A high-performance antibacterial and formaldehyde-removing negative ion coating and its preparation method

By combining water-based composite emulsions and modified negative ion powders, a stable coating system is constructed, which solves the problems of single function and rapid performance degradation of existing coatings. It achieves long-lasting antibacterial, formaldehyde removal and efficient negative ion release, and improves the film-forming stability and service life of the coating.

CN123107469APending Publication Date: 2026-11-17YUANYANGXING (CHONGQING) HEALTH TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611003573.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing antibacterial, formaldehyde-removing, and negative ion coatings have limited functionality, rapid performance degradation, and poor component compatibility, failing to meet the multiple requirements of long-lasting antibacterial effect, efficient formaldehyde removal, stable release of high-concentration negative ions, low VOC, and stain resistance and durability.

Method used

By combining water-based composite emulsion, modified negative ion powder, composite nano antibacterial and formaldehyde-removing agent and porous adsorption filler, and through high-temperature calcination, surface activation with coupling agent and polymerization grafting modification process, a stable coating system is constructed to ensure uniform adhesion and long-lasting activity of functional components.

Benefits of technology

It achieves long-lasting purification, antibacterial and anti-mildew properties of the coating, improves negative ion release efficiency and formaldehyde degradation efficiency, improves film-forming stability and interfacial adhesion performance, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

This application relates to the field of coating preparation technology, specifically disclosing an antibacterial and formaldehyde-removing high-performance negative ion coating and its preparation method. The antibacterial and formaldehyde-removing high-performance negative ion coating comprises the following raw materials: water-based composite emulsion, modified negative ion powder, composite nano antibacterial and formaldehyde-removing agent, porous adsorption filler, dispersant, defoamer, film-forming aid, wetting agent, preservative and mildew inhibitor, thickener, and deionized water. The preparation method of the antibacterial and formaldehyde-removing high-performance negative ion coating is as follows: an inorganic functional slurry and a coating base are prepared separately; the inorganic functional slurry is added to the coating base, stirred evenly at a constant temperature, the modified negative ion powder is added, mixed evenly, the defoamer and thickener are added, stirred evenly, and allowed to stand for curing to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating. The prepared antibacterial and formaldehyde-removing high-performance negative ion coating exhibits excellent comprehensive performance, strong adhesion, a firm bond between the coating and the substrate, high formaldehyde removal rate and antibacterial rate, excellent mildew resistance, and long-lasting release of negative ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of coating preparation technology, and more specifically, it relates to an antibacterial and formaldehyde-removing high-performance negative ion coating and its preparation method. Background Technology

[0002] With the increasing health awareness of the public and the widespread adoption of indoor decoration, indoor air pollution has become the third major form of environmental pollution after coal smoke pollution and photochemical smog pollution, seriously threatening human health. There are over 500 kinds of volatile organic compounds (VOCs) in indoor air, among which formaldehyde, benzene, and TVOCs are the most harmful carcinogens / pathogens. As the building material covering the largest area indoors, paint's environmental and functional properties directly determine indoor air quality. Traditional interior wall paints only meet basic decorative and protective needs, but their single function, high VOC content, susceptibility to mold and bacterial growth, and lack of long-term purification capabilities for harmful substances like formaldehyde make them unsuitable for the market demand for healthy living spaces.

[0003] To address these issues, functional coatings with antibacterial, formaldehyde-removing, and negative ion properties have become a hot research topic in the industry. Currently, negative ion coatings primarily use tourmaline, rare earth materials, or nano-titanium dioxide as core functional components. Tourmaline relies on temperature and humidity changes to release negative ions, resulting in low release rates, poor stability, and rapid long-term decay; its typical release concentration is only 800–2200 ions / cm³, making sustained air purification difficult. While rare earth-doped TiO2 can synergistically remove formaldehyde and release negative ions, its weak visible light response, low quantum efficiency, and tendency for nanoparticles to aggregate lead to low formaldehyde removal efficiency and rapid decay of antibacterial properties. Although porous aluminosilicate-supported materials offer good slow-release properties, their initial negative ion concentration is low, resulting in significant shortcomings in overall performance.

[0004] Current antibacterial and formaldehyde-removing coatings generally suffer from technical bottlenecks such as poor functional compatibility, weak interfacial compatibility, and insufficient durability. Antibacterial components and negative ion materials easily inhibit each other, leading to poor antibacterial effects and a simultaneous decline in negative ion release and formaldehyde removal efficiency. Functional fillers have weak interfacial bonding with the polymer matrix, easily agglomerating and settling, and the film is prone to cracking and peeling after formation, resulting in a shortened lifespan. Most products can only achieve a single function and cannot simultaneously meet the multiple requirements of long-lasting antibacterial effect, efficient formaldehyde removal, stable release of high-concentration negative ions, low VOC, and stain resistance and durability. In summary, existing antibacterial, formaldehyde-removing, and negative ion coatings suffer from defects such as single function, rapid performance degradation, poor component compatibility, and insufficient construction stability. Therefore, there is an urgent need to develop a high-performance negative ion coating that is multi-functional, synergistic, stable, environmentally friendly, and durable to address the core pain points of current indoor air purification and health protection. Summary of the Invention

[0005] To address the technical problems mentioned in the background section, this application provides an antibacterial and formaldehyde-removing high-performance negative ion coating and its preparation method.

[0006] Firstly, this application provides an antibacterial and formaldehyde-removing high-performance negative ion coating, which adopts the following technical solution: A high-performance negative ion coating for antibacterial and formaldehyde removal, comprising the following raw materials by weight: 40-60 parts of water-based composite emulsion, 8-15 parts of modified negative ion powder, 3-8 parts of composite nano antibacterial and formaldehyde-removing agent, 10-20 parts of porous adsorption filler, 0.8-1.5 parts of dispersant, 0.3-0.8 parts of defoamer, 0.5-1.2 parts of film-forming aid, 0.2-0.5 parts of wetting agent, 0.2-0.5 parts of preservative and mildew inhibitor, 0.4-1.0 parts of thickener, and 15-25 parts of deionized water.

[0007] Preferably, the aqueous composite emulsion is composed of an acrylic emulsion, an aqueous styrene-butadiene emulsion, and a silicone-modified acrylic emulsion; wherein the amount of the aqueous styrene-butadiene emulsion added is 12-20% of the total mass of the acrylic emulsion and the silicone-modified acrylic emulsion, and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4-7:1-3.

[0008] Preferably, the preparation method of the modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline, sieve it, calcine it at high temperature, and then let it cool naturally to obtain pretreated tourmaline powder; Step 2: Mix pretreated tourmaline powder with anhydrous ethanol and disperse at high speed to obtain a suspension; add coupling agent to the suspension, heat and stir at a constant temperature to obtain activated tourmaline suspension; add composite monomer and initiator to activated tourmaline suspension, heat and polymerize at a constant temperature under nitrogen protection, centrifuge, wash, vacuum dry, pulverize and sieve to obtain modified negative ion powder.

[0009] Preferably, the high-temperature calcination treatment in step 1 specifically involves heating to 550-650℃ at a heating rate of 5-8℃ / min and calcining at high temperature for 2-3 hours.

[0010] Preferably, in step 2, the mass ratio of activated tourmaline suspension, composite monomer and initiator is 80-100: 8-15: 0.3-0.8.

[0011] Preferably, in step 2, the composite monomer is composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5-8:1-3.

[0012] Preferably, the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3-5:2-4:1-2.

[0013] Preferably, the porous adsorption filler is one or more of zeolite powder, activated carbon powder, and attapulgite.

[0014] Preferably, the dispersant is sodium polyacrylate dispersant.

[0015] Preferably, the defoamer is a polyether-modified silicone defoamer.

[0016] Preferably, the film-forming aid is 12-ol ester.

[0017] Preferably, the wetting agent is an acetylenic diol wetting agent.

[0018] Preferably, the preservative and antifungal agent is an isothiazolinone-based antifungal agent.

[0019] Preferably, the thickener is a nonionic polyurethane associative thickener.

[0020] Secondly, this application also provides a method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating, using the following technical solution: A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Add dispersant and wetting agent to deionized water, stir at low speed for 3-5 minutes, mix evenly, add porous adsorption filler and composite nano antibacterial and formaldehyde-removing agent, disperse at high speed for 15-20 minutes to obtain inorganic functional slurry; add water-based composite emulsion to deionized water, stir at low speed, add film-forming aid and anti-corrosion and anti-mildew agent in sequence during stirring, continue stirring to obtain coating base; add inorganic functional slurry to coating base, heat to 40-50℃, stir evenly at constant temperature, add modified negative ion powder, continue high-speed dispersion, mix evenly, reduce stirring speed, add defoamer, stir at low speed, add thickener, stir evenly, let stand to mature, to obtain antibacterial and formaldehyde-removing high-performance negative ion coating.

[0021] In summary, this application has the following beneficial effects: This application constructs a ternary aqueous composite emulsion system composed of acrylic emulsion, waterborne styrene-butadiene emulsion, and silicone-modified acrylic emulsion. Leveraging the complementary and synergistic properties of the three emulsions, the aqueous composite emulsion system exhibits excellent film-forming flexibility, density, and interfacial adhesion. Specifically, the acrylic emulsion ensures the basic film-forming properties and stability of the coating, the silicone-modified acrylic emulsion enhances the coating's weather resistance and hydrophobic protective properties, and the appropriate amount of waterborne styrene-butadiene emulsion effectively optimizes the crosslinking density and adhesion of the emulsion system, significantly improving industry pain points such as easy cracking, poor adhesion, and loose coating after film formation. The stable and dense cross-linked film structure not only ensures that the dry film adhesion of the coating reaches a stable level of 0, achieving a firm bond between the coating and the polymer substrate, but also provides a uniform and stable attachment carrier for functional components such as modified negative ion powder, composite nano antibacterial and formaldehyde removal agent, and porous adsorption filler in the system. This prevents the functional filler from agglomerating and falling off, and maximizes the retention of the activity of various functional components. From the film-forming substrate level, it ensures the coating's core performance of long-lasting purification, antibacterial and mildew prevention.

[0022] This application employs an integrated modification process for tourmaline negative ion powder, involving high-temperature calcination pretreatment, surface activation with coupling agents, and polymer grafting modification. High-temperature calcination pretreatment effectively removes impurities and crystal water from the tourmaline powder, unclogs the microporous structure within the powder, and activates its negative ion release activity, significantly improving its negative ion release efficiency and sustainability. Combined with subsequent composite monomer grafting polymerization modification, a stable organic modified layer can be constructed on the surface of the tourmaline powder, further enhancing the powder's stability and avoiding problems such as powder sedimentation and activity decay. Ultimately, this results in modified negative ion powder possessing a long-lasting and stable negative ion release capability.

[0023] This application utilizes a composite monomer system of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate to synergistically graft and modify tourmaline powder. This allows the two monomers to fully exert their synergistic effect, overcoming the performance limitations of single fluorinated monomer modification and significantly optimizing the powder's surface structure and functional properties. The two fluorinated monomer composite system can form a uniform and dense modified coating layer on the tourmaline powder surface. This modified structure can efficiently synergize with the composite antibacterial and formaldehyde-removing agent composed of nano-titanium dioxide, nano-zinc oxide, and sepiolite within the system, enhancing the dual effects of physical adsorption and photocatalytic degradation of the negative ion coating, and significantly improving its formaldehyde degradation efficiency and broad-spectrum antibacterial ability. Detailed Implementation

[0024] The present application will be further described in detail below with reference to the embodiments.

[0025] The acrylic emulsion used in the embodiments and comparative examples of this application was purchased from Guangzhou Qiyuan New Materials Co., Ltd.; the water-based styrene-butadiene emulsion was purchased from Dongguan Xinrui New Materials Co., Ltd.; the organosilicon-modified acrylic emulsion was purchased from Cansen Chemical New Materials (Shenzhen) Co., Ltd.; the nano titanium dioxide was purchased from Hebei Tengbimetallic Materials Co., Ltd.; the nano zinc oxide was purchased from Qinghe County Chaotai Metal Materials Co., Ltd.; the sepiolite was purchased from Lingshou County Jinhong New Materials Co., Ltd.; the zeolite powder was purchased from Lingshou County Yehui Mineral Products Co., Ltd.; the activated carbon powder was purchased from Jinan Mingjiang Chemical Co., Ltd.; and the attapulgite was purchased from [unclear - possibly a company name]. The following products were purchased from Lingshou County Laipeng Mineral Products Business Department: Sodium polyacrylate dispersant from Pande (Shanghai) International Trade Co., Ltd.; Polyether modified silicone defoamer from Shanghai Zhenlishi Network Technology Co., Ltd.; Acetylene diol wetting agent from Wuhan Boli New Materials Co., Ltd.; Isothiazolinone mildew inhibitor from Hubei Xingyan New Materials Technology Co., Ltd.; Nonionic polyurethane associative thickener from Greenlink (Jining) Chemical Technology Co., Ltd.; Dodecafluoroheptyl methacrylate from Wuhan Shuer Biotechnology Co., Ltd.; and Hexafluorobutyl acrylate from Jinan Qitian Chemical Co., Ltd.

[0026] Examples 1-3 provide an antibacterial and formaldehyde-removing high-performance negative ion coating and its preparation method.

[0027] Example 1 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 12%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0028] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and benzoyl peroxide were heated to 75°C under nitrogen protection and polymerized at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 80:8:0.3. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5:1.

[0029] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0030] Example 2 A high-performance negative ion coating for antibacterial and formaldehyde removal, comprising the following raw materials by weight: 50 parts of water-based composite emulsion, 12 parts of modified negative ion powder, 5 parts of composite nano antibacterial and formaldehyde-removing agent, 15 parts of porous adsorption filler, 1.2 parts of dispersant, 0.5 parts of defoamer, 0.8 parts of film-forming aid, 0.4 parts of wetting agent, 0.4 parts of preservative and mildew inhibitor, 0.7 parts of thickener, and 20 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is equal to the amount added to the acrylic emulsion. The liquid and the silicone-modified acrylic emulsion together account for 16% of the total mass; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 6:2; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 4:3:1.5; the porous adsorption filler is activated carbon powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0031] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through a 1000-mesh sieve. Heat the tourmaline to 600°C at a heating rate of 7°C / min. After high-temperature calcination for 2.5 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1.5:10. Disperse the mixture at room temperature with a stirring speed of 1100 rpm for 15 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to 4% of the mass of the pretreated tourmaline powder. Heat to 65℃ and stir at a stirring speed of 250 rpm for 1.5 hours to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and other compounds were heated to 80°C under nitrogen protection and polymerized at a stirring speed of 250 rpm for 3.5 h. After centrifugation at 7000 rpm for 25 min, the mixture was washed three times with anhydrous ethanol, vacuum dried at 65°C for 10 h under a vacuum of -0.09 MPa, and pulverized through a 1000-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 90:12:0.5. The composite monomer consisted of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 7:2.

[0032] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 65 wt% deionized water and stirred at 250 rpm at room temperature for 4 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 1000 rpm at room temperature for 18 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 35 wt% deionized water and stirred at 250 rpm at room temperature for 15 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 250 rpm at room temperature. Mix for 25 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 45℃, stir at a constant temperature for 35 minutes, then add the modified negative ion powder, and continue to disperse at high speed for 25 minutes at 45℃ with a stirring speed of 1000 rpm. After mixing evenly, reduce the stirring speed to 150 rpm, add the defoamer at 45℃, stir at low speed for 8 minutes, then add the thickener, and stir at room temperature for 15 minutes with a stirring speed of 150 rpm. After mixing evenly, let it stand at room temperature for 18 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0033] Example 3 A high-performance negative ion coating for antibacterial and formaldehyde removal, comprising the following raw materials by weight: 60 parts of water-based composite emulsion, 15 parts of modified negative ion powder, 8 parts of composite nano antibacterial and formaldehyde-removing agent, 20 parts of porous adsorption filler, 1.5 parts of dispersant, 0.8 parts of defoamer, 1.2 parts of film-forming aid, 0.5 parts of wetting agent, 0.5 parts of preservative and mildew inhibitor, 1.0 part of thickener, and 25 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 20%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 7:3; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 5:4:2; the porous adsorption filler is attapulgite, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0034] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through a 1200-mesh sieve. Heat the tourmaline to 650°C at a heating rate of 8°C / min. After high-temperature calcination for 3 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 2:12. Disperse the mixture at room temperature with a stirring speed of 1200 rpm for 20 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to 5% of the mass of the pretreated tourmaline powder. Heat to 70℃ and stir at a stirring speed of 300 rpm for 2 hours to obtain an activated tourmaline suspension. Add composite monomers and... Benzoyl peroxide was polymerized at 85°C under nitrogen protection with a stirring speed of 300 rpm for 4 hours. After centrifugation at 8000 rpm for 30 minutes, it was washed three times with anhydrous ethanol, vacuum dried at 70°C for 12 hours under a vacuum of -0.09 MPa, and pulverized through a 1200-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 100:15:0.8. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 8:3.

[0035] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 70 wt% deionized water and stirred at 300 rpm at room temperature for 5 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 1200 rpm at room temperature for 20 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 30 wt% deionized water and stirred at 300 rpm at room temperature for 20 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 300 rpm at room temperature for 3 minutes. 0 min, to obtain the coating base material; add the inorganic functional slurry to the coating base material, heat to 50℃, stir at a constant temperature for 40 min, then add the modified negative ion powder, stir at a stirring speed of 1200 rpm, continue to disperse at high speed for 30 min at 50℃, after mixing evenly, reduce the stirring speed to 200 rpm, add the defoamer at 50℃, stir at low speed for 10 min, then add the thickener, stir at a stirring speed of 200 rpm, stir at room temperature for 10-20 min, stir evenly, let stand at room temperature for 24 h to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0036] Comparative Example 1 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 5%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0037] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and benzoyl peroxide were heated to 75°C under nitrogen protection and polymerized at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 80:8:0.3. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5:1.

[0038] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0039] Comparative Example 2 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 30%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0040] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and benzoyl peroxide were heated to 75°C under nitrogen protection and polymerized at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 80:8:0.3. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5:1.

[0041] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0042] Comparative Example 3 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 12%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 1:4; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0043] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and benzoyl peroxide were heated to 75°C under nitrogen protection and polymerized at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 80:8:0.3. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5:1.

[0044] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0045] Comparative Example 4 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 12%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0046] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Hexafluorobutyl acrylate and benzoyl peroxide were added to a tourmaline suspension. Under nitrogen protection, the temperature was raised to 75°C, and the polymerization reaction was carried out at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, hexafluorobutyl acrylate, and benzoyl peroxide was 80:8:0.3.

[0047] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0048] Comparative Example 5 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 12%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0049] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add the activated tourmaline... Dodecyl fluoroheptyl methacrylate and benzoyl peroxide were added to the tourmaline suspension. Under nitrogen protection, the temperature was raised to 75°C, and the polymerization reaction was carried out at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, dodecyl fluoroheptyl methacrylate, and benzoyl peroxide was 80:8:0.3.

[0050] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0051] Comparative Example 6 A high-performance antibacterial and formaldehyde-removing negative ion coating, by weight, comprises the following raw materials: 40 parts of water-based composite emulsion, 8 parts of modified negative ion powder, 3 parts of composite nano antibacterial and formaldehyde-removing agent, 10 parts of porous adsorption filler, 0.8 parts of dispersant, 0.3 parts of defoamer, 0.5 parts of film-forming aid, 0.2 parts of wetting agent, 0.2 parts of preservative and mildew inhibitor, 0.4 parts of thickener, and 15 parts of deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is [amount missing - likely referring to acrylic acid]. The total mass of the emulsion and the silicone-modified acrylic emulsion is 12%; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3:2:1; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is nonionic polyurethane associative thickener.

[0052] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix the pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature and at a stirring speed of 1000 rpm for 10 min to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of silane coupling agent KH-570 to be 2% of the mass of the pretreated tourmaline powder. Heat the mixture to 60℃ and stir at a stirring speed of 200 rpm for 4 h. After centrifugation at 5000 rpm for 20 min, wash twice with anhydrous ethanol, vacuum dry at 60℃ for 8 h under a vacuum of -0.09 MPa, and pulverize through an 800-mesh sieve to obtain modified negative ion powder.

[0053] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0054] Comparative Example 7 A high-performance negative ion coating for antibacterial and formaldehyde removal, comprising the following raw materials by weight: 40 parts water-based composite emulsion, 8 parts modified negative ion powder, 3 parts composite nano antibacterial and formaldehyde-removing agent, 10 parts porous adsorption filler, 0.8 parts dispersant, 0.3 parts defoamer, 0.5 parts film-forming aid, 0.2 parts wetting agent, 0.2 parts preservative and mildew inhibitor, 0.4 parts thickener, and 15 parts deionized water. The water-based composite emulsion is composed of acrylic emulsion, water-based styrene-butadiene emulsion, and silicone-modified acrylic emulsion. The amount of water-based styrene-butadiene emulsion added is... The acrylic emulsion and the silicone-modified acrylic emulsion together comprise 12% of the total mass; and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4:1; the composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide and nano zinc oxide in a mass ratio of 3:2; the porous adsorption filler is zeolite powder, the dispersant is sodium polyacrylate dispersant, the defoamer is polyether-modified silicone defoamer, the film-forming aid is alcohol ester dodecyl, the wetting agent is acetylenic diol wetting agent, the preservative and mildew inhibitor is isothiazolinone mildew inhibitor, and the thickener is a nonionic polyurethane associative thickener.

[0055] The preparation method of modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline and pass it through an 800-mesh sieve. Heat the tourmaline to 550°C at a heating rate of 5°C / min. After high-temperature calcination for 2 hours, allow it to cool naturally to room temperature to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder and anhydrous ethanol at a mass ratio of 1:8. Disperse the mixture at room temperature with a stirring speed of 1000 rpm for 10 minutes to obtain a suspension. Add silane coupling agent KH-570 to the suspension, controlling the amount of KH-570 added to be 2% of the mass of the pretreated tourmaline powder. Heat to 60℃ and stir at a stirring speed of 200 rpm for 1 hour to obtain an activated tourmaline suspension. Add a composite monomer to the activated tourmaline suspension. Benzoyl peroxide and benzoyl peroxide were heated to 75°C under nitrogen protection and polymerized at a stirring speed of 200 rpm for 3 hours. After centrifugation at 5000 rpm for 20 minutes, the mixture was washed twice with anhydrous ethanol, vacuum dried at 60°C for 8 hours under a vacuum of -0.09 MPa, and pulverized through an 800-mesh sieve to obtain modified negative ion powder. The mass ratio of activated tourmaline suspension, composite monomer, and benzoyl peroxide was 80:8:0.3. The composite monomer was composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5:1.

[0056] A method for preparing an antibacterial and formaldehyde-removing high-performance negative ion coating includes the following preparation steps: Dispersant and wetting agent were added to 60 wt% deionized water and stirred at 200 rpm at room temperature for 3 minutes until homogeneous. Then, porous adsorption filler and composite nano-antibacterial and formaldehyde-removing agent were added and dispersed at 800 rpm at room temperature for 15 minutes to obtain an inorganic functional slurry. Aqueous composite emulsion was added to 40 wt% deionized water and stirred at 200 rpm at room temperature for 10 minutes. During stirring, film-forming aid and preservative / mildew inhibitor were added sequentially, and stirring was continued at 200 rpm at room temperature. Mix for 20 minutes to obtain the coating base; add the inorganic functional slurry to the coating base, heat to 40℃, stir at a constant temperature for 30 minutes, add the modified negative ion powder, stir at 800 rpm, continue high-speed dispersion at 40℃ for 20 minutes, mix evenly, reduce the stirring speed to 100 rpm, add the defoamer at 40℃, stir at low speed for 5 minutes, then add the thickener, stir at 100 rpm, stir at room temperature for 10 minutes, stir evenly, let stand at room temperature for 12 hours to obtain the antibacterial and formaldehyde-removing high-performance negative ion coating.

[0057] Performance testing The performance of the antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 of this application was tested. The specific test results are as follows: Adhesion: Referring to the national standard GB / T 9286-1998 "Cross-cut test of paint and varnish film", the antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 were respectively coated on a standard tinplate with a size of 150mm×100mm×5mm. The dry film thickness of the coating was controlled at (60±5)μm. After curing at room temperature for 7 days, a 1mm×1mm grid was drawn using a cross-cut tester. The grid area was tightly pasted with 3M 600 tape. The coating peeling in the grid area was observed, and the adhesion level was evaluated. Formaldehyde removal rate: The antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 were respectively coated on standard float glass plates (300mm×300mm), with the coating amount controlled at 120g / m². 2 Under ambient temperature (23±2)℃ and relative humidity (50±5)%, the mixture was cured for 7 days. Following the national standard GB / T 23985-2009 "Determination of Volatile Organic Compounds (VOC) Content in Paints and Varnishes - Difference Method", a 1m... 3 A sealed test chamber was used, with the internal temperature controlled at (23±2)℃ and relative humidity at (50±5)%. Formaldehyde standard gas was introduced into the test chamber, with the initial formaldehyde concentration controlled at (1.0±0.1) mg / m³. 3 The formaldehyde residual concentration in the chamber was measured after 72 hours, and the formaldehyde removal rate was calculated. The formula for calculating the formaldehyde removal rate is: ; Antibacterial rate: The antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 were coated on the surface of sterile glass plates with a size of 50mm×50mm. The dry film thickness was controlled at (60±5)μm. The plates were then cured for 7 days in a standard environment with a temperature of (23±2)℃ and a relative humidity of (50±5)% to obtain antibacterial coating samples. A blank control group (sterile glass plates of the same size without coating) was also set up. Three parallel samples were set up for each group of samples. According to the national standard GB / T 21866-2025 "Determination of Antiviral Activity and Antibacterial Properties of Coatings", common indoor pathogens, Escherichia coli (ATCC 25922) and Staphylococcus aureus (ATCC 6538), were selected as test bacteria, and the initial concentration of the bacterial solution was controlled at 1.0×10⁻⁶. 6 CFU / mL, add 0.1mL of bacterial solution to the surface of the antibacterial coating sample and the blank control group sample, and evenly coat the entire plate surface. Place all samples horizontally at (37±1)℃, relative humidity ≥90%, and continuously incubate in the dark for 24h. Use the plate count method to count the number of viable bacteria and calculate the antibacterial rate after 24h. If the antibacterial rate is ≥99%, it is judged as a strong antibacterial effect. The calculation formula is: ; Anti-mildew performance: Referring to the national standard GB / T 1741-2020 "Determination of Anti-mildew Resistance of Paint Films", the antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 were respectively coated on the surface of a 50mm×50mm sterile glass plate. The dry film thickness was controlled at (60±5)μm. The samples were cured for 7 days in a standard environment of (23±2)℃ and (50±5)% relative humidity to obtain antibacterial coating samples. A mixed strain of Aspergillus niger (CGMCC3.5487), Penicillium wanyi (CGMCC3.4253), Trichoderma viride (CGMCC3.2941), and Brachymyces buddingii (CGMCC3.837) was continuously cultured for 28 days in a constant temperature and humidity incubator at (28±2)℃ and ≥95% relative humidity. Grade 0 was no mold growth; Grade 1 was mold growth area <10%; Grade 2 and above were unqualified for anti-mildew performance. Negative ion release: Referring to industry standard JC / T 2110-2012 "Indoor Air Ion Concentration Test Method", the antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 and Comparative Examples 1-7 were respectively coated on the surface of a 50mm×50mm sterile glass plate. The dry film thickness was controlled at (60±5)μm. The plates were placed in a standard environment of (23±2)℃ and (50±5)% relative humidity for 7 days to obtain antibacterial coating samples. The antibacterial coating samples were used as test samples. The concentration of negative ions in the air was measured at a distance of 5cm from the coating surface using an air negative ion concentration tester. The unit was ions / cm³. Each group of samples was tested in parallel 3 times, and the average value was taken as the final negative ion release test result. The specific test results are shown in Table 1.

[0058] Table 1 Performance parameters of antibacterial and formaldehyde-removing high-performance negative ion coatings in Examples 1-3 and Comparative Examples 1-7 As shown in Table 1, the antibacterial and formaldehyde-removing high-performance negative ion coatings prepared in Examples 1-3 of this application exhibit excellent comprehensive performance. They possess strong adhesion, ensuring a firm bond between the coating and the substrate; they have a high formaldehyde removal rate, demonstrating outstanding purification capabilities; their antibacterial rates against Escherichia coli and Staphylococcus aureus both exceed 99%, achieving a strong antibacterial effect; their anti-mold performance reaches level 0, with no mold growth observed after 28 days of incubation; and their negative ion release reaches 3850-4020 ions / cm³. 3 It can release negative ions for a long time.

[0059] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. An antibacterial, aldehyde-removing, high performance anionic coating, characterized in that, By weight, it includes the following raw materials: 40-60 parts of water-based composite emulsion, 8-15 parts of modified negative ion powder, 3-8 parts of composite nano antibacterial and formaldehyde-removing agent, 10-20 parts of porous adsorption filler, 0.8-1.5 parts of dispersant, 0.3-0.8 parts of defoamer, 0.5-1.2 parts of film-forming aid, 0.2-0.5 parts of wetting agent, 0.2-0.5 parts of preservative and mildew inhibitor, 0.4-1.0 parts of thickener, and 15-25 parts of deionized water.

2. The antibacterial, aldehyde-removing, high performance anionic coating according to claim 1, characterized in that, The aqueous composite emulsion is composed of an acrylic emulsion, an aqueous styrene-butadiene emulsion, and a silicone-modified acrylic emulsion; wherein the amount of the aqueous styrene-butadiene emulsion added is 12-20% of the total mass of the acrylic emulsion and the silicone-modified acrylic emulsion, and the mass ratio of the acrylic emulsion to the silicone-modified acrylic emulsion is 4-7:1-3.

3. The antibacterial and aldehyde-removing high performance anion coating according to claim 1, characterized in that, The preparation method of the modified negative ion powder includes the following preparation steps: Step 1: Crush the tourmaline, sieve it, calcine it at high temperature, and then cool it naturally to obtain pretreated tourmaline powder. Step 2: Mix pretreated tourmaline powder with anhydrous ethanol and disperse at high speed to obtain a suspension; add coupling agent to the suspension, heat and stir at a constant temperature to obtain activated tourmaline suspension; add composite monomer and initiator to activated tourmaline suspension, heat and polymerize at a constant temperature under nitrogen protection, centrifuge, wash, vacuum dry, pulverize and sieve to obtain modified negative ion powder.

4. The antibacterial, aldehyde-removing, high performance anionic coating according to claim 3, characterized in that, The high-temperature calcination treatment in step 1 specifically involves heating to 550-650℃ at a heating rate of 5-8℃ / min and calcining at high temperature for 2-3 hours.

5. The antibacterial and aldehyde-removing high performance anion coating according to claim 3, characterized in that, In step 2, the mass ratio of activated tourmaline suspension, composite monomer and initiator is 80-100: 8-15: 0.3-0.

8.

6. The antibacterial, aldehyde-removing, high performance anionic coating according to claim 3, characterized in that, In step 2, the composite monomer is composed of dodecafluoroheptyl methacrylate and hexafluorobutyl acrylate in a mass ratio of 5-8:1-3.

7. The antibacterial, aldehyde-removing, high performance anion coating of claim 1, wherein, The composite nano antibacterial and formaldehyde-removing agent is composed of nano titanium dioxide, nano zinc oxide and sepiolite in a mass ratio of 3-5:2-4:1-2.

8. The antibacterial, aldehyde-removing, high performance anionic coating according to claim 1, characterized in that, The porous adsorption filler is one or more of zeolite powder, activated carbon powder, and attapulgite.

9. A process for the preparation of the antibacterial aldehyde-free high performance anionic coating as claimed in any one of claims 1 to 8, characterized in that, The preparation steps include the following: Add dispersant and wetting agent to deionized water, stir at low speed for 3-5 minutes, mix evenly, add porous adsorption filler and composite nano antibacterial and formaldehyde-removing agent, disperse at high speed for 15-20 minutes to obtain inorganic functional slurry; add water-based composite emulsion to deionized water, stir at low speed, add film-forming aid and anti-corrosion and anti-mildew agent in sequence during stirring, continue stirring to obtain coating base; add inorganic functional slurry to coating base, heat to 40-50℃, stir evenly at constant temperature, add modified negative ion powder, continue high-speed dispersion, mix evenly, reduce stirring speed, add defoamer, stir at low speed, add thickener, stir evenly, let stand to mature, to obtain antibacterial and formaldehyde-removing high-performance negative ion coating.