate hydroxyl density, thereby forming a sufficient crosslinking network with the isocyanate curing agent and retaining the hydrogen bonding between the hydroxyl groups and the sapphire surface, enhancing the interfacial adhesion. If the hydroxyl value is too low, the crosslinking density is insufficient, and the cohesive strength and solvent resistance of the film layer decrease. If the hydroxyl value is too high, the hydroxyl groups excessively consume the isocyanate groups, thereby weakening the adhesion between the coupling agent and the resin matrix. The acid value of the amorphous copolyester resin is ≤5 mgKOH / g, which reduces the excessive carboxyl groups that would lead to increased water absorption of the coating film, thereby allowing the cured film layer to maintain high water resistance and damp heat resistance under high temperature and high humidity conditions.

[0034] In one embodiment, the diluent is at least one selected from isophorone, propylene glycol methyl ether acetate, and cyclohexanone. In this embodiment, cyclohexanone has a low boiling point and evaporates the fastest, promoting rapid surface drying of the ink on the silicone head and maintaining pattern setting; propylene glycol methyl ether acetate has a moderate boiling point and a moderate evaporation rate, ensuring complete transfer of ink from the stencil to the silicone head and then to the sapphire substrate; isophorone has the highest boiling point and evaporates the slowest, maintaining the open time of the ink on the stencil and preventing pattern sticking during multicolor printing.

[0035] Furthermore, in one embodiment, the mass ratio of isophorone, propylene glycol methyl ether acetate, and cyclohexanone is 1-5:1-8:1-3. In this embodiment, by matching the ratio of the three solvents with the evaporation rate gradient, it is possible to avoid the pad printing ink drying too quickly on the silicone head when the cyclohexanone content is too high, and to avoid the pad printing ink drying too slowly when the isophorone content is too high, which would lead to overprinting adhesion and blurring of the pattern. This balances the printability of the ink with the surface drying time, thereby meeting the high-precision printing requirements of sapphire structural components for fine scales and patterns.

[0036] In one embodiment, the filler is fumed silica. In this embodiment, the surface of the fumed silica is rich in silanol groups, which form a three-dimensional network structure in the ink system through hydrogen bonds, giving the ink excellent thixotropic properties. This allows it to thicken when stationary to prevent pigment sedimentation and thin when sheared, ensuring that the ink is completely transferred from the steel plate to the silicone head and then to the substrate during the pad printing process. Simultaneously, the silanol groups on the surface of the fumed silica can undergo a condensation reaction with the silanol groups generated after the methoxy group of γ-glycidoxypropyltrimethoxysilane is hydrolyzed, enhancing the dispersion and anchoring of the coupling agent in the resin system, thereby improving the adhesion of the pad printing ink. The nanoparticles of fumed silica improve the hardness, abrasion resistance, and scratch resistance of the cured film and block the erosion of the interface by environmental moisture, thereby improving the water resistance and damp heat resistance of the film.

[0037] In one embodiment, the additives include a superdispersant, a defoamer, and a leveling agent; and / or, the mass ratio of the superdispersant, the defoamer, and the leveling agent is (1-3):(0.5-1.5):(0.5-1.5). In this embodiment, the superdispersant, by adsorbing onto the surface of carbon black and fumed silica particles, forms a steric hindrance layer, preventing pigments and fillers from agglomerating and settling in the resin system, thus improving ink storage stability and printing color uniformity. The defoamer inhibits the generation of bubbles during ink dispersion and pad printing, reducing pinholes or bubble defects in the cured film. The leveling agent regulates the surface tension of the ink, improving the uniformity of ink spreading on the sapphire substrate and reducing pinholes and orange peel effects.

[0038] In one embodiment, the isocyanate curing agent is HDI biuret. In this embodiment, HDI biuret reacts fully with the primary hydroxyl groups of the polyester resin and the secondary hydroxyl groups of the acrylic resin to form a crosslinking network. The molecular structure of HDI biuret is a linear skeleton, thereby introducing a certain degree of segmental flexibility into the crosslinking network, making the cured film layer less brittle while maintaining sufficient hardness, thus improving the flexibility and impact resistance of the pad printing ink. Specifically, the HDI biuret is Covestro Desmodur® N75, with an NCO content of 16%-17%.

[0039] Further, in one embodiment, the carbon black includes coarse-grained carbon black and short-grained carbon black. The particle size of the coarse-grained carbon black is 26nm-40nm, and the particle size of the short-grained carbon black is 14nm-26nm. The ratio of the short-grained carbon black to the coarse-grained carbon black is 1:3-4:1. It is understood that if only short-grained carbon black is used, although the blackness is high, the large specific surface area leads to high oil absorption, increased system viscosity, difficulty in dispersion, easy flocculation and coarsening, and increased internal stress in the cured film, resulting in decreased adhesion. If only coarse-grained carbon black is used, although dispersion is easy and viscosity is controllable, both blackness and opacity are insufficient. In this embodiment, a dual-particle-size compound system is formed by coarse-grained carbon black and short-grained carbon black. The short-grained carbon black has a smaller particle size and a larger specific surface area, resulting in a larger light absorption cross section per unit mass of carbon black, which dominates the blackness and light absorption capacity of the ink curing layer. The coarse-grained carbon black has a larger particle size, and its aggregates form a loose three-dimensional chain structure in the cured film layer. Incident light undergoes multiple scattering within the aggregates and between adjacent aggregates, significantly extending the light propagation path in the film layer, thereby achieving high light-blocking efficiency with a lower carbon black addition amount. The mass ratio of short-grained carbon black to coarse-grained carbon black is 1:3-4:1, achieving a balance between blackness, light-blocking properties, dispersion stability, and viscosity control. This solves the problem that it is difficult to achieve a balance between blackness, light-blocking properties, dispersion stability, viscosity control, and light leakage in thin layers with a single carbon black, enabling the ink on the back of the sapphire structural component to achieve high light-blocking, high adhesion, and high printing accuracy even with an extremely thin ink layer. Specifically, the short-particle carbon black is Cabot Monarch 1100, which has an average native particle size of 14 nm and a BET specific surface area of ​​240 m². 2 / g, DBP oil absorption value 65cm 3 / 100g, this is a high specific surface area, low-structure pigment carbon black with high tinting strength and excellent blackness, suitable for ink systems requiring high blackness; the coarse-grained carbon black is Orion Printex 35, with an average native particle size of 31nm and a BET specific surface area of ​​65m². 2 With a DBP oil absorption value of 42 mL / 100 g, it belongs to the low-structure pigment furnace black category, exhibiting good dispersibility, high gloss, and a bluish hue. Mitsubishi Chemical MA8 has an average primary particle size of 24 nm and a nitrogen adsorption specific surface area of ​​120 m². 2 / g, DBP absorption capacity is 57cm³ 3 With a tinting strength of 139% per 100g, it belongs to medium blackness and medium structure pigment carbon black; Printex 35 and MA8 both have suitable light scattering properties and can be used as coarse carbon black components in combination with Monarch 1100.

[0040] like Figure 1As shown, this application also provides a method for preparing sapphire substrate pad printing ink, used to prepare the sapphire substrate pad printing ink described in any of the above embodiments, comprising the following steps: S101, pre-dispersion treatment, involves mixing and dispersing modified polyester resin, modified acrylic resin, dispersant and some diluent at a speed of 300 r / min-500 r / min and a dispersion time of 5 min-10 min to obtain a premix.

[0041] S103, filler dispersion treatment: carbon black and filler are added sequentially to the premix, the dispersion speed is increased to 800r / min-1200r / min, and the dispersion time is 10min-15min, so as to obtain a dispersed mixture.

[0042] S105, Grinding process: Grinding the dispersed mixture to a fineness of ≤8μm to obtain a ground mixture.

[0043] S107, Auxiliary agent dispersion treatment: Coupling agent, leveling agent, defoamer and remaining diluent are added to the grinding mixture, the rotation speed is 300r / min-500, the dispersion time is 5min-10min, and component A is obtained.

[0044] S109, Mixing treatment, mixing component A and component B at a mass ratio of 100:8-100:20, wherein component B is an isocyanate curing agent, to obtain sapphire substrate pad printing ink.

[0045] In this embodiment, during the pre-dispersion treatment, the dispersant adsorbs onto the surface of the subsequently added carbon black and filler particles, forming a steric hindrance layer to prevent pigments and fillers from agglomerating and settling in the resin system; a portion of the diluent is used to pre-dissolve the resin, allowing the modified polyester resin and modified acrylic resin to fully dissolve and uniformly mix at a lower viscosity, thereby producing a uniform and stable premix; the dispersion mixture is then ground to a fineness of ≤8 μm using a roller mill, thereby further refining the carbon black and filler particles. Adding the coupling agent after grinding prevents excessive condensation of the coupling agent with the silanol groups on the fumed silica surface during grinding, thus avoiding pre-consumption and maintaining a high free concentration of the coupling agent in the ink system. This allows the coupling agent to migrate more effectively to the sapphire interface during pad printing and curing, forming Al-O-Si covalent bonds with the residual hydroxyl groups on the sapphire surface. The coupling agent also levels and adjusts the surface tension of the pad printing ink, improving the uniformity of ink spreading on the sapphire substrate. The defoamer inhibits bubble formation, preventing pinholes in the cured film. The remaining diluent adjusts the ink viscosity to the range suitable for the pad printing process. The isocyanate curing agent reacts with the hydroxyl groups of the modified polyester and acrylic resins to form a polyurethane crosslinking network, providing cohesive strength, hardness, and solvent resistance. The inorganic end of the coupling agent forms Al-O-Si covalent bonds with the sapphire surface, while the organic end reacts with the hydroxyl or carboxyl groups of the resin in a ring-opening reaction, integrating into the polyurethane crosslinking network and constructing a chemical crosslinking network between the inorganic substrate and the organic ink.

[0046] The above-mentioned method for preparing sapphire substrate pad printing ink uses a modified polyester resin and modified acrylic resin compound system, which makes the cured layer formed by the pad printing ink have both flexibility and adhesion, while improving weather resistance, alcohol resistance and fast drying. By adding materials in steps, adding coupling agent after grinding, adding diluent in stages, and controlling the mass ratio of component A to component B, the coupling agent and isocyanate curing agent synergistically form a double cross-linking network, making the pad printing ink suitable for sapphire substrates that have not been plasma cleaned.

[0047] like Figures 2 to 4 As shown, this application also provides a method for preparing a sapphire structural component, which is manufactured using the sapphire substrate pad printing ink prepared in any of the above embodiments, and includes the following steps: S201, ink pad printing, the sapphire substrate is not plasma cleaned before pad printing, and pad printing ink is transferred to the sapphire substrate by pad printing equipment to form an ink pad printing layer to obtain a pad printing substrate. S203, Baking and curing: The pad printing substrate is baked and cured at a temperature of 120℃-150℃ for 20min-40min. After the pad printing layer is cured, an ink curing layer is obtained to obtain a sapphire cured part. S205, Cooling treatment: Cool the sapphire cured part to room temperature to obtain a sapphire structural part.

[0048] In this embodiment, the sapphire substrate is not subjected to plasma cleaning, flame treatment, or chemical primer before pad printing. The pad printing ink is transferred to the surface of the sapphire substrate by a pad printing machine. The polar ester bonds and hydroxyl groups of the modified polyester resin have good wetting ability on the sapphire surface, thereby reducing the contact angle of the ink on the sapphire surface and improving the spreadability. The epoxy groups of the coupling agent undergo ring-opening reactions with the hydroxyl and carboxyl groups in the resin, allowing the coupling agent to directly access the polyurethane crosslinking network and form a double crosslinking network with Al-O-Si covalent bonds. During the baking and curing process, the isocyanate curing agent first reacts with the modified polyester resin to quickly establish a polyurethane crosslinking skeleton and provide interfacial adhesion. Subsequently, the isocyanate curing agent reacts gradually with the modified acrylic resin to increase the crosslinking density and increase hardness and wear resistance, thereby forming a differentiated gradient crosslinking network. During the cooling process, the internal stress of the cured film is gradually released, reducing the risk of film cracking or decreased adhesion due to sudden cooling.

[0049] The above-mentioned method for preparing sapphire structural components utilizes a modified polyester resin and modified acrylic resin compound system, enabling the ink curing layer to achieve high adhesion on sapphire substrates that have not undergone plasma cleaning, thus saving investment in plasma cleaning equipment and process time. Through the gradient crosslinking of modified polyester resin and modified acrylic resin, as well as the dual crosslinking network of coupling agent and isocyanate curing agent, the ink curing layer achieves a balance between adhesion and hardness, flexibility and weather resistance, meeting the requirements of sapphire structural components for high precision, high reliability and long lifespan of the ink film.

[0050] In one embodiment, after the cooling process, in which the sapphire cured part is cooled to room temperature to obtain the sapphire structural part, the following steps are further included: Conductive adhesive is applied to the surface of the ink-cured layer on the back of the sapphire structural component; The sapphire structural component is placed in an electrostatic device for electrostatic treatment, so that the light-shielding material adheres to the surface of the conductive adhesive under the action of an electrostatic field. After the light-shielding material is attached, the sapphire structural component is removed, and the conductive adhesive is cured to fix the light-shielding material to the surface of the ink curing layer, thereby enhancing the light-shielding properties of the ink curing layer.

[0051] Understandably, when pad printing ink onto the back of sapphire structural components, insufficient light shielding in the cured ink layer, especially when the ink layer thickness is less than 5μm, can easily lead to light leakage, necessitating improved light shielding. By fixing a light-shielding material to the surface of the cured ink layer, its light shielding is enhanced. The conductive adhesive comprises acrylate or polyurethane resin, graphite powder, and a curing agent. The acrylate or polyurethane resin serves as the base resin, acting as a film-forming and adhesive agent; the graphite powder acts as a conductive filler to enhance the conductivity of the adhesive layer; and the curing agent improves the cohesive strength of the cured adhesive layer and the firmness of the light-shielding material. The curing agent is an aliphatic polyamine curing agent or an isocyanate-based water-based curing agent; the light-shielding material is ultra-fine black fiber flocking, which is made of one of ultra-fine nylon fiber, ultra-fine polyester fiber, and ultra-fine viscose fiber, with a length of 0.3mm-0.5mm; when curing the conductive flocking adhesive, the curing temperature is 80℃-120℃, and the curing time is 20min-30min; after the black ultra-fine fiber flocking is electrostatically implanted into the conductive adhesive layer, a dense black velvet light-shielding layer is formed on the back of the sapphire structural component. Through the synergistic effect of the light-shielding layer and the underlying ink curing layer, the overall light-shielding performance of the back of the sapphire structural component meets the strict requirements of the dial for light leakage; the light-shielding layer is composed of vertically arranged ultra-fine fiber flocking. When the back of the dial makes slight contact or vibrates with the bracket or movement, the ultra-fine fiber flocking absorbs the impact energy and provides cushioning, reducing direct hard contact between the ink curing layer and hard parts, and reducing the risk of friction, wear, and abnormal noise between the back of the dial and adjacent parts.

[0052] Furthermore, in one embodiment, after the light-shielding material is attached, the sapphire structural component is removed, and the conductive adhesive is cured. Before assembling the sapphire structural component, the following steps are also included: A roller brush is used to brush the surface of the light-shielding layer to remove loose fibers that are not firmly attached. The loose fibers brushed off are sucked up and recovered using a vacuum system; Ultrasonic cleaning is used for deep cleaning. Clean compressed air is used to blow away the surface of the light-shielding layer.

[0053] In this embodiment, a roller brush is used to remove loose fibers from the surface of the light-shielding layer and the fiber roots; vacuum suction can be used to collect the brushed-off fibers in a timely manner, reducing the secondary adhesion to the surface of the light-shielding layer or their dispersion into the working environment; ultrasonic cleaning is used to deeply clean the light-shielding layer, and the cavitation effect is used to remove the tiny fibers embedded in the fiber gaps; clean compressed air is used to blow the surface of the light-shielding layer, so that there are no loose fiber residues on the sapphire structural components before assembly.

[0054] Compared with the prior art, this disclosure has at least the following advantages: The aforementioned sapphire substrate pad printing ink uses modified polyester resin as the dominant component of the resin system. The modified polyester resin molecular chain contains a large number of polar ester bonds and hydroxyl groups, exhibiting excellent wetting ability on low surface energy substrates, effectively reducing the contact angle of the ink on the sapphire surface and improving spreadability. The polyester resin preferentially reacts with the curing agent, rapidly establishing a cross-linked framework and providing interfacial adhesion. Acrylic resin gradually participates in the reaction during the subsequent high-temperature curing stage, providing hardness and abrasion resistance, thus forming a differentiated curing cross-linking network. This allows the cured ink to balance adhesion and hardness. Through the inorganic end of the coupling agent chemically bonding with the sapphire surface, and the organic end reacting with the hydroxyl and carboxyl groups of the modified polyester and modified acrylic resins to integrate into the polyurethane cross-linking network, a dual effect is achieved with the cured cross-linking network, further enhancing adhesion to the sapphire substrate. The sapphire substrate pad printing ink achieves high adhesion on the inert surface of sapphire without plasma cleaning, simplifying the process, reducing costs, and improving yield.

[0055] The embodiments of this application will be described in detail below with reference to examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0056] In the specific embodiments described below, the measurement parameters involving raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.

[0057] It should be understood that in the various embodiments of this application, the order of the above-mentioned processes does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0058] Example 1

[0059] Add 35 parts of Vylon 630 modified saturated polyester resin, 20 parts of Desmophen A 365 modified saturated polyester resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersed mixture. Grind the dispersed mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse at r / min for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir evenly, and let stand to defoam for 5-10 min.

[0060] Preparation of sapphire structural components: Pad printing ink was applied to sapphire glass substrates that had not undergone plasma cleaning, and then cured by baking at 150°C for 30 min; the performance of the pad printing ink for the sapphire structural components was tested.

[0061] Example 2

[0062] The difference from Example 1 is that the proportion of amorphous copolyester resin is increased to 40 parts, and the proportion of hydroxyl acrylic resin is reduced to 15 parts.

[0063] Add 40 parts of Vylon 630 amorphous copolyester resin, 15 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0064] Example 3

[0065] The difference from Example 2 is that the proportion of amorphous copolyester resin is increased to 45 parts, and the proportion of hydroxyl acrylic resin is reduced to 10 parts.

[0066] Add 45 parts of Vylon 630 amorphous copolyester resin, 10 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0067] Example 4

[0068] The difference from Example 1 is that the proportion of amorphous copolyester resin is increased to 30 parts, and the proportion of hydroxyl acrylic resin is reduced to 25 parts.

[0069] Add 30 parts of Vylon 630 amorphous copolyester resin, 25 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0070] Example 5

[0071] The difference from Example 1 is that the proportion of hydroxyl acrylic resin is increased to 30 parts, and the proportion of non-crystalline copolyester resin is reduced to 25 parts.

[0072] Add 25 parts of Vylon 630 amorphous copolyester resin, 30 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0073] Example 6

[0074] The difference from Example 1 is that the non-crystalline copolyester resin is replaced with Vylon BX-7000A.

[0075] Add 35 parts of Vylon BX-7000A amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0076] Example 7

[0077] The difference from Example 1 is that the amount of fumed silica used is reduced to 3 parts.

[0078] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 3 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0079] Example 8

[0080] The difference from Example 1 is that the amount of fumed silica is increased to 10 parts.

[0081] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 10 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersed mixture. Grind the dispersed mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a constant speed for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0082] Example 9

[0083] The difference from Example 1 is that the amount of curing agent used is reduced.

[0084] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a speed of 100 rpm for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:5, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0085] Example 10

[0086] The difference from Example 1 is that the amount of curing agent used is increased.

[0087] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a speed of 100 rpm for 5-10 min to obtain component A. Before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:10, stir well, and let stand for 5-10 min to defoam. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0088] Comparative Example 1 The difference from Example 1 is that only non-crystalline copolyester resin is used, and hydroxyl-free acrylic resin is not used.

[0089] Add 55 parts of Vylon 630 amorphous copolyester resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the rotation speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersed mixture. Grind the dispersed mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min for 5-10 min. Minutes were collected to obtain component A. Before use, Desmodur® N75 curing agent was added at a mass ratio of component A:component B = 100:8, stirred evenly, and allowed to stand for 5-10 minutes to defoam. The pad printing ink was then transferred onto a sapphire glass substrate that had not undergone plasma cleaning and baked at 150°C for 30 minutes for curing. Performance tests were performed on the pad printing ink for the sapphire structural components.

[0090] Comparative Example 2 The difference from Example 1 is that only hydroxyl acrylic resin is used, and no non-crystalline copolyester resin is used.

[0091] Add 55 parts of Desmophen A 365 hydroxy acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the rotation speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min for 5-10 min. Minutes were collected to obtain component A. Before use, Desmodur® N75 curing agent was added at a mass ratio of component A:component B = 100:8, stirred evenly, and allowed to stand for 5-10 minutes to defoam. The pad printing ink was then transferred onto a sapphire glass substrate that had not undergone plasma cleaning and baked at 150°C for 30 minutes for curing. Performance tests were performed on the pad printing ink for the sapphire structural components.

[0092] Comparative Example 3 The difference from Example 1 is that the two resins are compounded but without the silane coupling agent KH-560.

[0093] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, increase the rotation speed to 800-1200 r / min, and disperse for 10-15 min to obtain a dispersed mixture. Grind the dispersed mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture, excluding KH-560, and disperse at 300-500 r / min for 5-10 min. Min, obtain component A; before use, add Desmodur® N75 curing agent at a mass ratio of component A: component B = 100:8, stir evenly, and let stand for 5-10 minutes to defoam. Transfer the pad printing ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 minutes to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0094] Comparative Example 4 The difference from Example 1 is that the two resins are compounded but no curing agent is added.

[0095] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black, 15 parts of Printex 35 carbon black, and 7 parts of AEROSIL 200 fumed silica to the premix sequentially, and increase the speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersion mixture. Grind the dispersion mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min. Disperse the ink at a speed of 10 r / min for 5-10 min to obtain component A; do not add curing agent N75. Transfer the ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 min. Perform performance tests on the pad printing ink for the sapphire structural parts.

[0096] Comparative Example 5 The difference from Example 1 is that no fumed silica is added.

[0097] Add 35 parts of Vylon 630 amorphous copolyester resin, 20 parts of Desmophen A 365 hydroxyl acrylic resin, 2 parts of BYK-163 superdispersant, and the first part of the mixed diluent to a dispersion tank and disperse at 300-500 r / min for 5-10 min to obtain a premix. Add 5 parts of Monarch 1100 carbon black and 15 parts of Printex 35 carbon black to the premix sequentially, without adding AEROSIL 200, and increase the rotation speed to 800-1200 r / min and disperse for 10-15 min to obtain a dispersed mixture. Grind the dispersed mixture four times using a three-roll mill until the fineness is ≤8 μm to obtain a ground mixture. Add 2 parts of KH-560 silane coupling agent, 1 part of BYK-358N leveling agent, 1 part of BYK-051 defoamer, and the remaining mixed diluent to the ground mixture and disperse at 300-500 r / min for 5-10 min. Min, obtain component A; before use, add Desmodur® N75 curing agent at a mass ratio of component A:component B = 100:8, stir evenly, and let stand for 5-10 minutes to defoam. Transfer the pad printing ink onto a sapphire glass substrate that has not undergone plasma cleaning, and bake at 150℃ for 30 minutes to cure. Perform performance tests on the pad printing ink for sapphire structural components.

[0098] It should be noted that the raw materials used in the examples and comparative examples came from the following sources: Modified saturated polyester resin 1: Toyobo Vylon 630, hydroxyl value ≈ 5 mg KOH / g, acid value ≤ 4 mg KOH / g, Tg ≈ 55℃.

[0099] Modified saturated polyester resin 2: Vylon BX-7000A, hydroxyl value 3-8 mgKOH / g, acid value <2 mgKOH / g.

[0100] Modified hydroxyl acrylic resin: Covestro Desmophen® A 365, Tg≈55℃, Silane coupling agent: γ-glycidoxypropyltrimethoxysilane (KH-560) Curing agent: Covestro Desmodur® N75 (HDI trimer, NCO content 16.5±0.5%); Superdispersant: BYK-163 (superdispersant for carbon black); Leveling agent: BYK-358N (polyacrylate leveling agent, improves leveling and prevents pinholes); Defoamer: BYK-051 (a non-silicone defoamer for solvent-based inks, with good compatibility); Filler: Evonik AEROSIL® 200 fumed silica; Pigments: Cabot Monarch 1100 carbon black, Orion Printex 35 Diluent: Isophorone (IP): Propylene glycol methyl ether acetate (PMA): Cyclohexanone (CYC) in a ratio of 1:1:1.

[0101] It should be noted that the performance testing method is as follows: Adhesion: Compliance test according to GB / T 13217.7-2023 (100-cross test). Alcohol resistance: With a 500g load, wipe with a white lint-free cloth soaked in 99.5% anhydrous ethanol 50 times and observe whether there is discoloration or dissolution; Water resistance: Place in 100℃ water and boil for 4 hours, then remove and cool to room temperature to observe the appearance and test the adhesion. Resistance to stripping: Ultrasonic cleaning in stripping solution at 70℃ for 10 minutes, observe whether the scribing area is chipped or peeled off and measure the adhesion; High temperature and high humidity: Place at 60℃ / 90%RH for 240h, observe the appearance and test the adhesion; Weather resistance: Xenon lamp aging at 1.22W / cm² 2 After 200 hours, observe yellowing and measure adhesion. Printing effect: Observe under a 10x magnifying glass whether the edges of 0.2mm fine lines are clear and whether there are any jagged edges or roughness.

[0102] Table 1 shows the performance test results for the examples and comparative examples.

[0103] As shown in the table above, the examples differ from the comparative examples in that: Comparative Examples 1 and 2 showed poor adhesion, water-resistant adhesion, plating-resistant adhesion, UV-resistant adhesion, and printing edge performance, indicating that a single resin cannot simultaneously meet the requirements of adhesion, hardness, and weather resistance.

[0104] Examples 1-6 and 9-10 show that the adhesion, water-boiling resistance, plating removal resistance, high-temperature and high-humidity adhesion, UV aging resistance, and printing edge performance are generally better than those of Comparative Examples 1-5. This indicates that by using a modified saturated polyester resin and a modified hydroxyl acrylic resin, along with a silane coupling agent, isocyanate curing agent, and fumed silica, a comprehensive balance of adhesion, chemical resistance, weather resistance, and printability can be achieved on a sapphire substrate. Compared with Example 1, Comparative Example 3 showed that the adhesion decreased from 5B to 3-4B, the water resistance decreased from 5B to 2B, and the resistance to plating removal decreased from 5B to 2B. This indicates that without KH-560 coupling agent, the ink and the sapphire surface cannot form an effective chemical bridge, and the adhesion, water resistance, and plating removal performance deteriorated significantly. This shows that the coupling agent is the key component to solve the adhesion problem of the inert surface of sapphire. Compared to Example 1, Example 7 reduced the amount of fumed silica from 7 parts to 3 parts. While adhesion, water resistance, plating removal resistance, and UV aging resistance remained at 5B, the printed edges showed "very slight serrations," indicating that insufficient fumed silica resulted in insufficient ink thixotropy and reduced ink spreading control on the silicone head and substrate surface during pad printing, leading to decreased pattern edge precision. In Example 8, compared to Example 1, the amount of fumed silica increased from 7 parts to 10 parts. The printed edges were clear and serrated, but adhesion decreased from 5B to 4B. Water resistance and plating removal adhesion also decreased from 5B to 4B. This indicates that excessive fumed silica resulted in high system viscosity, decreased ink wettability on the sapphire substrate, and increased internal stress in the cured film, leading to deterioration in adhesion, water resistance, and plating removal resistance.

[0105] Compared with Example 1, the ink in Comparative Example 4 could not be cured and all performances failed to meet the standards, indicating that isocyanate curing agent is a necessary condition for the formation of cross-linked network. Compared with Example 1, although the adhesion of Comparative Example 5 met the standards, obvious jagged edges appeared at the printing edges, indicating that the ink thixotropy was insufficient when fumed silica was lacking, and the accuracy of the pad printing pattern could not meet the requirements.

[0106] The above comparison of the comparative examples and embodiments fully demonstrates that there is a synergistic effect among the modified polyester resin, modified acrylic resin, coupling agent, curing agent and fumed silica in the technical solution of this application, which together achieve the comprehensive performance of 5B adhesion, 5B water boiling resistance, 5B anti-chipping resistance, 5B UV aging resistance without yellowing and clear printing edges without jaggedness on sapphire substrates that have not been plasma cleaned.

[0107] The embodiments described above merely illustrate several implementation methods of this application to facilitate a detailed understanding of the technical solutions of this application, but should not be construed as limiting the scope of protection of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Furthermore, it should be understood that after reading the above teachings of this application, those skilled in the art can make various alterations or modifications to this application, and the equivalent forms obtained also fall within the scope of protection of this application. It should also be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided in this application through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this patent application should be determined by the content of the appended claims, and the specification and drawings can be used to interpret the content of the claims.

Claims

1. A pad printing ink for sapphire substrate, characterized in that, It includes component A and component B, wherein component A has the following mass components: 30-40 parts of modified polyester resin; 15-25 parts of modified acrylic resin; 5-10 parts of filler; 15-25 parts carbon black; 1-3 parts coupling agent; 1-4 parts of auxiliary agent; 10-20 parts diluent; Component B is an isocyanate curing agent; The mass ratio of component A to component B is 100:(8-20).

2. The sapphire substrate pad printing ink according to claim 1, characterized in that, The coupling agent is γ-glycidoxypropyltrimethoxysilane.

3. The sapphire substrate pad printing ink according to claim 1, characterized in that, The modified polyester resin is a non-crystalline copolyester resin.

4. The sapphire substrate pad printing ink according to claim 3, characterized in that, The hydroxyl value of the amorphous copolyester resin is 3mgKOH / g-12mgKOH / g, and the acid value of the amorphous copolyester resin is ≤5mgKOH / g.

5. The sapphire substrate pad printing ink according to claim 1, characterized in that, The diluent is at least one of isophor, propylene glycol methyl ether acetate, and cyclohexanone.

6. The sapphire substrate pad printing ink according to claim 1, characterized in that, The filler is fumed silica.

7. The sapphire substrate pad printing ink according to claim 1, characterized in that, The additives include a superdispersant, a defoamer, and a leveling agent; and / or, the mass ratio of the superdispersant, the defoamer, and the leveling agent is (1-3):(0.5-1.5):(0.5-1.5).

8. The sapphire substrate pad printing ink according to claim 1, characterized in that, The isocyanate curing agent is HDI biuret.

9. A method for preparing a sapphire substrate pad printing ink, characterized in that, The method for preparing the sapphire substrate pad printing ink according to any one of claims 1-8 includes the following steps: pre-dispersion treatment, mixing and dispersing modified polyester resin, modified acrylic resin, dispersant and part of diluent, dispersing speed of 300 r / min-500 r / min, dispersion time of 5 min-10 min, to obtain a premix; For the filler dispersion treatment, carbon black and filler are added sequentially to the premix, the dispersion speed is increased to 800 r / min-1200 r / min, and the dispersion time is 10 min-15 min to obtain a dispersed mixture; The dispersion mixture is ground to a fineness of ≤8μm to obtain a ground mixture. Additive dispersion treatment: Coupling agent, leveling agent, defoamer and remaining diluent are added to the grinding mixture. The speed is 300r / min-500 and the dispersion time is 5min-10min. After uniform mixing, component A is obtained. The mixing process involves uniformly mixing component A and component B at a mass ratio of 100:(8-20), wherein component B is an isocyanate curing agent, to obtain sapphire substrate pad printing ink.

10. A method for preparing a sapphire structural component, characterized in that, The process of fabricating using the sapphire substrate pad printing ink prepared according to claim 9 includes the following steps: Ink pad printing, the sapphire substrate is not plasma cleaned before pad printing. The pad printing equipment is used to transfer pad printing ink onto the sapphire substrate to form an ink pad printing layer, thereby obtaining a pad printing substrate; Baking and curing: The pad printing substrate is baked and cured at a temperature of 120℃-150℃ for 20min-40min. After the pad printing layer is cured, an ink curing layer is obtained to obtain a sapphire cured part. Cooling treatment is performed to cool the sapphire cured part to room temperature to obtain a sapphire structural part.

Citation Information

Patent Citations

  • A 3D mobile phone back cover pad printing ink, its preparation method and application

    CN118725642B