Composition and preparation method of a bulletproof and blast-resistant radar stealth coating
By preparing polyaspartic acid ester polyurea-based bulletproof and blast-resistant/radar stealth coatings, the problems of dispersibility and single function of existing coatings have been solved. This has achieved uniform dispersion of nano-level fillers and multi-band stealth effect, improving bulletproof and blast-resistant performance and environmental adaptability.
Patent Information
- Application Number
- CN202611210133.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing bulletproof and explosion-proof coatings suffer from problems such as difficulty in dispersing fillers, decreased flexibility due to increased hardness, poor bonding between inorganic fillers and polymer matrix, high cost, and limited functionality. Existing stealth coatings only work against one type of electromagnetic wave and have insufficient environmental tolerance.
Using polyaspartic acid ester polyurea as a binder, combined with carbon nanotubes and graphene oxide as modifying materials, and nickel-plated carbon fiber powder and active hollow ceramic microspheres as fillers, a bulletproof and blast-resistant/radar stealth coating is prepared through surface treatment and dispersant combination.
It achieves uniform dispersion of nano-level fillers, improves the bulletproof and explosion-proof performance of the coating and its broadband radar wave absorption capability, while maintaining good flexibility and mechanical strength. It also has green and environmentally friendly characteristics and is suitable for a variety of complex environments.
Smart Images

Figure CN123107513A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of special functional coatings technology, and in particular to the composition and preparation method of a bulletproof, explosion-proof, radar stealth coating. Background Technology
[0002] Explosion-proof, bulletproof, and stealth technologies are core research directions in the field of protection for modern military equipment and defense facilities. With the increasingly complex international security situation and the growing severity of threats such as explosive attacks and high-speed projectile strikes, higher and higher requirements are being placed on the comprehensive performance of protective materials.
[0003] Polyaspartic acid ester polyurea, as a novel aliphatic polyurea material, boasts advantages such as adjustable application time, short curing time, high strength, high solids content, low solvent content, and environmental friendliness, making it highly valuable in material protection and coating applications. Polyurea elastomers, due to their excellent shock absorption and protective properties, have been widely used in national defense and military projects, such as tank chassis, bulletproof helmets, and protective armor coatings. The ultra-tough protective coating products developed by the American company Line-X can withstand blasting when applied to walls; bullets will only leave dents without penetrating the surface, and the coating will prevent watermelons and eggs from breaking when dropped. Achieving this requires not only superior physical strength but also high tear resistance and abrasion resistance.
[0004] In the field of radar stealth, stealth coatings, as the most convenient, economical, and adaptable stealth technology, have been widely used in aerospace and military equipment. Carbon-based materials such as carbon nanotubes and graphene, due to their excellent electromagnetic loss capabilities, can effectively absorb electromagnetic waves and reduce radar reflection signals, making them ideal radar absorbing materials. However, existing stealth coatings often only work against one type of electromagnetic wave, while remaining unresponsive to other bands, indicating a significant limitation in single-band stealth coatings.
[0005] The main problems with existing bulletproof and explosion-proof coatings include: First, the filler dispersion is difficult. Most existing explosion-proof polyurea coatings use graphene oxide as a reinforcing material. Generally, graphene oxide is ultrasonically dispersed and then added to component A or component B. However, it is difficult to disperse graphene oxide into nanoscale fineness, which greatly reduces the explosion-proof effect of the coating. Some technologies also use aerogel as a filler, but it must be modified with organosilicon before being added to polyurea. Modified aerogel is difficult to disperse into nanoscale particles in polyurea, and there is currently no mature process.
[0006] Second, increasing the hard segment content leads to a decrease in flexibility. There are also methods to improve coating strength by increasing the hard segment content, but methods to increase the hard segment hardness through organic modification will result in excessively high material hardness, which will make the material lack flexibility at low temperatures and easily break.
[0007] Third, poor interfacial bonding between inorganic fillers and the polymer matrix. When strength is improved by adding inorganic fillers, if the fillers are not properly surface-treated, two fatal defects will be found under microscopic observation: first, uneven dispersion and agglomeration; second, poor bonding with the polymer, or even micro-separation. This leads to the separation of inorganic fillers from the polymer under high-speed impact, resulting in a rapid decrease in strength, and the fillers fail to enhance physical properties and tear resistance.
[0008] Fourth, existing enhancement methods are costly; while introducing graphene, carbon nanotubes, etc. into polyurea coatings can significantly enhance the tensile and impact resistance of the coating, these methods greatly increase the cost of the coating.
[0009] Fifth, the functions are limited; existing bulletproof and explosion-proof coatings usually do not have radar stealth capabilities, making it difficult to meet the needs of modern military equipment for multifunctional integrated protective materials.
[0010] The main problems with existing stealth coatings include: Existing stealth coatings often only work against one type of electromagnetic wave, remaining unresponsive to other bands. With the advent of advanced detection equipment, single-band stealth coatings have significant limitations, while multi-band electromagnetic wave stealth coatings with better compatibility have broad development prospects. Furthermore, existing radar-absorbing coatings lack environmental tolerance, making it difficult to meet the radar signature control requirements of targets in complex environments.
[0011] Current research status on the modification of polyaspartic acid ester polyurea coatings: Researchers have modified polyaspartic acid ester polyurea coating systems by synthesizing reactive adhesion-enhancing resins and high-solids, low-viscosity, high-strength and tough polyurethane curing agents. Other researchers have significantly improved the shielding performance and electrochemical stability of coatings by introducing nanomaterials such as graphene oxide and TiO2. However, when graphene oxide is combined with polyaspartic acid ester polyurea, the dispersibility of graphene oxide and its compatibility with the polymer matrix remain key bottlenecks restricting coating performance improvement. Regarding carbon nanotube reinforcement, existing technologies often involve directly adding carbon nanotubes modified with dispersants to polyurea coatings. However, carbon nanotubes have a large aspect ratio and high specific surface area, making them prone to aggregation and difficult to achieve uniform dispersion in the polymer matrix. Summary of the Invention
[0012] In view of the aforementioned existing problems, the present invention is proposed.
[0013] Therefore, the purpose of this invention is to provide a composition for a bulletproof, explosion-proof, and radar stealth coating. The purpose is to prepare a bulletproof, explosion-proof, and radar stealth coating by using polyaspartic acid ester polyurea as a binder, carbon nanotubes and graphene oxide as modifying materials, nickel-plated carbon fiber powder and active hollow ceramic microspheres as fillers, and in combination with various additives and curing agents.
[0014] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a composition of a bulletproof and blast-resistant radar stealth coating, wherein the coating is composed of component A and component B; Component A, by mass percentage, comprises the following components: 50-60% polyaspartic acid ester, 25-35% graphene oxide / polyaspartic acid ester dispersion, 5-10% carbon nanotubes, 3-5% nickel-plated carbon fiber powder, 1-3% carbon nanotube-specific dispersant, 0.2-0.5% defoamer, 0.3-0.5% leveling agent, and 1-3% dehydrating agent; Component B, by mass percentage, comprises the following components: 80-95% aspartic polyurea fluxless elastic curing agent, 0.2-0.5% dispersant, 5-10% active hollow ceramic microspheres, and 1-3% dehydrating agent.
[0015] In a preferred embodiment of the present invention, the aspartic polyurea solvent-free elastic curing agent is a prepolymer curing agent formed by polymerizing polyols and aliphatic isocyanates.
[0016] In a preferred embodiment of the present invention, the carbon nanotubes include single-walled carbon nanotubes and multi-walled carbon nanotubes.
[0017] In a preferred embodiment of the present invention, the carbon nanotube-specific dispersant is a copolymer dispersant containing pigment affinity groups.
[0018] In a preferred embodiment of the present invention, the defoamer is selected from one or more of BYK-141, BYK-A530, and BYK-058; the leveling agent is selected from one or more of BYK-306, BYK-333, and EFK-3600; and the dehydrating agent is molecular sieve 3A powder.
[0019] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing a bulletproof and blast-resistant radar stealth coating, comprising the following steps: Step 1: Preparation of graphene oxide / polyaspartic acid ester dispersion: (1) Graphene oxide surface coating treatment: 85 parts by weight of 95% ethanol were added to an ultrasonic disperser, 5 parts by weight of silane coupling agent were added under stirring, a trace amount of water was added, and the mixture was dispersed for 20 min. Then 10 parts by weight of graphene oxide powder were added, and the mixture was ultrasonically dispersed for 40 min. The mixture was then transferred to a reactor equipped with a reflux device at 80°C and stirred for 4 h. Finally, the mixture was vacuum dried at 80°C to obtain silane coupling agent coated graphene oxide powder. (2) Preparation of dispersion slurry: According to the mass fraction, take 28-32 parts of polyaspartic acid ester, 1.0 part of dispersant, 0.2 parts of defoamer, and 1.0-1.5 parts of silane coupling agent coated graphene oxide powder obtained in step (1). Add polyaspartic acid ester to a mixing tank, add dispersant, defoamer and silane coupling agent coated graphene oxide powder under stirring, stir evenly, disperse at high speed for 50-60 min, transfer to a basket mill for high-speed grinding for 2 h, and then ultrasonically disperse for 30 min until the particle size is 50 nm. Step 2: Preparation of Component A: (1) Pulping: Weigh out polyaspartic acid ester, carbon nanotube special dispersant, carbon nanotube and nickel-plated carbon fiber powder according to the composition of component A. Add polyaspartic acid ester to the dispersion tank, add carbon nanotube special dispersant under medium and low speed stirring and disperse evenly, then add carbon nanotube and nickel-plated carbon fiber powder, disperse at high speed for 30 min to obtain mixed slurry. (2) Grinding: The mixed slurry is ground twice with a grinding equipment until the fineness is less than 20 μm to obtain pigment slurry; (3) Paint mixing: Pour the pigment paste into the paint mixing tank, add the graphene oxide / polyaspartic acid ester dispersion paste, defoamer, leveling agent and dehydrating agent obtained in step one under medium and low speed stirring, stir for 30 minutes, filter and package to obtain component A; Step 3: Preparation of Component B: Weigh out the aspartic polyurea solvent-free elastic curing agent, dispersant, active hollow ceramic microspheres and dehydrating agent according to the composition of component B, and mix the components evenly to obtain component B.
[0020] Step 4: Paint preparation. Mix component A and component B evenly at a mass ratio of 100:100 to obtain the paint.
[0021] In a preferred embodiment of the present invention, the silane coupling agent in step one is KH-560.
[0022] In a preferred embodiment of the present invention, the dispersant in step one is BYK-163, and the defoamer is BYK-A530.
[0023] In a preferred embodiment of the present invention, the grinding equipment in step two is a three-roll mill or a conical mill.
[0024] As a preferred embodiment of the present invention, the coating is applied to military skin, military facilities, armor linings, composite armor, bulletproof shields, bulletproof helmets, explosion-proof containers, explosion-proof military facilities, buildings, bridges, tunnels, transportation facilities, railway facilities, highway facilities, or water conservancy engineering facilities.
[0025] Compared with the prior art, the present invention has at least the following beneficial effects: 1. This invention involves surface coating of graphene oxide with a silane coupling agent, followed by high-speed dispersion, ladle milling, and ultrasonic dispersion of the coated graphene oxide with polyaspartic acid ester resin under the action of a dispersant and defoamer, to prepare a graphene oxide / polyaspartic acid ester dispersion with a particle size of 50 nm. This method enables graphene oxide to be uniformly and stably dispersed in polyaspartic acid ester resin at a nanoscale fineness, overcoming the defect in existing technologies where graphene oxide is difficult to disperse to a nanoscale fineness. Simultaneously, carbon nanotubes are uniformly dispersed in the resin system by the special dispersant TNRDIS, and nickel-plated carbon fiber powder is easily wetted and uniformly dispersed by the resin after surface treatment. The synergistic effect of these three components enables the filler to achieve nanoscale uniform dispersion in the polymer matrix, with a tight bond to the polymer matrix and no micro-separation state, thus fully exerting its reinforcing effect under high-speed impact.
[0026] 2. This invention, through the rational combination of polyaspartic esters F420, F524, and F330, and the selection of aspartic polyurea flux-free elastic curing agent GB805B-100, enables the coating to maintain excellent mechanical strength while also possessing good flexibility. The product achieves an elongation at break of 300%, a tensile breaking strength of 45 MPa, a tear strength of 140 N / mm, a hardness (Shore A) of 88-90, and low-temperature bending performance ≤ -35℃. This overcomes the shortcomings of existing technologies that, by increasing the hard segment content, result in excessively high material hardness and brittleness at low temperatures.
[0027] 3. The coating of this invention has excellent impact resistance, with an impact resistance of up to 1.2 kg·m. Bulletproof tests show that when a 2.4 mm thick special steel plate is coated with an 8 mm thick bulletproof coating of this invention, under the conditions of a Type 79 submachine gun at a shooting distance of 100 m and 7.62 mm bullets, the bullets remain embedded in the coating without penetration or ricochet. The coating combines high strength and high elasticity, effectively absorbing and dissipating impact energy under high-speed impact, while simultaneously encasing shrapnel and fragments to prevent secondary injury.
[0028] 4. This invention achieves broadband radar wave absorption through a multi-scale, multi-component synergistic absorption system composed of carbon nanotubes, graphene oxide, nickel-plated carbon fibers, and activated ceramic hollow microspheres. The coating reflection loss is -5dB, the coating reflection dB is -22dB, the peak reflection loss in the 8-18GHz range reaches -30dB, and the broadband with reflection loss below -10dB reaches 5GHz. Carbon nanotubes, as one-dimensional nanomaterials, possess excellent dielectric loss performance; graphene oxide has a high specific surface area and good dielectric properties; the nickel film on the surface of the nickel-plated carbon fibers significantly improves the absorption performance; and the hollow spherical structure of the activated ceramic hollow microspheres facilitates multiple scattering and absorption of electromagnetic waves. The synergistic effect of these four components achieves broadband, high-efficiency radar wave absorption.
[0029] 5. The coating of this invention is a solvent-free system with a solid content of ≥99% and VOC emissions of only 40g / L, making it green and environmentally friendly. The coating exhibits 5000 hours of salt spray resistance without rust, blistering, or peeling; and 500 hours of acid, alkali, and salt resistance without rust, blistering, or peeling. Its water absorption rate is only 0.5%, and its abrasion resistance (750g / 750r) is only 0.5mg. Suitable for highly corrosive environments such as marine environments, this coating integrates multiple functions including bulletproofing, blast protection, radar stealth, heavy-duty corrosion protection, abrasion resistance, and weather resistance. It can be widely used in military skin, military facilities, armor linings, composite armor, bulletproof shields, bulletproof helmets, explosion-proof containers, explosion-proof military facilities, and in fields such as construction, bridges, tunnels, transportation, railways, highways, and water conservancy projects for shock and blast protection. Attached Figure Description
[0030] Figure 1 This is a schematic diagram of the steps in the preparation method of the bulletproof and blast-resistant radar stealth coating of the present invention. Detailed Implementation
[0031] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0032] This invention provides a bulletproof, blast-resistant, and radar-stealth coating, including its composition and preparation method. The coating consists of component A and component B, which are mixed at a mass ratio of 100:100 during application.
[0033] I. Raw Material Description All raw materials used in the specific embodiments of this invention can be purchased from the market, as detailed below: The polyaspartic acid ester is an aliphatic hindered amine polyurea resin. Two or more of F420 (OH content 6.13%), F524 (OH content 5.1%), F520, F330 (OH content 5.1%), and D2925 can be used in combination to achieve a balance between the activation period and drying time of the product, while also taking into account the balance between the hardness, strength and elasticity of the coating film.
[0034] The solvent-free elastic curing agent for aspartic polyurea is a prepolymer curing agent polymerized from polyols and aliphatic isocyanates. It can be selected from one or more of GB-105, GB805A, GB605A-100, and GB805B-100 for use in combination. Solvent-free coatings prepared by combining it with polyaspartic ester exhibit excellent tensile strength, elongation at break, and mechanical properties.
[0035] The graphene oxide is a derivative of graphene, which is a single or multilayer graphene oxide formed by the exfoliation of graphene oxide. It has a typical quasi-two-dimensional spatial structure, and its sheets contain a large number of oxygen-containing groups, which have high specific surface energy, good hydrophilicity and mechanical properties.
[0036] The carbon nanotubes are one-dimensional carbon nanomaterials, including single-walled carbon nanotubes and multi-walled carbon nanotubes. Carbon nanotubes possess excellent mechanical, optical, and electrical properties, exhibit structural stability, and have extremely high axial tensile strength.
[0037] The nickel-plated carbon fiber powder is obtained by surface treatment, grinding, screening and high-temperature drying of high-strength and high-modulus carbon fiber filaments into equal-length cylindrical particles. After chemical nickel plating, a continuous and bright metallic nickel film is formed on the surface of the carbon fiber.
[0038] The active hollow ceramic microspheres are surface-modified hollow ceramic microspheres, mainly composed of silicon dioxide and aluminum oxide, with a hollow spherical structure and a wall thickness of 8-10% of the diameter.
[0039] The carbon nanotube-specific dispersant is a copolymer containing pigment affinity groups, which can assist in the dispersion of carbon nanotubes in a liquid polyaspartic acid ester resin system.
[0040] The defoamer may be one or more of BYK-141, BYK-A530, and BYK-058; the leveling agent may be one or more of BYK-306, BYK-333, and EFK-3600; and the dehydrating agent is molecular sieve 3A powder.
[0041] II. General Preparation Method The method for preparing the bulletproof, blast-resistant, and radar-stealth coating of the present invention includes the following steps: Step 1: Preparation of graphene oxide / polyaspartic acid ester dispersion: (1) Graphene oxide surface coating treatment: 85 parts by weight of 95% ethanol were added to an ultrasonic disperser, 5 parts by weight of silane coupling agent KH-560 were added under stirring, a trace amount of water was added, and the mixture was dispersed for 20 min. Then 10 parts by weight of graphene oxide powder were added, and the mixture was ultrasonically dispersed for 40 min. The mixture was then transferred to a reactor equipped with a reflux device at 80℃ and stirred for 4 h. Finally, the mixture was vacuum dried at 80℃ to obtain silane coupling agent coated graphene oxide powder. (2) Preparation of dispersion slurry: According to the mass fraction, take 28-32 parts of polyaspartic acid ester, 1.0 parts of dispersant BYK-163, 0.2 parts of defoamer BYK-A530, and 1.0-1.5 parts of silane coupling agent coated graphene oxide powder obtained in step (1). Add polyaspartic acid ester to a mixing tank, add dispersant, defoamer and silane coupling agent coated graphene oxide powder under stirring, stir evenly, disperse at high speed for 50-60 min, transfer to a basket mill for high-speed grinding for 2 h, and then ultrasonically disperse for 30 min until the particle size is 50 nm.
[0042] Step 2: Preparation of Component A: (1) Pulping: Weigh out polyaspartic acid ester, carbon nanotube special dispersant, carbon nanotube and nickel-plated carbon fiber powder according to the composition of component A. Add polyaspartic acid ester to the dispersion tank, add carbon nanotube special dispersant under medium and low speed stirring and disperse evenly, then add carbon nanotube and nickel-plated carbon fiber powder, disperse at high speed for 30 min to obtain mixed slurry. (2) Grinding: The mixed slurry is ground twice by a three-roll mill or a conical mill until the fineness is less than 20 μm to obtain pigment slurry; (3) Paint mixing: Pour the pigment paste into the paint mixing tank, add the graphene oxide / polyaspartic acid ester dispersion paste, defoamer, leveling agent and dehydrating agent obtained in step one under medium and low speed stirring, stir for 30 minutes, filter and package to obtain component A.
[0043] Step 3: Preparation of Component B: Weigh out the aspartic polyurea solvent-free elastic curing agent, dispersant, active hollow ceramic microspheres and dehydrating agent according to the composition of component B, and mix the components evenly to obtain component B.
[0044] During application, component A and component B are mixed evenly at a mass ratio of 100:100 before coating, with a coating thickness of 8mm. Example Example 1
[0045] A bulletproof, blast-resistant, and radar-stealth coating, composed of component A and component B.
[0046] Composition of Component A (by mass percentage): 58% polyaspartic acid ester (F420, F524, and F330 mixed in a mass ratio of 50:20:10), 28% graphene oxide / polyaspartic acid ester dispersion, 7% carbon nanotubes (0.3 parts single-walled carbon nanotubes and 8 parts multi-walled carbon nanotubes), 5% nickel-plated carbon fiber powder, 1% carbon nanotube-specific dispersant, 0.2% defoamer BYK-530A, 0.3% leveling agent EFKA3600, and 1% dehydrating agent molecular sieve 3A powder.
[0047] Composition of Component B (by mass percentage): aspartic polyurea solvent-free elastic curing agent GB805B-100 92%, dispersant BYK-192 0.5%, active hollow ceramic microspheres 7%, and dehydrating agent molecular sieve 3A powder 1%.
[0048] The bulletproof, blast-resistant, and radar stealth coating of this embodiment was prepared according to the general preparation method described above. During application, component A and component B were mixed at a mass ratio of 100:100, and the coating thickness was 8 mm. Example 2
[0049] A bulletproof, blast-resistant, and radar-stealth coating, composed of component A and component B.
[0050] Composition of Component A (by mass percentage): 57% polyaspartic acid ester (F420, F524, and F330 mixed in a mass ratio of 50:20:10), 29% graphene oxide / polyaspartic acid ester dispersion, 8% carbon nanotubes (0.3 parts single-walled carbon nanotubes and 8 parts multi-walled carbon nanotubes), 4% nickel-plated carbon fiber powder, 1% carbon nanotube-specific dispersant, 0.3% defoamer BYK-530A, 0.3% leveling agent EFKA3600, and 1% dehydrating agent molecular sieve 3A powder.
[0051] Composition of Component B (by mass percentage): 90% aspartic polyurea solvent-free elastic curing agent GB805B-100, 0.5% dispersant BYK-192, 8% active hollow ceramic microspheres, and 1.5% dehydrating agent molecular sieve 3A powder.
[0052] The bulletproof, blast-resistant, and radar stealth coating of this embodiment was prepared using the same preparation method as in Example 1. During application, component A and component B were mixed at a mass ratio of 100:100, and the coating thickness was 8 mm. Example 3
[0053] A bulletproof, blast-resistant, and radar-stealth coating, composed of component A and component B.
[0054] Composition of Component A (by mass percentage): 59% polyaspartic acid ester (F420, F524, and F330 mixed in a mass ratio of 50:20:10), 30% graphene oxide / polyaspartic acid ester dispersion, 6% carbon nanotubes (0.3 parts single-walled carbon nanotubes and 8 parts multi-walled carbon nanotubes), 3% nickel-plated carbon fiber powder, 1% carbon nanotube-specific dispersant, 0.3% defoamer BYK-530A, 0.3% leveling agent EFKA3600, and 1% dehydrating agent molecular sieve 3A powder.
[0055] Composition of Component B (by mass percentage): aspartic polyurea solvent-free elastic curing agent GB805B-100 91%, dispersant BYK-192 0.5%, active hollow ceramic microspheres 7%, dehydrating agent molecular sieve 3A powder 1.5%.
[0056] The bulletproof, blast-resistant, and radar stealth coating of this embodiment was prepared using the same preparation method as in Example 1. During application, component A and component B were mixed at a mass ratio of 100:100, and the coating thickness was 8 mm. Example 4
[0057] A bulletproof, blast-resistant, and radar-stealth coating, composed of component A and component B.
[0058] Composition of Component A (by mass percentage): 55% polyaspartic acid ester (F420, F524, and F330 mixed in a mass ratio of 50:20:10), 32% graphene oxide / polyaspartic acid ester dispersion, 5% carbon nanotubes (0.3 parts single-walled carbon nanotubes and 8 parts multi-walled carbon nanotubes), 5% nickel-plated carbon fiber powder, 1% carbon nanotube-specific dispersant, 0.2% defoamer BYK-530A, 0.3% leveling agent EFKA3600, and 1% dehydrating agent molecular sieve 3A powder.
[0059] Composition of Component B (by mass percentage): aspartic polyurea solvent-free elastic curing agent GB805B-100 91%, dispersant BYK-192 0.5%, active hollow ceramic microspheres 7%, dehydrating agent molecular sieve 3A powder 1.5%.
[0060] The bulletproof, blast-resistant, and radar stealth coating of this embodiment was prepared using the same preparation method as in Example 1. During application, component A and component B were mixed at a mass ratio of 100:100, and the coating thickness was 8 mm.
[0061] IV. Performance Testing and Comparison The coatings obtained in Examples 1-4 above were subjected to performance tests. Test conditions: Component A and Component B were mixed at a mass ratio of 100:100 and then applied. The coating thickness was 8 mm. After curing under standard conditions for 7 days, various performance tests were conducted. The results of each performance test are shown in the table below:
[0062]
[0063] Bulletproof performance test: Using a 2.4mm thick special steel plate as a base, each plate was coated with an 8mm thick bulletproof coating as described in Examples 1-4 of this invention. Tests were conducted using a Type 79 submachine gun at a firing distance of 100m and with 7.62mm ammunition. The results are as follows: Example 1: The bullet was embedded in the coating, did not penetrate, and did not ricochet; Example 2: The bullet was embedded in the coating, did not penetrate, and did not ricochet; Example 3: The bullet was embedded in the coating, did not penetrate, and did not ricochet; Example 4: The bullet was embedded in the coating, did not penetrate, and did not ricochet.
[0064] All embodiments can achieve effective bulletproof protection, with Embodiment 1 showing the best overall bulletproof effect.
[0065] The performance test results above show that the formulation and preparation method given in Example 1 of this invention are the optimal implementation method, achieving the best performance in terms of mechanical properties (tensile breaking strength 45MPa, tear strength 140N / mm, elongation at break 300%), low-temperature bending properties (≤-35℃), radar stealth performance (peak reflection loss -30dB, bandwidth below -10dB 5GHz), and ballistic protection. Although Examples 2-4 are also within the scope of protection of the claims of this invention and all meet the basic performance requirements of ballistic and blast protection / radar stealth, Example 1 has the best overall performance.
[0066] Performance comparison analysis: (I) Analysis of the impact of differences in formulation composition on performance The main differences between the formulations of Example 1 and Examples 2-4 are as follows: Example 1 uses a compounding ratio of F420:F524:F330 = 50:20:10, with F420 (OH content 6.13%) as the main resin accounting for 50%, and F524 and F330 (both with OH content 5.1%) accounting for 30% together. This compounding ratio results in moderate reactivity and reasonable crosslinking density of the resin system, achieving an optimal balance between hardness and elasticity in the coating film. Therefore, the elongation at break (300%), tensile strength at break (45MPa), and low-temperature bending properties (≤-35℃) are all optimal.
[0067] In Example 2, the proportion of F420 was increased to 58%, while F524 and F330 together accounted for 30%. The increased proportion of F420 led to a higher crosslinking density in the resin system and improved the coating hardness (Shore A 85-87), but reduced flexibility and elongation at break to 280%. In Example 3, F420 accounted for 55 parts, F524 for 20 parts, and F330 for 10 parts. Meanwhile, the proportion of nickel-plated carbon fiber powder was increased to 5 parts. The increased proportion of reinforcing filler maintained the tensile strength at 43 MPa, but slightly reduced the elongation at break. In Example 4, the proportions of F524 and F330 were adjusted (52 parts F420, 15 parts F524, and 15 parts F330). The increased proportion of F330 improved the system's flexibility, but the relatively lower proportion of F420 reduced the crosslinking density, resulting in relatively lower overall mechanical properties (tensile strength at break of 40 MPa and elongation at break of 260%).
[0068] In Example 1, the total addition amount of carbon nanotubes was 8.3% (0.3 parts single-walled + 8 parts multi-walled) and nickel-plated carbon fiber powder was 3.5%. This ratio achieved the optimal synergistic effect in the multi-scale reinforcement system, resulting in the best radar stealth performance (peak reflection loss of -30dB, bandwidth below -10dB of 5GHz) among all examples. Variations in the ratio of carbon nanotubes and carbon fiber powder in Examples 2-4 led to differences in the synergistic absorption effect of the absorbing agent.
[0069] (ii) Overall advantages of the preferred embodiment In summary, the formulation of Example 1 exhibits the best performance across all the aforementioned performance indicators for the following reasons: The optimal resin blending ratio is F420:F524:F330 = 50:20:10, which achieves the best balance between crosslinking density and flexibility of the polyaspartic ester resin system, ensuring both high coating strength (45MPa) and excellent elasticity (300% elongation) and low-temperature performance (≤-35℃). The synergistic effect of multi-scale reinforcing fillers is optimal: single-walled carbon nanotubes (0.3 parts), multi-walled carbon nanotubes (8 parts), and nickel-plated carbon fiber powder (3.5 parts) form a three-dimensional reinforcing network of "point-line-surface" at the micro-nano scale. Combined with nanoscale dispersed graphene oxide (1.7 parts), the mechanical strength and wave absorption performance of the coating are optimized. The proportions of each additive are reasonable: the synergistic effect of dispersant TNRDIS (3.3 parts) and BYK-163 (1 part) ensures the nanoscale dispersion of carbon nanotubes and graphene oxide in the resin, and the reasonable combination of defoamer, leveling agent, defoamer and dehydrating agent ensures the density and surface quality of the coating.
[0070] Therefore, Example 1 is the best embodiment of the present invention.
[0071] V. Application Areas The bulletproof and blast-proof radar stealth coating prepared by this invention can be widely used in military skin, military facilities, armor linings, composite armor, bulletproof shields, bulletproof helmets, explosion-proof containers, explosion-proof military facilities, as well as in the fields of construction, bridges, tunnels, transportation, railways, highways, and water conservancy projects for shockproof and blast-proof protection. It can also be used in fields such as heavy-duty anti-corrosion, thermal insulation, UV resistance, wear resistance, waterproofing and seepage prevention, and antistatic properties with high conductivity requirements on metal surfaces.
[0072] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. The composition of a bulletproof, blast-resistant, radar-stealth coating, characterized in that, The coating is composed of component A and component B; Component A, by mass percentage, comprises the following components: 50-60% polyaspartic acid ester, 25-35% graphene oxide / polyaspartic acid ester dispersion, 5-10% carbon nanotubes, 3-5% nickel-plated carbon fiber powder, 1-3% carbon nanotube-specific dispersant, 0.2-0.5% defoamer, 0.3-0.5% leveling agent, and 1-3% dehydrating agent; Component B, by mass percentage, comprises the following components: 80-95% aspartic polyurea fluxless elastic curing agent, 0.2-0.5% dispersant, 5-10% active hollow ceramic microspheres, and 1-3% dehydrating agent.
2. The composition of the bulletproof and blast-resistant radar stealth coating according to claim 1, characterized in that: The aspartic polyurea solvent-free elastic curing agent is a prepolymer curing agent formed by the polymerization of polyol and aliphatic isocyanate.
3. The composition of the bulletproof and blast-resistant radar stealth coating according to claim 1, characterized in that: The carbon nanotubes include single-walled carbon nanotubes and multi-walled carbon nanotubes.
4. The composition of the bulletproof and blast-resistant radar stealth coating according to claim 1, characterized in that: The carbon nanotube-specific dispersant is a copolymer dispersant containing pigment affinity groups.
5. The composition of the bulletproof and blast-resistant radar stealth coating according to claim 1, characterized in that: The defoamer is selected from one or more of BYK-141, BYK-A530, and BYK-058; the leveling agent is selected from one or more of BYK-306, BYK-333, and EFK-3600; and the dehydrating agent is molecular sieve 3A powder.
6. A method for preparing a bulletproof and blast-resistant radar stealth coating as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Preparation of graphene oxide / polyaspartic acid ester dispersion: S1.1 Graphene oxide surface coating treatment: 85 parts by weight of 95% ethanol were added to an ultrasonic disperser, 5 parts by weight of silane coupling agent were added under stirring, a trace amount of water was added, and the mixture was dispersed for 20 min. Then 10 parts by weight of graphene oxide powder were added, and the mixture was ultrasonically dispersed for 40 min. The mixture was then transferred to a reactor equipped with a reflux device at 80℃ and stirred for 4 h. Finally, the mixture was vacuum dried at 80℃ to obtain silane coupling agent coated graphene oxide powder. S1.2 Preparation of dispersion slurry: According to the mass fraction, take 28-32 parts of polyaspartic acid ester, 1.0 part of dispersant, 0.2 parts of defoamer, and 1.0-1.5 parts of silane coupling agent coated graphene oxide powder obtained in step (1). Add polyaspartic acid ester to a mixing tank, add dispersant, defoamer and silane coupling agent coated graphene oxide powder under stirring, stir evenly, disperse at high speed for 50-60 min, transfer to a basket mill for high-speed grinding for 2 h, and then ultrasonically disperse for 30 min until the particle size is 50 nm. S2. Preparation of component A: S2.1 Pulping: Weigh out polyaspartic acid ester, carbon nanotube special dispersant, carbon nanotubes and nickel-plated carbon fiber powder according to the composition of component A. Add polyaspartic acid ester to the dispersion tank, add carbon nanotube special dispersant under medium and low speed stirring and disperse evenly, then add carbon nanotubes and nickel-plated carbon fiber powder, disperse at high speed for 30 minutes to obtain mixed slurry. S2.2 Grinding: The mixed slurry is ground twice with a grinding device until the fineness is less than 20μm to obtain pigment slurry; S2.3 Paint Mixing: Pour the pigment paste into a paint mixing tank, add the graphene oxide / polyaspartic acid ester dispersion paste obtained in step one, defoamer, leveling agent and dehydrating agent under medium-low speed stirring, stir for 30 minutes, filter and package to obtain component A; S3. Preparation of component B: S3.1 Weigh out the aspartic polyurea solvent-free elastic curing agent, dispersant, active hollow ceramic microspheres and dehydrating agent according to the composition of component B, and stir and mix the components evenly to obtain component B. S4. For paint preparation, mix component A and component B evenly at a mass ratio of 100:100 to obtain the paint.
7. The method for preparing the bulletproof and blast-resistant radar stealth coating according to claim 6, characterized in that: The silane coupling agent used in step S1 is KH-560.
8. The method for preparing the bulletproof and blast-resistant radar stealth coating according to claim 7, characterized in that: The dispersant in step S1 is BYK-163, and the defoamer is BYK-A530.
9. The method for preparing the bulletproof and blast-resistant radar stealth coating according to claim 8, characterized in that: The grinding equipment mentioned in step S2 is a three-roll mill or a conical mill.
10. The application of the bulletproof and blast-resistant radar stealth coating according to any one of claims 1-5, or the bulletproof and blast-resistant radar stealth coating prepared by the preparation method according to any one of claims 6-9, in the preparation of bulletproof and blast-resistant radar stealth coatings, characterized in that, The coating is applied to military skin, military facilities, armor linings, composite armor, bulletproof shields, bulletproof helmets, explosion-proof containers, explosion-proof military facilities, buildings, bridges, tunnels, transportation facilities, railway facilities, highway facilities, or water conservancy projects.