A robust superhydrophobic conductive coating, its preparation method and application
By driving free radical chain transformation with GHz femtosecond laser pulse sequences to generate intermetallic compounds, the problems of insufficient chemical modification and mechanical stability in the preparation of superhydrophobic surfaces are solved, and the efficient preparation of superhydrophobic conductive coatings is realized.
Patent Information
- Application Number
- CN202611224299.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the preparation methods for superhydrophobic surfaces require subsequent low surface energy chemical modification, the mechanical stability of the micro-nano structures is insufficient, and the preparation process is complex, making it difficult to achieve large-area rapid preparation.
By using a GHz femtosecond laser pulse sequence to drive free radical chain transformation, intermetallic compounds are generated in an organic-inorganic composite coating, achieving one-step synergistic regulation of surface chemical composition and microstructure, and forming a robust superhydrophobic conductive coating.
It achieves superhydrophobic properties without subsequent chemical modification, and the coating has excellent mechanical durability and conductivity. It is suitable for a variety of substrate materials and is suitable for large-area rapid preparation.
Smart Images

Figure CN123107538A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to ultrafast laser processing and functional surface preparation technology, specifically to a one-step method for constructing superhydrophobic surfaces without post-processing by using ultrafast femtosecond laser pulse sequences to drive the temporal accumulation of free radicals in an organic-inorganic composite coating system, in-situ reducing metal oxides and generating intermetallic compound reinforcing phases. Background Technology
[0002] Superhydrophobic surfaces have broad application prospects in self-cleaning, anti-icing and de-icing, corrosion prevention, oil-water separation, and drag reduction. Two key elements for achieving superhydrophobic properties are: constructing a rough structure at the micro-nano scale and endowing the surface with a low surface energy chemical composition. Currently, the main methods for preparing superhydrophobic surfaces include sol-gel methods, chemical vapor deposition, template methods, spraying methods, and electrospinning methods. While these methods can achieve superhydrophobic functionality to a certain extent, they generally suffer from the following technical bottlenecks: First, subsequent low-surface-energy chemical modification is required. Most methods, after constructing micro / nano rough structures, require chemical modification with low-surface-energy reagents such as fluorinated silanes or long-chain fatty acids to reduce the surface energy. This not only increases the number of process steps and costs but also introduces organic solvent pollution. The low-surface-energy modified layer is prone to wear or photodegradation during use, leading to a gradual loss of hydrophobic function.
[0003] Second, the mechanical stability of micro / nano structures is insufficient. The micro / nano rough structures (especially nanoscale protrusions) upon which superhydrophobic surfaces rely are highly susceptible to fracture or wear under friction, impact, or shear. Once the structure is damaged, the Cassie-Baxter gas-liquid interface state transforms into the Wenzel wetting state, and the superhydrophobic properties are lost. How to improve the mechanical stability of the structure while maintaining micro / nano roughness has long been a core challenge in this field.
[0004] Third, the preparation process is complex and inefficient. Most methods involve multiple steps (such as template preparation, casting, demolding, and surface finishing), making it difficult to achieve rapid preparation of large areas. Furthermore, the process parameters require strict control, which is not conducive to industrialization.
[0005] Pulsed laser processing offers advantages such as non-contact operation, high precision, and strong controllability, making it an effective means of constructing surface micro- and nano-structures. Femtosecond lasers, with their ultrashort pulse duration and ultra-high peak power, can achieve non-thermal material removal through mechanisms such as multiphoton absorption and avalanche ionization, resulting in a minimal heat-affected zone and widespread application in precision micro- and nano-fabrication. However, traditional femtosecond laser processing technology still suffers from the following inherent limitations: First, the pulse repetition frequency of traditional femtosecond laser systems is typically on the order of kHz (1-1000 kHz), corresponding to pulse intervals on the order of milliseconds to microseconds. After a single laser pulse, electronic excitation, free radical generation, and transient thermal effects in the material relax or quench within a nanosecond to microsecond timescale. Because the pulse interval is much larger than the characteristic relaxation time of active species (on the order of nanoseconds), the active groups generated by the preceding pulse are completely dissipated before the arrival of subsequent pulses, and effective temporal coupling cannot be established between adjacent pulses. The entire processing exhibits a series of isolated non-equilibrium excitation events.
[0006] Secondly, in the aforementioned isolated pulse mode, femtosecond lasers can only achieve ablation or modification of the material surface morphology (such as forming periodic stripes, micropore arrays, nanoparticle deposition, etc.), but it is difficult to continuously control the intrinsic chemical composition of the material across pulses. If it is necessary to endow the surface with low surface energy properties or other chemical functions, it is still necessary to rely on subsequent chemical modification steps (such as fluorosilane immersion, plasma treatment, chemical vapor deposition, etc.), which does not fundamentally solve the problem of process complexity.
[0007] Third, due to the lack of continuous accumulation of active species and temporal coupling of reaction pathways, traditional femtosecond laser processing is unable to establish a stable chemical kinetic evolution process within the action region, and cannot achieve the active design of a complete chemical transformation pathway from initial reactants to target products.
[0008] Therefore, it is urgent to develop a new mechanism that can overcome the bottleneck of the mismatch between pulse interval and active species lifetime, and extend the processing capability of femtosecond lasers from single morphology construction to the synergistic regulation of morphology and chemical composition, so as to realize the true one-step superhydrophobic surface preparation.
[0009] GHz femtosecond laser pulse trains represent a significant advancement in ultrafast laser technology in recent years. Unlike traditional single-pulse modes with repetition frequencies of kHz, GHz pulse train modes tightly arrange a series of subpulses within a pulse train envelope at nanosecond intervals, with subpulse intervals ranging from hundreds of picoseconds to a few nanoseconds. This unique temporal structure offers a way to overcome the aforementioned bottleneck of "pulse interval-active species lifetime mismatch": the nanosecond-level subpulse intervals fall precisely within the relaxation time window of reactive intermediates such as free radicals, allowing the reactive species generated by preceding subpulses to be effectively "reused" by subsequent subpulses before they are completely dissipated, thus achieving continuous accumulation of reactive species across pulses. Summary of the Invention
[0010] The purpose of this invention is to provide a method and product for preparing superhydrophobic coatings based on free radical chain conversion driven by GHz femtosecond laser pulse sequences, in order to solve the technical bottleneck in the prior art where femtosecond laser processing relies on subsequent chemical modification and cannot achieve synergistic control of surface chemical composition and microstructure.
[0011] The core principle of this invention lies in utilizing the unique physical characteristic of GHz femtosecond laser pulse sequences—that the nanosecond-level sub-pulse intervals and free radical relaxation times are on the same timescale—to transform the isolated pulse excitation events in traditional femtosecond laser processing into a time-coupled free radical chain reaction triggering process. After the free radicals driven by the pulse sequence continuously accumulate and cross a critical threshold, a self-accelerating positive feedback process is triggered, driving the in-situ reduction of CuFe2O4 within the coating to generate metallic iron. This iron combines with silicon atoms released from the broken silicon-oxygen framework to form a FeSi intermetallic compound reinforcing phase. Simultaneously, the silicon-oxygen segments undergo re-oxidation and disordered condensation to transform into amorphous SiO2, which, together with the original crystalline SiO2 nanoparticles in the coating, constructs a micro / nano composite rough structure on the surface, achieving one-step synergistic control of surface chemical composition and microstructure.
[0012] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a robust superhydrophobic conductive coating includes the following steps: (1) Graphene, copper ferrite and silica nanoparticles are mixed and sheared and stirred (200-2000 rpm, 5-20 minutes) to obtain composite powder; the composite powder is then mixed with methylphenyl silicone resin and sheared and stirred (200-2000 rpm, 10-30 minutes) to obtain composite slurry; the obtained slurry is vacuum degassed at room temperature for 15-60 minutes to remove bubbles and is ready for use.
[0013] (2) The composite slurry is coated onto the substrate surface to form a pre-coating layer; (3) The pre-coated surface is scanned using a GHz femtosecond laser pulse sequence to obtain a conductive coating with superhydrophobic properties in situ.
[0014] In this process, the nanosecond-level sub-pulse intervals of the GHz femtosecond laser pulse sequence are on the same timescale as the radical relaxation time. This allows the active radicals induced by the preceding pulses to be effectively reused by subsequent pulses before they are completely dissipated. This enables the continuous accumulation of radicals across pulses within the local micro-region of the coating, triggering a chain reaction and simultaneously achieving the following in-situ physicochemical transformations: selective breaking of C-Si bonds in methylphenyl silicone resin, releasing methyl and phenyl radicals; simultaneously, the silicon-oxygen framework is exposed and undergoes structural rearrangement, followed by re-oxidation and disordered aggregation to form amorphous SiO2 microspheres, which, together with the original SiO2 nanoparticles in the coating, construct a surface micro / nano rough structure; the accumulated radicals act as strong electron donors, releasing Fe³⁺ from CuFe₂O₄. + In situ, the iron is reduced to metallic state and combines with silicon atoms released by the breakage of C-Si bonds to form an in situ FeSi intermetallic compound reinforcing phase, which significantly improves the mechanical robustness of the coating; graphene is exposed during laser irradiation and forms a continuous conductive network, giving the coating conductivity. The above process can be completed in one step after laser scanning, without any subsequent heat treatment or chemical surface modification. The coating surface immediately acquires multifunctional properties that combine superhydrophobicity, conductivity and mechanical robustness.
[0015] The preparation process flow chart is shown below. Figure 1 .
[0016] Preferably, the composite slurry contains 0.05 to 0.1 parts graphene, 10 to 20 parts copper ferrite, 10 to 20 parts quartz powder, and 7 to 8 parts methylphenyl silicone resin by weight.
[0017] The methylphenyl silicone resin, as a free radical precursor, contains Si-C6H5 and Si-CH3 bonds in its molecular structure. Under laser pulse irradiation, the C-Si bonds can undergo selective cleavage, releasing methyl free radicals to trigger and maintain subsequent chain reactions. The high reactivity of methyl free radicals is beneficial for driving subsequent reduction reactions.
[0018] The copper ferrite (CuFe2O4) has the following multiple functions: (1) As a highly efficient photothermal conversion material. CuFe2O4 has a spinel-type crystal structure with a narrow band gap (approximately 1.4-1.9 eV), which can effectively absorb photon energy in the ultraviolet to near-infrared bands and efficiently convert light energy into heat energy through non-radiative relaxation. This photothermal effect can help increase the local temperature and reduce the activation energy threshold for C-Si bond breaking during laser processing.
[0019] (2) As an iron source supplier. The Fe³⁺ in CuFe₂O₄ + Ions can be reduced to metallic iron (Fe) after accumulating to a certain concentration of free radicals.0 This provides an iron source for the subsequent in-situ formation of FeSi intermetallic compounds. Simultaneously, Cu²⁺ in CuFe₂O₄... + It can also be reduced simultaneously, and the generated Cu+ can serve as an additional catalytic active site.
[0020] (3) The synergistic light absorption effect of CuFe2O4 and graphene enables the composite coating to have efficient photon capture capability over a wide wavelength range, ensuring that the selective breaking of C-Si bonds in silicone resin can be driven at a low average laser power (0.6-16 W), reducing the requirements for laser power and improving processing efficiency and controllability.
[0021] The graphene has the following multiple functions: (1) Highly efficient light absorber. Graphene has a broad-spectrum absorption characteristic in the ultraviolet to infrared band. When combined with CuFe2O4, it can further enhance the absorption efficiency of the coating to incident laser energy and reduce the laser power threshold required to trigger C-Si bond breaking.
[0022] (2) Radical Stabilization Carrier. The sp² conjugated carbon network of graphene can adsorb radical species and stabilize phenyl radicals through π-π interactions, prolonging their effective survival time and facilitating the cross-pulse accumulation of radicals within the sub-pulse interval.
[0023] (3) Constructing a continuous conductive network inside the coating gives the coating conductive function, which can provide a basis for subsequent applications (such as electrothermal de-icing).
[0024] The silica nanoparticles (SiO2) serve as a structural reinforcing phase, and their function is as follows: (1) It is uniformly dispersed in the coating matrix before laser processing to serve as a rigid skeleton to improve the initial mechanical properties of the coating.
[0025] (2) During laser processing, the silanol groups (Si-OH) on its surface can undergo a condensation reaction with the active siloxane segments generated by the breakage of the siloxane skeleton, promoting the formation of the amorphous SiO2 network.
[0026] (3) Nanoparticles themselves, as components of micro-nano rough structures, increase the micro-roughness of the surface.
[0027] Preferably, the coating method in step (2) is any one of the following: blade coating, spin coating, spray coating, or dip coating, and the wet film thickness is controlled between 100-500 μm. The coating is allowed to cure naturally at room temperature for 1-24 hours, or cured by heating at 40-80 ℃ for 0.5-4 hours, so that the silicone resin is fully cross-linked to form an MGCS composite coating with good adhesion.
[0028] Preferably, the substrate includes, but is not limited to, glass, metal (aluminum, copper, stainless steel), ceramic, polymer (polyimide, polycarbonate, polymethyl methacrylate), composite material, etc.
[0029] Preferably, in step (3), the laser beam controls the scanning path through a galvanometer system or a displacement platform, and performs cross-scanning or line-by-line scanning on the selected area under ambient atmosphere (air). The key laser parameters are set as follows: center wavelength 1030 nm (or 515 nm or 343 nm), pulse width 300 fs to 10 ps, pulse repetition frequency 200 kHz (or 100 kHz to 1 MHz), GHz sub-pulse interval 0.92 ns, number of sub-pulses in a single pulse train 200-1500, average power 0.6-16 W, focused spot diameter 30-100 μm, scanning speed 50-500 mm / s, and scanning line spacing 0.05-0.2 mm.
[0030] After laser processing, no heat treatment (such as annealing) or chemical surface modification (such as fluorosilane immersion) is required. The coating surface immediately acquires stable superhydrophobic properties in situ, with a water contact angle of up to 161±0.7° and a sliding angle of 2±0.4°.
[0031] The present invention also provides a robust superhydrophobic conductive coating prepared by the above method, which has a static water contact angle of 158°~161°, a roll-off angle of 2°~8°, and a surface resistivity of 400~1000Ω; after applying a 100g load and rubbing it on 100-grit sandpaper for 20 cycles, its static water contact angle decreases by less than 11°.
[0032] Finally, the present invention also provides the application of the aforementioned robust superhydrophobic conductive coating in anti-icing, de-icing, and surface protection.
[0033] Compared with the prior art, the present invention has the following beneficial effects: One-step in-situ construction with simple process: The composite coating is directly scanned and processed using a GHz femtosecond laser pulse sequence. No subsequent heat treatment or chemical surface modification is required to obtain superhydrophobic properties in situ, which greatly simplifies the preparation process.
[0034] Excellent performance: The resulting coating has a water contact angle as high as 161±0.7° and a sliding angle as low as 2±0.4°, exhibiting excellent superhydrophobicity and self-cleaning properties; at the same time, graphene constructs a continuous conductive network inside the coating, giving the coating good conductivity, which can be applied to scenarios such as electrothermal de-icing.
[0035] Rugged and durable: Using silicone resin as the matrix, and inducing complex physicochemical reactions inside through laser processing, the coating structure is reconstructed and strengthened at the microscale, forming a robust micro-nano composite structure, which significantly improves the mechanical durability of the coating.
[0036] Synergistic effect of multifunctional materials: Through a carefully designed material system (graphene, copper ferrite and silicon dioxide nanoparticles), the synergistic effect of multiple functions such as photothermal conversion (copper ferrite), free radical stabilization carrier (graphene), and structural enhancement (SiO2) is achieved, which lowers the threshold of laser processing and improves processing efficiency.
[0037] Environmentally friendly and widely applicable: The preparation process requires no fluorinated chemicals or organic solvents, making it environmentally friendly. The coating method is flexible and suitable for various substrate materials such as glass, metal, ceramics, and polymers, facilitating large-scale application. Attached Figure Description
[0038] Figure 1 This is a flowchart illustrating the preparation process of the present invention and a schematic diagram illustrating the coating performance.
[0039] Figure 2 SEM images of the coating surfaces prepared for Example 1(a) and Comparative Example 3(b).
[0040] Figure 3 The image shows a comparison of the FTIR spectra of the coating in Example 1 (processed with different laser sub-pulse numbers).
[0041] Figure 4 The XRD pattern of the coating in Example 1 shows the diffraction peaks of FeSi and Cu4O3.
[0042] Figure 5 The image shows a comparison of the Raman spectra of the coating in Example 1 (processed with different laser sub-pulse numbers).
[0043] Figure 6 This is a schematic diagram of the surface water contact angle and roll-off angle test of the coating in Example 1.
[0044] Figure 7 This is a schematic diagram of the abrasion resistance test (sandpaper friction test) results of the coating in Example 1. Detailed Implementation
[0045] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments, but this does not limit the present invention in any way. Any modifications or improvements made based on the teachings of the present invention shall fall within the protection scope of the present invention.
[0046] The processes, conditions, reagents, and experimental methods used in implementing this invention, except as specifically mentioned below, are all common knowledge and general knowledge in the field, and this invention does not have any particular limitations. Experimental methods in the embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the manufacturer.
[0047] Unless otherwise stated, all technical terms and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. However, in the event of any conflict, the specification containing the definitions shall prevail.
[0048] Example 1 Raw material preparation: Weigh 0.1g graphene nanosheets, 1.0g copper ferrite nanoparticles, 1.0g quartz powder with a particle size of 20μm, and 8.0g methylphenyl silicone resin. Mix the above materials evenly at 200 rpm for 20 minutes, and then degas under vacuum for 20 minutes to obtain a uniform black slurry.
[0049] Pre-coating preparation: The glass substrate (30 mm × 30 mm × 1 mm) was ultrasonically cleaned with anhydrous ethanol and dried. The above slurry was uniformly sprayed onto the surface of the glass substrate using a blade coating method, and pre-cured in air for 1 hour to form a pre-coating with a thickness of approximately 200 μm.
[0050] Laser processing: A GHz femtosecond laser processing system (center wavelength 1030 nm, repetition rate 100 kHz) was used. The average laser power was set to 3 W, the scanning speed to 50 mm / s, the scan line spacing to 100 μm, and the spot diameter to approximately 50 μm. A full-coverage scan was performed on the pre-coated surface. Slight white smoke was observed during the processing.
[0051] Post-treatment: Gently blow the surface with compressed air to remove any loose particles that may be attached.
[0052] Characterization and Testing: To systematically evaluate the morphology, chemical structure, phase composition, and overall properties of the coating, the following characterization and testing methods were employed: Morphology analysis: The microstructure of the coating surface was observed using scanning electron microscopy (SEM).
[0053] Chemical structure analysis: Fourier transform infrared spectroscopy (FTIR) was used to analyze the changes in chemical bonds before and after laser treatment of the coating.
[0054] Phase analysis: X-ray diffraction (XRD) was used to determine the crystalline phase composition of the coating.
[0055] Graphene state analysis: Micro-confocal Raman spectroscopy was used to analyze the exposure and defect state of graphene.
[0056] Wetting performance test: Static water contact angle and roll-off angle were measured using a contact angle measuring instrument.
[0057] Conductivity test: The sheet resistance of the coating surface was measured using a four-probe resistance tester.
[0058] Mechanical robustness test: The abrasion resistance of the coating is evaluated using a sandpaper friction test.
[0059] The test results are as follows: Morphology (SEM): such as Figure 2 As shown in Figure a, the coating surface is covered with a large number of irregular SiO2 microspheres with a particle size between 0.5 and 5 μm. They are stacked and adhered to each other, forming a multi-scale rough structure.
[0060] Chemical composition (FTIR): such as Figure 3 As shown, the number of methyl groups on the coating surface gradually decreases with the increase of the number of laser sub-pulses.
[0061] Phase analysis (XRD): such as Figure 4 As shown, a distinct FeSi crystal diffraction peak appeared at 2θ≈45°, confirming the in-situ formation of the FeSi reinforcing phase.
[0062] Raman spectroscopy: such as Figure 5 As shown, with the increase of the number of sub-pulses, the crystalline silicon dioxide on the coating surface becomes amorphous silicon dioxide, and the strength gradually increases.
[0063] Hydrophobicity test: such as Figure 6 As shown, the static contact angle of deionized water on the coating surface was measured to be 161° and the roll-off angle was 2°, which shows excellent superhydrophobic and low adhesion properties.
[0064] Conductivity test: The sheet resistance of the coating surface was measured to be approximately 400Ω using a four-probe resistor, indicating good conductivity.
[0065] Robustness test: Abrasion resistance: such as Figure 7 As shown, the coated sample (contact angle side down) was placed on 100-grit sandpaper, a 100 g weight was applied, and the sample was pulled horizontally by 10 cm as one cycle. The test showed that after 20 cycles, the contact angle of the coating remained above 150°, and there was no obvious damage to the surface, demonstrating excellent wear resistance.
[0066] Example 2 The difference between this embodiment and Example 1 is that the raw material ratio is adjusted: graphene 0.05 g, copper ferrite 0.5 g, quartz powder 2.0 g, and methylphenyl silicone resin 7.0 g. The laser parameters are adjusted to: average power 16 W, scanning speed 500 mm / s, and scanning line spacing 100 μm.
[0067] The resulting coating exhibits slightly smaller SiO2 microspheres with a relatively sparse distribution. The water contact angle is 158°, and the roll-off angle is 8°. The surface sheet resistance is approximately 1.0 kΩ. After 22 cycles of abrasion resistance testing, the contact angle decreased to 152°. This example demonstrates that the hydrophobicity, conductivity, and abrasion resistance of the coating can be controlled within a certain range by adjusting the composition and laser parameters.
[0068] Example 3 The difference between this embodiment and Embodiment 1 is that the substrate is replaced with a fiber-reinforced epoxy resin composite material. Before applying the slurry, the surface of the composite material is subjected to plasma treatment to improve wettability.
[0069] A robust superhydrophobic and conductive coating was successfully prepared on the surface of the composite material after laser treatment. The water contact angle was 160° and the roll-off angle was 2°. The coating bonded well to the polymer substrate and maintained its superhydrophobicity after 20 sandpaper abrasion cycles. This demonstrates that the method of this invention is applicable to other material substrates.
[0070] Comparative Example 1 (without quartz powder) The difference between this comparative example and Example 1 is that no quartz powder is added, and the raw materials are only graphene, copper ferrite and methylphenyl silicone resin.
[0071] After laser treatment, the coating surface exhibits a porous, carbonized appearance and a certain degree of roughness, with a water contact angle reaching 159° (see...). Figure 6 It exhibits superhydrophobicity. However, the coating peels off in large quantities when the surface is gently wiped with a cotton swab. Raman spectroscopy still shows strong broad peaks of amorphous carbon (see...). Figure 5 This comparison demonstrates that quartz powder is crucial for the formation of robust SiO2 microsphere structures, and without it, a durable coating cannot be obtained.
[0072] Comparative Example 2 (Copper Ferrate-Free) The difference between this comparative example and Example 1 is that copper ferrite is not added, while the other conditions are the same as in Example 1.
[0073] After laser treatment, SiO2 microspheres form on the coating surface, exhibiting superhydrophobicity (contact angle 157°). However, XRD analysis did not detect the FeSi phase. Abrasion resistance testing showed that after only 5 cycles of friction, the coating contact angle dropped significantly to below 145°, and the surface showed severe wear. This comparison demonstrates the crucial role of in-situ generated FeSi in enhancing the mechanical robustness of the coating.
[0074] Comparative Example 3 The difference from Example 1 is that the laser is replaced with a conventional single-pulse femtosecond laser with the same average power and the same repetition frequency for scanning processing, while the other conditions are the same as in Example 1.
[0075] The surface is ablated or forms laser-induced periodic stripes, but it is difficult to form a uniform and robust SiO2 microsphere structure; FeSi phase formation is minimal; the coating is loose and easily peels off, such as... Figure 2 As shown in b.
[0076] This demonstrates that the unique “heat-relaxation” cycle of the GHz pulse train mode is crucial for achieving mild and controllable melting (quartz powder spheroidization) and promoting solid-state diffusion reactions (FeSi generation), and is a necessary condition for initiating the desired in-situ chemical reactions.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a robust superhydrophobic conductive coating, characterized in that, Includes the following steps: (1) Graphene, copper ferrite and silica nanoparticles are mixed and stirred once to obtain a composite powder; then the composite powder is mixed with methylphenyl silicone resin and stirred twice to obtain a composite slurry; (2) The composite slurry is coated onto the substrate surface and cured to form a pre-coating layer; (3) The pre-coated surface is scanned using a GHz femtosecond laser pulse sequence to obtain a conductive coating with superhydrophobic properties in situ; In this context, the nanosecond-level sub-pulse interval of the GHz femtosecond laser pulse sequence is on the same time scale as the free radical relaxation time.
2. The preparation method according to claim 1, characterized in that, The composite slurry comprises, by weight: 0.05 to 0.1 parts graphene, 10 to 20 parts copper ferrite, 10 to 20 parts quartz powder, and 7 to 8 parts methylphenyl silicone resin.
3. The preparation method according to claim 1, characterized in that, In step (1), the first stirring speed is 200-2000 rpm and the time is 5-20 minutes; the second stirring speed is 200-2000 rpm and the time is 10-30 minutes.
4. The preparation method according to claim 1, characterized in that, In step (1), the composite slurry is degassed at room temperature for 15-60 minutes before coating.
5. The preparation method according to claim 1, characterized in that, In step (2), the coating method is any one of the following: scraping, spin coating, spraying or dipping; the thickness of the wet film after coating is 100-500 μm; the curing is natural curing at room temperature for 1-24 hours, or heating and curing at 40-80 ℃ for 0.5-4 hours.
6. The preparation method according to claim 1, characterized in that, In step (3), the parameters of the GHz femtosecond laser pulse sequence are as follows: center wavelength is 1030 nm, 515 nm or 343 nm, pulse width is 300 fs to 10 ps, pulse repetition frequency is 100 kHz to 1 MHz, GHz sub-pulse interval is 0.92 ns, number of sub-pulses in a single pulse train is 200-1500, average power is 0.6-16 W, focused spot diameter is 30-100 μm, scanning speed is 50-500 mm / s, and scanning line spacing is 0.05-0.2 mm.
7. The preparation method according to claim 1, characterized in that, In step (3), the laser scanning process is performed in an ambient atmosphere, and the scanning method is cross scanning or line-by-line scanning.
8. The preparation method according to claim 1, characterized in that, The substrate is a metal, glass, ceramic, or polymer composite material.
9. A robust superhydrophobic conductive coating prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The coating has a water contact angle of 158°~161° and a roll-off angle of 2°~8°.
10. The application of the robust superhydrophobic conductive coating of claim 9 in anti-icing, de-icing, and surface protection.