A wear-resistant coating material for vehicle anti-slip stickers and its preparation method

By designing a two-component system and refining the preparation process, the problems of insufficient wear resistance, stain resistance and flexibility of traditional automotive anti-slip coatings have been solved, achieving strong adhesion and performance stability between the coating and the substrate, making it suitable for large-scale industrial production.

CN123107540APending Publication Date: 2026-11-17QINGDAO VICTORY TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611562259.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional automotive anti-slip coatings are inadequate in terms of wear resistance, stain resistance, and flexibility. Furthermore, nanofillers are prone to agglomeration, leading to unstable performance and difficulty in meeting the quality consistency requirements of large-scale industrial production.

Method used

A two-component system design is adopted, using organosilicon polymers as the matrix, compounding fluorine-containing functional monomers and surface-modified inorganic nanofillers, and combining them with a dedicated catalytic system. Through refined preparation process control, the raw material pretreatment, feeding dispersion and coating curing are optimized to construct a coating network with excellent comprehensive performance.

Benefits of technology

The coating has strong adhesion to the substrate and has excellent wear resistance, scratch resistance, stain resistance and flexibility. It is compatible with various automotive anti-slip sticker substrates, extends service life, reduces production costs and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107540A_ABST
    Figure CN123107540A_ABST
Patent Text Reader

Abstract

This invention discloses a wear-resistant coating material for automotive anti-slip stickers and its preparation method, relating to the technical field of automotive interior materials and functional coating materials. The material comprises: component A and component B in a weight ratio of 10:1 to 15:1, wherein: component A contains the following raw materials in parts by weight: 50-65 parts of alkoxysilane-terminated polysiloxane; 20-30 parts of perfluoropolyether-based epoxysilane; 3-5 parts of γ-glycidyl etheroxypropyltrimethoxysilane; 0.1-0.5 parts of trifluoromethanesulfonic acid metal salt catalyst; and 5-8 parts of nano-silicon carbide; component B contains the following raw materials in parts by weight: 2-4 parts of aminopropyltriethoxysilane; 1-2 parts of polyethyleneimine; and 2-4 parts of nano-boron nitride. This invention designs and constructs a high-quality coating through a two-component system, a compounded metal salt catalyst, and the introduction of modified nanofillers, enhancing adhesion to the automotive anti-slip sticker substrate and adapting to complex working conditions; and through refined process control, it solves industry problems, eliminates the need for high temperature and high pressure, achieves high production efficiency, and reduces costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive interior materials and functional coating materials, specifically to a wear-resistant coating material for the surface of an anti-slip sticker and its preparation method. Background Technology

[0002] As an indispensable functional accessory in automotive interiors, car anti-slip stickers are mainly used to secure various items placed inside the vehicle, preventing them from sliding or tipping over due to bumps, acceleration, or braking during driving, thus ensuring driving safety and the integrity of items inside the car. With the rapid development of the automotive industry and the continuous improvement of consumers' requirements for the quality of automotive interiors, the performance requirements of car anti-slip stickers are no longer limited to basic anti-slip functions. The durability, stain resistance, and ease of cleaning of their surfaces have gradually become core standards for measuring product quality. As the surface protective layer of car anti-slip stickers, the coating directly determines the overall performance of the product. Therefore, the research and development of high-performance coating materials has always been a key research direction in the field of automotive interior accessories. Currently, the industry mostly uses silicone materials as the base for anti-slip sticker coatings, relying on their good flexibility, adhesion, and weather resistance to meet basic usage requirements. However, a single silicone system has significant shortcomings in wear resistance and stain resistance. How to achieve synergistic improvement of multiple performances through material system optimization and process improvement has become a technical problem that the industry urgently needs to solve.

[0003] Traditional car anti-slip stickers often use a single-component silicone system for their surface coating. The cross-linking reaction process is difficult to control precisely, resulting in an uneven cross-linking structure within the coating after curing and low overall mechanical strength. During long-term use, the coating surface is constantly subjected to friction, scratches, and pressure from objects, easily leading to wear, scratches, and even peeling. This causes the basic anti-slip function of the sticker to rapidly diminish, significantly shortening the product's lifespan. Some technologies attempt to improve the coating's stain resistance by introducing fluorine-containing components, but these often employ simple physical blending methods. The compatibility between the fluorine-containing components and the silicone matrix is ​​poor, leading to… The coating is prone to phase separation, and the migration of fluorine-containing components to the coating surface is irregular, resulting in unstable oil and stain resistance. In addition, the addition of nano-reinforcing fillers in traditional processes is relatively crude, and the filler particles are prone to agglomeration. This not only fails to effectively enhance and toughen the coating but also increases its brittleness, causing it to crack when subjected to external impact. Furthermore, traditional preparation processes have relatively lax control over the production environment, raw material pretreatment, and feeding process, resulting in large performance fluctuations between different batches of coating materials, making it difficult to meet the quality consistency requirements of large-scale industrial production. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a wear-resistant coating material for automotive anti-slip stickers and its preparation method. It employs a two-component system design, using an organosilicon polymer as the matrix, compounded with fluorinated functional monomers and surface-modified inorganic nanofillers, and combined with a dedicated catalytic system to construct a coating network with excellent comprehensive performance. This invention, through refined process control throughout the entire preparation process, optimizes key steps such as raw material pretreatment, feeding and dispersion, grinding and filtration, and coating and curing, solving the problems of easy agglomeration of nanofillers, uneven coating cross-linking, and large batch-to-batch performance fluctuations in traditional technologies. The resulting coating has strong adhesion to the substrate and possesses excellent wear resistance, scratch resistance, stain resistance, and flexibility, making it suitable for various automotive anti-slip sticker substrates. The production process is simple and environmentally friendly, enabling large-scale production and effectively improving the service life and quality of automotive anti-slip stickers.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: In one aspect, a wear-resistant coating material for the surface of an automotive anti-slip sticker is composed of component A and component B in a weight ratio of 10:1 to 15:1, wherein: Component A contains the following raw materials in parts by weight: Alkoxysilane-terminated polysiloxane: 50-65 parts; Perfluoropolyether-based epoxysilane: 20-30 parts; γ-glycidyl etheroxypropyltrimethoxysilane: 3-5 parts; Trifluoromethanesulfonic acid metal salt catalyst: 0.1-0.5 parts; Nano silicon carbide: 5-8 parts; Component B contains the following raw materials in parts by weight: aminopropyltriethoxysilane: 2-4 parts; Polyethyleneimine: 1-2 parts; Nano boron nitride: 2-4 parts.

[0006] Furthermore, the alkoxysilane-terminated polysiloxane is α,ω-ethoxy / methoxy dual-terminated polydimethylsiloxane, with a molar ratio of ethoxy to methoxy of 1:0.8-1.2, a number-average molecular weight of 18,000-25,000, a total alkoxy content of 2.8-3.2 wt%, a rotational viscosity of 2500-3500 mPa·s at 25°C, and a volatile content of ≤0.5% after 2 hours at 105°C.

[0007] Furthermore, the chemical structural formula of the perfluoropolyether-based epoxysilane is: CF3O-(CF2CF2O). m -(CF2O) n-CF2-CH2-O-CH2-CH(O)CH2-O-CH2-CH2-CH2-Si(OCH3)3, where m=8-12, n=2-4, number average molecular weight is 1300-1700, epoxy value is 0.32-0.38mmol / g, fluorine content is 55-60wt%, and viscosity at 25℃ is 700-900mPa·s.

[0008] Furthermore, the trifluoromethanesulfonic acid metal salt catalyst is a compound composed of scandium trifluoromethanesulfonic acid and lanthanum trifluoromethanesulfonic acid in a mass ratio of 1.5-2.5:1, with a moisture content of ≤0.1% and a total metal ion content of ≥98.5%.

[0009] Furthermore, the nano-silicon carbide is cubic β-silicon carbide with a primary particle size of 25-35 nm, a secondary agglomerate particle size ≤150 nm, and a specific surface area of ​​70-90 m². 2 / g, the surface is modified with γ-aminopropyltriethoxysilane, the amount of modifier being 1.5-2.5% of the mass of nano-silicon carbide; the nano-boron nitride is plate-shaped hexagonal boron nitride with a plate diameter of 60-80nm, a thickness of 4-8nm, a plate diameter to thickness ratio of 12-18:1, and a specific surface area of ​​30-40m². 2 / g, the surface is modified with dopamine hydrochloride, and the amount of modifier is 1.2-1.8% of the mass of nano boron nitride.

[0010] On the other hand, a method for preparing a wear-resistant coating material for the surface of a vehicle anti-slip sticker includes the following specific steps: Preparation of component A: Add alkoxysilane-terminated polysiloxane, perfluoropolyether-based epoxysilane, and γ-glycidyl etheroxypropyltrimethoxysilane to a reactor and stir at 300-500 rpm for 10-15 minutes; add trifluoromethanesulfonic acid metal salt catalyst and stir at 250-300 rpm for 5-10 minutes; add nano-silicon carbide and disperse at 600-800 rpm for 15-20 minutes; grind the material to a fineness ≤20μm, filter through a 200-mesh filter, and package. Preparation of component B: Add aminopropyltriethoxysilane and polyethyleneimine to a reaction vessel and stir at 200-300 rpm for 5-8 minutes; add nano boron nitride and disperse at 400-500 rpm for 10 minutes; filter through a 200-mesh filter and package. Coating and curing: Mix component A and component B evenly at the weight ratio of 10-15:1 as described in claim 1, and apply the mixture to the surface of the vehicle anti-slip sticker substrate, controlling the wet film thickness to be 40-60 μm; place the coated substrate in an environment with a relative humidity of 50-80% and a temperature of 20-35℃ for 20-40 minutes.

[0011] Furthermore, in the preparation of component A, the inner wall of the reactor is polished to a roughness Ra≤0.8μm before feeding, and the air is replaced with dry nitrogen; the material temperature is kept ≤25℃ when adding the catalyst; nano silicon carbide is added in batches and the material temperature is controlled ≤38℃; the roller surface temperature is controlled ≤35℃ during grinding; and nitrogen protection is provided during filling.

[0012] Furthermore, the grinding in the preparation of component A is carried out using a three-roll mill with a roller speed ratio of 1:3:9, and the grinding is carried out to a fineness of ≤20μm; the mixing in the coating and curing process is controlled by a metering pump with an accuracy of ±0.5%, the static mixer is 20-40cm long and contains 12-20 spiral blades, and the mixed material is transported through an insulated pipeline at 23±2℃.

[0013] Furthermore, in the preparation of component B, the inner wall of the reactor is polished and the air is replaced with dry nitrogen before feeding; after adding aminopropyltriethoxysilane and polyethyleneimine, the material temperature is controlled to be ≤28℃; when adding nano boron nitride, it is added in batches and the material temperature is controlled to be ≤32℃; nitrogen protection is provided during filling.

[0014] Furthermore, during the coating and curing process, the substrate surface is wiped with anhydrous ethanol and purged with dry compressed air before coating; components A and B are mixed using a static mixer, and the usable period of the mixed material is 10-15 minutes; the wet film thickness is controlled at 40-60 μm, the curing environment is 25±2℃, relative humidity is 65±5%, air flow rate is 0.3-0.5 m / s, and the curing time is 20-40 minutes.

[0015] Compared with existing technologies, the wear-resistant coating material and its preparation method for the vehicle anti-slip sticker have the following advantages: I. This invention utilizes a two-component system design, combining the synergistic effect of an organosilicon matrix and fluorinated functional monomers to construct a coating network structure with both low surface energy and high crosslinking density. A composite metal salt catalytic system is employed to regulate the rate and process of the crosslinking reaction, avoiding increased coating brittleness due to excessive local crosslinking, while ensuring the uniformity and stability of the curing process. Surface-modified inorganic nanofillers are introduced, and through specific dispersion and grinding processes, the nanoparticles are uniformly distributed within the organic matrix, effectively filling micro-defects within the coating, enhancing its mechanical strength and scratch resistance. A strong chemical bond is formed between the coating and the automotive anti-slip sticker substrate, significantly enhancing interfacial adhesion and preventing problems such as coating peeling and flaking during long-term use. Simultaneously, the coating possesses excellent oil and stain resistance, adapting to the complex operating conditions in the automotive environment and extending the overall service life of the automotive anti-slip sticker.

[0016] II. This invention employs refined process control, standardizing the entire process from raw material pretreatment and reaction environment regulation to coating and curing. This ensures the consistency and stability of coating material performance across batches. By using stepwise feeding and gradient dispersion processes, it solves the industry problem of easy agglomeration of nanofillers, fully leveraging the reinforcing and toughening effects of nanomaterials. Through strict control of the environmental conditions during the reaction and curing processes, it optimizes the crosslinking structure and surface morphology of the coating, enabling the coating to maintain excellent wear resistance while also possessing good flexibility and impact resistance. The preparation process does not require high temperature and high pressure conditions, has low energy consumption, and is easy to operate. The coating methods are flexible and diverse, adaptable to different types of automotive anti-slip sticker substrates, and have high production efficiency, making it suitable for large-scale industrial production. This effectively reduces the manufacturing cost and subsequent maintenance cost of automotive anti-slip stickers.

[0017] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.

[0019] Figure 1 A schematic diagram of the process flow for preparing the wear-resistant coating material for the surface of vehicle anti-slip stickers; Figure 2 A schematic diagram showing the composition and preparation process of component A in the wear-resistant coating material of vehicle anti-slip stickers; Figure 3 A schematic diagram showing the composition and preparation process of component B in the wear-resistant coating material of vehicle anti-slip stickers; Figure 4 A schematic diagram of the overall preparation, coating, and curing process of the wear-resistant coating for vehicle anti-slip stickers. Detailed Implementation

[0020] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.

[0021] Example 1: The preparation steps for the wear-resistant coating material on the surface of car anti-slip stickers are as follows: Figure 1 As shown.

[0022] Preparation of component A: First, the inner wall of the reactor is finely polished to meet production standards. Then, dry nitrogen is continuously introduced into the reactor to completely replace the air inside. According to the formula, 55 parts of alkoxysilane-terminated polysiloxane, 25 parts of perfluoropolyether-based epoxysilane, and 4 parts of γ-glycidyl etheroxypropyltrimethoxysilane are added to the reactor. The stirring device is started, and the stirring speed is set to 400 rpm for 12 minutes to ensure the three raw materials are fully mixed and form a homogeneous liquid system. Then, 0.3 parts of trifluoromethanesulfonic acid metal salt catalyst are slowly added to the homogeneous mixture. Throughout the feeding process, the material temperature is continuously controlled to not exceed 25 degrees Celsius. The stirring speed is adjusted to 280 rpm for 8 minutes to ensure the catalyst is uniformly dispersed in the material system without local aggregation. Seven parts of nano-silicon carbide were slowly added to the material system in three portions, with a three-minute interval between each addition. The material temperature was controlled to not exceed 38 degrees Celsius throughout the process. After each addition, the stirring speed was increased to 700 rpm, and high-speed dispersion was performed for 18 minutes to ensure the nano-silicon carbide was fully dispersed in the system without agglomeration or sedimentation. The dispersed material was then fed into a three-roll mill with a roller speed ratio of 1:3:9. The roller surface temperature was strictly controlled to not exceed 35 degrees Celsius. The material was repeatedly ground until the fineness reached ≤20μm. After grinding, the material was pressure filtered using a 200-mesh filter to thoroughly remove large particles and undispersed agglomerates. After filtration, the material was filled and sealed under nitrogen protection to obtain stable and qualified component A. Figure 2 As shown.

[0023] Preparation of component B: After polishing the inner wall of the reactor, the air inside was completely replaced with dry nitrogen to eliminate the influence of air on the raw materials. According to the formula, 3 parts aminopropyltriethoxysilane and 1.5 parts polyethyleneimine were added to the reactor. The stirring device was started, and the stirring speed was set to 250 rpm for 6 minutes to fully integrate the two raw materials and form a homogeneous system. During stirring, the material temperature was continuously controlled to not exceed 28 degrees Celsius. 3 parts nano-boron nitride were slowly added to the material system in two portions, with a 2-minute interval between each addition. The material temperature was controlled to not exceed 32 degrees Celsius throughout the process. After the addition was completed, the stirring speed was adjusted to 450 rpm, and dispersion was continued for 10 minutes to ensure that the nano-boron nitride was uniformly dispersed in the system without agglomeration. After dispersion, the material was precisely filtered using a 200-mesh filter to remove impurities and agglomerated particles. After filtration, the material was filled and sealed under nitrogen protection to obtain stable and qualified component B. Figure 3 As shown.

[0024] Coating and curing: First, repeatedly wipe the surface of the automotive anti-slip sticker substrate with anhydrous ethanol to thoroughly remove oil, dust, and other impurities. Then, continuously blow dry compressed air onto the substrate surface to ensure it is clean, dry, and free of residue. Precisely mix the prepared components A and B at a weight ratio of 12:1, using a metering pump to control the feeding ratio. The mixture is thoroughly homogenized using a static mixer, and then stably transported through an insulated pipeline. The homogenized material is then evenly coated onto the pre-treated substrate surface, with the wet film thickness precisely controlled to 50 micrometers using coating equipment. The coated substrate is then placed stably in a constant temperature and humidity environment (25°C, 65% relative humidity, 0.4 m / s airflow) for 30 minutes to allow the coating to fully undergo a cross-linking reaction and completely cure. Figure 4 As shown.

[0025] Example 2: Characterization of raw materials and physical and chemical properties of wear-resistant coating on the surface of vehicle anti-slip stickers.

[0026] Characterization of the physicochemical properties of core raw materials: Comprehensive testing was conducted on alkoxysilane-terminated polysiloxane using specialized testing equipment. The raw material was α,ω-ethoxymethoxy double-terminated polydimethylsiloxane, with an ethoxy to methoxy molar ratio of 1:1, a number-average molecular weight of 22,000, a total alkoxy content of 3.0%, a rotational viscosity of 3000 mPa·s at 25°C, and a volatile matter content of 0.4% after baking at 105°C for 2 hours. Chemical titration and particle size analysis were used to test perfluoropolyether-based epoxysilane. This raw material had a number-average molecular weight of 1500, an epoxy value of 0.35 mmol / g, a fluorine content of 57%, and a viscosity of 800 mPa·s at 25°C. Moisture and elemental analysis were used to test the trifluoromethanesulfonic acid metal salt catalyst. This catalyst was a mixture of scandium trifluoromethanesulfonate and lanthanum trifluoromethanesulfonate in a 2:1 mass ratio, with a moisture content of 0.1% and a total metal ion content of 98.5%. Electron microscopy and specific surface area analysis were used to analyze nano-silicon carbide. The raw material was cubic β-silicon carbide with a primary particle size of 30 nm, a secondary agglomerated particle size of 150 nm, and a specific surface area of ​​80 m² / g. The surface of the raw material was modified with γ-aminopropyltriethoxysilane at a dosage of 2% of the nano-silicon carbide mass. Electron microscopy and specific surface area analysis were also used to analyze nano-boron nitride. The raw material was plate-like hexagonal boron nitride with a plate diameter of 70 nm and a thickness of 6 nm, a plate diameter to thickness ratio of 15:1, and a specific surface area of ​​35 m² / g. The surface of the raw material was modified with dopamine hydrochloride at a dosage of 1.5% of the nano-boron nitride mass.

[0027] Characterization of the basic physical and chemical properties of the coating: The cured coating was visually inspected using a combination of visual inspection and microscopic observation equipment. The coating surface was smooth and even, free of bubbles, pinholes, particle agglomerations, and drip marks, with a uniform overall color. The curing state was tested using a touch test; after complete curing, the surface was not sticky, and the film was continuous, intact, and without breaks or missing corners. The coating thickness was measured at multiple points using a coating thickness gauge; the dry film thickness was consistently maintained at 30 micrometers, with minimal deviation in thickness uniformity across multiple points. The hydrophobicity of the coating surface was tested using a contact angle meter; the water droplet contact angle on the coating surface was consistently above 110 degrees, indicating stable and good hydrophobic and antifouling properties, effectively resisting the adhesion of external stains.

[0028] Example 3: Optimization test of process parameters for preparing wear-resistant coating on the surface of vehicle anti-slip stickers.

[0029] With the raw material ratio kept constant, key process parameters such as stirring speed, dispersion time, and curing temperature were gradually adjusted. Multiple parallel experiments were conducted to compare the material dispersion state, coating curing time, and film quality under different parameters, ultimately identifying the optimal combination of process parameters. During the experiments, the order of raw material addition, feeding method, and environmental cleanliness were kept completely consistent; only the process parameters to be optimized were changed. Each experiment was repeated three times, and the average value was used as the test result.

[0030] Table 1. Comparison of test results for optimization of preparation process parameters:

[0031] Test Result Analysis: Under the process parameter combination of Group 2, the material dispersion state is optimal, with no stratification, agglomeration, or sedimentation within the system. The uniformity of raw material mixing is the highest, and the coating can be completely cured within 30 minutes. The film surface is smooth and free of any defects, resulting in the best overall performance. Group 1 has a lower base stirring speed and catalyst stirring speed, leading to insufficient raw material mixing, a shorter dispersion time resulting in uneven nanoparticle dispersion, and a lower curing temperature, which slows down the coating crosslinking reaction rate and extends the curing time to 40 minutes. Group 3 has an excessively high stirring speed, which easily introduces air bubbles into the system, affecting the material dispersion stability. The higher curing temperature accelerates the film formation rate on the coating surface, leading to insufficient internal crosslinking and increased film brittleness. Considering all test data, the parameter combination of a base stirring speed of 400 rpm, a catalyst stirring speed of 280 rpm, a dispersion time of 18 minutes, and a curing temperature of 25 degrees Celsius ensures thorough mixing and dispersion of the raw materials, achieving the best balance between coating curing rate and film quality.

[0032] Example 4: Abrasion resistance test of the abrasion-resistant coating on the surface of vehicle anti-slip stickers.

[0033] A professional abrasion testing machine was used to test the abrasion resistance of the fully cured coating. Standard steel wool was used as the friction medium, and a constant pressure of 500 grams was applied to the friction area. The reciprocating friction frequency of the testing machine was set to 60 times per minute, and the coating was subjected to 5000, 10000, and 15000 reciprocating friction tests. The ambient temperature and humidity were kept constant during the test. After each set of friction tests, the integrity, weight loss rate, and hydrophobicity retention rate of the coating were accurately measured, and the changes in the surface condition of the coating were recorded to compare the differences in abrasion resistance of the coating under different numbers of friction cycles.

[0034] Table 2 Comparison of wear resistance test results:

[0035] Test Result Analysis: With the gradual increase in the number of friction cycles, the coating integrity and hydrophobicity retention rate showed a steady downward trend, while the weight loss rate showed a slow upward trend. The changes in all performance indicators were relatively small, demonstrating the coating's excellent wear resistance stability. After 5000 friction cycles, the coating surface showed no obvious damage, with coating integrity remaining at 98% and hydrophobicity retention rate reaching 97%, essentially maintaining its initial performance. After 10000 friction cycles, the coating surface showed only very slight fine scratches, with no peeling, flaking, or exposed substrate, and a weight loss rate of only 0.3%, still exhibiting excellent protective and usability performance. After 15000 friction cycles, the coating surface showed only a few shallow scratches, with no large-area wear, and the integrity remained at 90%, with a hydrophobicity retention rate of 92%, still providing good protection. The test data fully demonstrates that the coating has excellent wear resistance and can meet the wear resistance requirements of long-term, high-frequency use of automotive anti-slip stickers.

[0036] Example 5: Test on the weather resistance and environmental adaptability of the wear-resistant coating on the surface of vehicle anti-slip stickers.

[0037] The coated and cured automotive anti-slip sticker samples underwent three weather resistance tests: high and low temperature cycling, high humidity environment, and ultraviolet aging. During the tests, all test conditions were strictly controlled. After the tests, the appearance and performance retention of the coating were examined to evaluate its adaptability to the complex automotive environment. The high and low temperature cycling test was conducted at 60 degrees Celsius and -20 degrees Celsius for 50 cycles; the high humidity environment test was conducted at 90% humidity and 25 degrees Celsius for 120 hours; and the ultraviolet aging test was conducted at an ultraviolet wavelength of 365 nanometers for 200 hours.

[0038] Table 3. Comparison of weather resistance test results:

[0039] Test Result Analysis: After completing the three weathering tests, the coating showed no defects such as cracking, blistering, peeling, dampness, whitening, mildew, yellowing, chalking, or embrittlement. Its appearance remained intact and smooth, and its performance retention rate remained above 96%, demonstrating extremely strong environmental adaptability. In the high and low temperature cycling test, the coating withstood 50 cycles of extreme temperature alternation, maintaining a tight bond with the substrate without peeling or separation, achieving a performance retention rate of 98%. In the high humidity environment test, the coating showed no moisture absorption, expansion, or structural damage under prolonged high humidity and sealed conditions, exhibiting stable surface hydrophobic properties, with a performance retention rate of 97%. In the ultraviolet aging test, the coating showed no aging or degradation after prolonged ultraviolet irradiation, with no significant attenuation in abrasion resistance and adhesion, achieving a performance retention rate of 96%. This coating maintains stable physical and chemical properties in complex automotive environments such as high and low temperatures, high humidity, and ultraviolet irradiation, demonstrating outstanding weather resistance and environmental adaptability.

[0040] Example 6: Test on the adhesion and mechanical compatibility of the wear-resistant coating on the surface of vehicle anti-slip stickers.

[0041] The fully cured coating was subjected to a cross-cut adhesion test, a flexural strength test, and a peel strength test in sequence to comprehensively test the coating's adhesion to the substrate, flexural resistance, and tensile strength, verifying the coating's mechanical adaptability in daily automotive use. The cross-cut adhesion test involved cutting 100 1mm squares into the coating surface; the flexural strength test involved 1000 180-degree bends; and the peel strength test involved peeling at a speed of 50 mm / min at 180 degrees. Each test was repeated three times, and the average value was taken.

[0042] Table 4. Comparison of adhesion and mechanical properties test results:

[0043] Test Result Analysis: In the cross-cut adhesion test, none of the 100 squares on the coating surface peeled off, showed any lifting or curling, achieving the highest standard of Grade 0. This demonstrates a very strong bond between the coating and the substrate, exhibiting excellent adhesion. In the bending resistance test, after 1000 180-degree bends, the coating showed no cracks, peeling, or curling at the bends, maintaining its overall structural integrity and demonstrating good flexible mechanical adaptability, suitable for flexible bending applications of anti-slip stickers. In the peel strength test, the peel strength between the coating and the substrate reached 12 N / cm. During the test, there was no overall peeling of the coating, only a very small amount of minor damage at the edges, indicating a strong and stable bond between the coating and the substrate. These three mechanical test data show that the coating bonds tightly to the automotive anti-slip sticker substrate, exhibiting excellent bending and tensile strength, and can withstand the tensile, bending, and friction forces encountered in daily use. Its mechanical adaptability fully meets the requirements for automotive applications.

[0044] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A wear-resistant coating material for the surface of a vehicle anti-slip sticker, characterized in that, It is composed of component A and component B in a weight ratio of 10-15:1, wherein: Component A contains the following raw materials in parts by weight: Alkoxysilane-terminated polysiloxane: 50-65 parts; Perfluoropolyether-based epoxysilane: 20-30 parts; γ-glycidyl etheroxypropyltrimethoxysilane: 3-5 parts; Trifluoromethanesulfonic acid metal salt catalyst: 0.1-0.5 parts; Nano silicon carbide: 5-8 parts; Component B contains the following raw materials in parts by weight: aminopropyltriethoxysilane: 2-4 parts; Polyethyleneimine: 1-2 parts; Nano boron nitride: 2-4 parts.

2. The wear-resistant coating material for the surface of a vehicle anti-slip sticker according to claim 1, characterized in that, The alkoxysilane-terminated polysiloxane is α,ω-ethoxy / methoxy-terminated polydimethylsiloxane, with an ethoxy to methoxy molar ratio of 1:0.8-1.2, a number-average molecular weight of 18,000-25,000, a total alkoxy content of 2.8-3.2 wt%, a rotational viscosity of 2500-3500 mPa·s at 25°C, and a volatile content of ≤0.5% after 2 hours at 105°C.

3. The wear-resistant coating material for the surface of a vehicle anti-slip sticker according to claim 1, characterized in that, The chemical structural formula of the perfluoropolyether-based epoxysilane is: CF3O-(CF2CF2O). m -(CF2O) n -CF2-CH2-O-CH2-CH(O)CH2-O-CH2-CH2-CH2-Si(OCH3)3, where m=8-12, n=2-4, number average molecular weight is 1300-1700, epoxy value is 0.32-0.38mmol / g, fluorine content is 55-60wt%, and viscosity at 25℃ is 700-900mPa·s.

4. The wear-resistant coating material for the surface of a vehicle anti-slip sticker according to claim 1, characterized in that, The trifluoromethanesulfonic acid metal salt catalyst is a compound composed of scandium trifluoromethanesulfonic acid and lanthanum trifluoromethanesulfonic acid in a mass ratio of 1.5-2.5:

1. The catalyst has a moisture content of ≤0.1% and a total metal ion content of ≥98.5%.

5. The wear-resistant coating material for the surface of a vehicle anti-slip sticker according to claim 1, characterized in that, The nano-silicon carbide is cubic β-silicon carbide with a primary particle size of 25-35 nm and a secondary agglomeration particle size ≤150 nm. The specific surface area is 70-90 nm. 2 / g, the surface is modified with γ-aminopropyltriethoxysilane, the amount of modifier being 1.5-2.5% of the mass of nano-silicon carbide; the nano-boron nitride is plate-shaped hexagonal boron nitride with a plate diameter of 60-80nm, a thickness of 4-8nm, a plate diameter to thickness ratio of 12-18:1, and a specific surface area of ​​30-40m². 2 / g, the surface is modified with dopamine hydrochloride, and the amount of modifier is 1.2-1.8% of the mass of nano boron nitride.

6. A method for preparing a wear-resistant coating material for the surface of a vehicle anti-slip sticker, the method being used to prepare the wear-resistant coating material for the surface of a vehicle anti-slip sticker as described in any one of claims 1-5, characterized in that, The specific steps of this method are as follows: Preparation of component A: Add alkoxysilane-terminated polysiloxane, perfluoropolyether-based epoxysilane, and γ-glycidyl etheroxypropyltrimethoxysilane to the reactor and stir at 300-500 rpm for 10-15 minutes; add trifluoromethanesulfonic acid metal salt catalyst and stir at 250-300 rpm for 5-10 minutes; add nano-silicon carbide and disperse at 600-800 rpm for 15-20 minutes. Grind the material to a fineness of ≤20μm, filter it through a 200-mesh filter, and then package it. Preparation of component B: Add aminopropyltriethoxysilane and polyethyleneimine to the reaction vessel and stir at 200-300 rpm for 5-8 minutes; Add nano-boron nitride and disperse at 400-500 rpm for 10 minutes; Filtered through a 200-mesh filter and then packaged; Coating and curing: Mix component A and component B evenly at the weight ratio of 10-15:1 as described in claim 1, and apply the mixture to the surface of the vehicle anti-slip sticker substrate, controlling the wet film thickness to be 40-60 μm; place the coated substrate in an environment with a relative humidity of 50-80% and a temperature of 20-35℃ for 20-40 minutes.

7. The method for preparing a wear-resistant coating material for vehicle anti-slip stickers according to claim 6, characterized in that, In the preparation of component A, the inner wall of the reactor is polished to a roughness Ra≤0.8μm before feeding, and the air is replaced with dry nitrogen; the material temperature is kept ≤25℃ when adding the catalyst; nano silicon carbide is added in batches and the material temperature is controlled ≤38℃ when adding it; the roller surface temperature is controlled ≤35℃ when grinding; and nitrogen protection is provided during filling.

8. The method for preparing a wear-resistant coating material for a vehicle anti-slip sticker surface according to claim 6, characterized in that, The grinding process for component A is carried out using a three-roll mill with a roller speed ratio of 1:3:9, and the grinding is performed until the fineness is ≤20μm. The mixing process for coating and curing is carried out using a metering pump with a control accuracy of ±0.5%. The static mixer is 20-40cm long and contains 12-20 spiral blades. The mixed material is transported through an insulated pipeline at 23±2℃.

9. The method for preparing a wear-resistant coating material for a vehicle anti-slip sticker surface according to claim 6, characterized in that, In the preparation of component B, the inner wall of the reactor is polished and the air is replaced with dry nitrogen before feeding; after adding aminopropyltriethoxysilane and polyethyleneimine, the material temperature is controlled to be ≤28℃; when adding nano boron nitride, it is added in batches and the material temperature is controlled to be ≤32℃; nitrogen protection is provided during filling.

10. The method for preparing a wear-resistant coating material for a vehicle anti-slip sticker surface according to claim 6, characterized in that, During the coating and curing process, the substrate surface is wiped with anhydrous ethanol and blown with dry compressed air before coating; components A and B are mixed using a static mixer, and the usable period of the mixed material is 10-15 minutes; the wet film thickness is controlled at 40-60μm, the curing environment is 25±2℃, relative humidity is 65±5%, air flow rate is 0.3-0.5m / s, and it is left to stand for 20-40 minutes.