A composition and method for protecting cast aluminum surfaces
By spraying and baking a protective layer on the surface of cast aluminum, the problem of blackening of the surface due to mud and rainwater corrosion is solved, achieving efficient protection without affecting heat dissipation, and also has the advantages of environmental protection and low cost.
Patent Information
- Application Number
- CN202611525284.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for protecting the surface of cast aluminum are costly and cannot effectively prevent blackening caused by mud and rainwater erosion, which affects heat dissipation.
A protective layer with a thickness of 6-8 μm is formed by spraying and baking a cast aluminum surface protective agent composition comprising 1-methoxy-2-propanol, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, diisopropoxybis(ethoxyacetyl)titanium, methyltrimethoxysilane and 2-methoxyethanol.
It significantly improves the corrosion resistance and anti-discoloration performance of cast aluminum. The protective layer is extremely thin and does not affect heat dissipation. It is environmentally friendly, low in cost, highly adaptable, and has adjustable color and high appearance matching.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal surface treatment technology, specifically relating to a protective agent composition and method for cast aluminum surfaces, and more specifically to a protective agent composition for the protection of cast aluminum alloy surfaces, and a method for protecting cast aluminum surfaces using the protective agent composition. Background Technology
[0002] With the increasing demands for lightweight vehicles, cast aluminum parts are being used more and more widely in automobiles. However, when the surface of cast aluminum parts comes into contact with mud or rainwater, it is prone to react with acids or alkalis in the medium, resulting in the formation of stubborn black spots that severely affect the appearance and frequently cause market complaints. Therefore, effective protective treatment of cast aluminum surfaces is necessary.
[0003] Currently, the commonly used methods for surface protection of cast aluminum alloys mainly fall into the following three categories: (1) Chemical oxidation method: The finished parts are oxidized in an acidic oxidation solution. The process flow is usually: degreasing → water washing → pickling → water washing → chemical oxidation → water washing → drying. The oxide film formed by this method is relatively thin and has poor protective performance. At the same time, the surface roughness of cast aluminum parts is relatively large, and the protective effect of a thin oxide film on a rough surface is even worse. In addition, the change in the content of trace elements (such as silicon) in cast aluminum has a significant impact on the protective effect of the oxide film, resulting in high adaptability requirements for the chemical oxidation process.
[0004] (2) Electrochemical oxidation method: The finished parts are immersed in a sulfuric acid solution of a certain concentration, and an electric current is applied to the parts. A relatively thick oxide film is generated on the surface of the parts through electrochemical action. The process flow is usually: degreasing → water washing → pickling → water washing → electrochemical oxidation → water washing → drying. The thickness of the oxide film can be adjusted as needed, but special tooling must be used. The process time is long, production is limited, and the cost is high. Moreover, the oxide film still cannot effectively prevent the corrosion of acids and alkalis in mud or rainwater.
[0005] (3) Varnish or transparent powder spraying method: After pretreatment such as grinding and oxidation, the finished parts are sprayed with varnish or transparent powder. The process flow is usually as follows: degreasing → water washing → pickling → water washing → phosphating → water washing → drying → varnish spraying (or transparent powder spraying) → baking → cooling. The paint layer or powder coating formed by this method is relatively thick, which may affect heat dissipation on some parts.
[0006] Therefore, how to solve the problem of blackening of cast aluminum surfaces due to erosion by mud and rainwater without affecting the heat dissipation and other functions of cast aluminum parts at low cost is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] In view of the deficiencies in the existing technology, the purpose of this invention is to provide a protective agent composition and protection method for cast aluminum surfaces, so as to solve the technical problems of high cost, impaired heat dissipation, and inability to effectively prevent cast aluminum surfaces from turning black due to mud and rainwater erosion.
[0008] To achieve the above objectives, the first aspect of the present invention provides a cast aluminum surface protective agent composition, which comprises the following components by weight: 1-Methoxy-2-propanol 45wt%~55wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 25wt%~35wt% Diisopropoxydi(ethoxyacetyl)titanium 5wt%~10wt% Methyltrimethoxysilane 1.5wt%~2.5wt% 2-Methoxyethanol (ethylene glycol monomethyl ether) 10wt%~15wt% Pigment 0~4wt%.
[0009] In some embodiments, the viscosity of the cast aluminum surface protectant composition is 10-13 s.
[0010] A second aspect of the present invention provides a method for protecting a cast aluminum surface using a cast aluminum surface protective agent composition as described in the first aspect of the present invention, comprising the following steps: Pre-treatment of cast aluminum parts; The cast aluminum surface protective agent composition is applied to the pretreated surface of the cast aluminum part; The cast aluminum parts to which the protective agent composition is applied are post-treated to form a protective layer on the surface of the cast aluminum parts.
[0011] In some embodiments, the pretreatment includes chromium-free passivation and / or trivalent chromium passivation.
[0012] In some embodiments, the method of application includes spraying.
[0013] In some embodiments, the post-processing includes baking the cast aluminum part to which the protective agent composition has been applied, wherein the baking temperature is 180-200°C and the baking time is 20-25 minutes.
[0014] In some embodiments, the method further includes shot peening and ultrasonic cleaning of the cast aluminum parts before pretreatment.
[0015] In some embodiments, the shot peening treatment time is 3-4 minutes; and / or The ultrasonic cleaning temperature is 20~25℃, and the ultrasonic cleaning time is 2~3 minutes.
[0016] In some embodiments, after pretreating the cast aluminum part and before applying the cast aluminum surface protective agent composition to the pretreated cast aluminum part surface, the method further includes: washing and drying the pretreated cast aluminum part; wherein the drying temperature is 80~100°C.
[0017] In some embodiments, the thickness of the protective layer is 6-8 μm.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Significantly improved corrosion resistance and anti-discoloration properties. This invention utilizes a cast aluminum surface protective agent composition to form a protective layer on the surface of cast aluminum parts. This not only effectively seals the micropores on the cast aluminum surface and in the pretreatment film, but also significantly improves the corrosion resistance and acid / alkali corrosion resistance of the cast aluminum parts. Testing shows that the protective layer obtained by this invention has a neutral salt spray time ≥264h and a UV aging resistance time ≥240h.
[0019] 2. The protective layer is extremely thin and does not affect the heat dissipation function of the cast aluminum parts. The protective layer of this invention is only 6~8μm thick. This extremely thin thickness not only provides excellent protective performance, but also does not adversely affect the heat dissipation function of the cast aluminum parts, thus solving the technical contradiction of "difficulty in balancing protective performance and heat dissipation function" in related technologies.
[0020] 3. Good environmental performance The components in the aluminum surface protective agent composition provided by this invention, as well as the steps in the protective method, all meet environmental protection requirements.
[0021] 4. Color adjustable, high degree of appearance matching This invention allows for the addition of appropriate pigments to the formulation as needed to achieve a transparent or specified color protective layer, solving the problem of fixed and monotonous film color in related traditional technologies and improving the matching degree with the overall vehicle appearance.
[0022] 5. Low cost, simple process, and strong adaptability Compared with electrochemical oxidation, this invention does not require special tooling, has a shorter process time, and lower production costs; compared with chemical oxidation, this invention is less sensitive to changes in the content of trace elements (such as silicon) in cast aluminum parts and has strong process adaptability; compared with spraying clear varnish or spraying transparent powder, this invention does not require complex pretreatment processes such as phosphating, simplifies the process flow, and reduces overall costs.
[0023] In summary, this invention effectively solves the problem of blackening of cast aluminum surfaces caused by mud and rainwater erosion, while maintaining low cost and without affecting the heat dissipation function of the cast aluminum parts. It also has advantages such as good environmental performance and adjustable appearance color, and has good prospects for industrial application. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0025] Common methods for surface protection of cast aluminum alloys include chemical oxidation, electrochemical oxidation, and spraying with varnish or transparent powder. Among these, chemical oxidation produces a thinner oxide film with poorer protective performance; furthermore, the surface roughness of cast aluminum parts is relatively high, and a thinner oxide film provides even less protection on rough surfaces; additionally, variations in the content of trace elements (such as silicon) in the cast aluminum significantly affect the protective effect of the oxide film, leading to high requirements for the adaptability of the chemical oxidation process. Electrochemical oxidation allows for adjustment of the oxide film thickness as needed, but requires specialized tooling, has a long processing time, significant production limitations, and high costs; furthermore, this oxide film still cannot effectively prevent corrosion from acids and alkalis in mud or rainwater. For parts with complex structures, spraying with varnish or transparent powder may not be possible to cover internal or hard-to-reach areas; and the thick paint or powder layer can affect heat dissipation on some parts.
[0026] In view of this, the present invention provides a protective agent composition and a protective method for cast aluminum surfaces, in order to solve the technical problems of high cost, impaired heat dissipation, and inability to effectively prevent cast aluminum surfaces from turning black due to erosion by mud and rainwater in related protective methods.
[0027] In a first aspect, embodiments of the present invention provide a surface protective agent composition for cast aluminum, which comprises the following components by weight: 1-Methoxy-2-propanol 45wt%~55wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 25wt%~35wt% Diisopropoxydi(ethoxyacetyl)titanium 5wt%~10wt% Methyltrimethoxysilane 1.5wt%~2.5wt% 2-Methoxyethanol (ethylene glycol monomethyl ether) 10wt%~15wt% Pigment 0~4wt%.
[0028] Of the above components, 1-methoxy-2-propanol is the solvent, used to disperse the other components and form a stable, homogeneous coating system. It evaporates during baking and film formation, and is not present in the film layer. 3-(2,3-epoxypropoxy)propyltrimethoxysilane is an auxiliary film-forming agent, used to improve film adhesion. Diisopropoxybis(ethoxyacetyl)titanium is an auxiliary film-forming agent, used to improve film adhesion, heat resistance, and hardness. Methyltrimethoxysilane is the main film-forming agent, used to form a 6-8 μm film layer. 2-Methoxyethanol (ethylene glycol monomethyl ether) is a leveling agent, used to improve leveling and lubrication properties and enhance film gloss. Pigments are used to change the film color as needed.
[0029] In some embodiments, the viscosity of the cast aluminum surface protective agent composition is 10~13s (Ford-4 cup, 25±1℃, measurement method according to GB / T 1723).
[0030] In this invention, the viscosity of the cast aluminum surface protective agent composition is limited to the range of 10-13 s to ensure a single spray thickness of 6-8 μm. If the viscosity exceeds this range, it is easy to spray too thick or too thin a layer, affecting the performance of the final protective layer. In actual use, the viscosity of the cast aluminum surface protective agent composition will increase with the duration of use. If the viscosity is found to be too high during use, water can be added to dilute it to the required viscosity range.
[0031] Secondly, embodiments of the present invention also provide a method for protecting a cast aluminum surface using the cast aluminum surface protective agent composition as described in the first aspect of the present invention, comprising the following steps: Pre-treatment of cast aluminum parts; The cast aluminum surface protective agent composition is applied to the pretreated surface of the cast aluminum part; The cast aluminum parts to which the protective agent composition is applied are post-treated to form a protective layer on the surface of the cast aluminum parts.
[0032] In some embodiments, the pretreatment includes chromium-free passivation and / or trivalent chromium passivation.
[0033] In some embodiments, the chromium-free passivation method includes: degreasing and derusting the cast aluminum parts, rinsing them with running water, and then placing them in a commercially available chromium-free passivation solution at room temperature (20~25℃) for 2~3 minutes.
[0034] In some embodiments, the trivalent chromium passivation method includes: cleaning the cast aluminum parts with running water after degreasing and derusting, and then placing them in a trivalent chromium passivation solution (commercially available) at room temperature (20~25℃) for 1~2 minutes.
[0035] In some embodiments, the method of application includes spraying.
[0036] In some embodiments, the post-processing includes baking the cast aluminum part to which the protective agent composition has been applied, wherein the baking temperature is 180-200°C and the baking time is 20-25 minutes.
[0037] In this invention, controlling the baking temperature and baking time is beneficial for achieving better results. If the baking temperature is too low or the baking time is too short, the film layer will not be able to form, and the corrosion resistance will decrease; if the baking temperature is too high or the baking time is too long, the film layer will be over-baked, which will also reduce the corrosion resistance.
[0038] In this invention, before pretreatment of the cast aluminum parts, the method further includes: shot peening and ultrasonic cleaning of the cast aluminum parts. The purpose of shot peening is to remove casting slag and oxide layer from the surface of the cast aluminum parts, and the purpose of ultrasonic cleaning is to remove oil and shot peening debris from the surface of the cast aluminum parts.
[0039] In some embodiments, the shot peening treatment time is 3-4 minutes; and / or The ultrasonic cleaning temperature is 20~25℃, and the ultrasonic cleaning time is 2~3 minutes.
[0040] In this invention, after pretreating the cast aluminum part and before applying the cast aluminum surface protective agent composition to the pretreated surface of the cast aluminum part, the method further includes: washing and drying the pretreated cast aluminum part. The purpose of washing is to remove residues from the previous treatment process; failure to do so will affect the subsequent film formation of the protective agent, resulting in a decrease in the performance of the protective layer. The purpose of drying is to ensure that there are no water stains on the surface of the cast aluminum part before spraying the protective agent composition; otherwise, the protective agent will not be able to form a film, resulting in a decrease in the performance of the protective layer.
[0041] In some embodiments, the drying process is carried out at a temperature of 80-100°C.
[0042] In some embodiments, the thickness of the protective layer is 6-8 μm.
[0043] In this invention, controlling the thickness of the protective layer to 6-8 μm is beneficial for achieving better results. If the protective layer is too thin, it will result in poor corrosion resistance; if the protective layer is too thick, it will affect heat dissipation. In some specific embodiments, the method of protecting the surface of cast aluminum using the aforementioned cast aluminum surface protective agent composition includes the following steps: S1, shot peening is performed on the cast aluminum parts for 3-4 minutes.
[0044] S2, the shot-peened cast aluminum parts are placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 20~25℃ and the time is 2~3min.
[0045] S3 is a pretreatment process for cast aluminum parts after ultrasonic cleaning.
[0046] S4, the pre-treated cast aluminum parts are washed with water.
[0047] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 80~100℃.
[0048] S6, the above-mentioned aluminum surface protectant composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protectant composition is 10~13s.
[0049] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition is baked at a temperature of 180~200℃ for 20~25min. After cooling, a protective layer with a thickness of 6~8μm is formed on the surface of the cast aluminum part.
[0050] The surface protective agent composition for cast aluminum provided by this invention can form a protective layer with a thickness of 6~8μm on the surface of cast aluminum parts. This extremely thin thickness not only provides excellent protective performance, but also does not adversely affect the heat dissipation function of cast aluminum parts, thus solving the technical contradiction of "difficulty in balancing protective performance and heat dissipation function" in related technologies.
[0051] Example Unless otherwise specified, all raw materials used in the embodiments of the present invention are commercially available, all instruments and equipment used are conventional instruments and equipment in the art, and all operating methods used are conventional methods in the art.
[0052] Example 1 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 50wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 30wt% Diisopropoxydi(ethoxyacetyl)titanium 7wt% Methyltrimethoxysilane 1.7wt% 2-Methoxyethanol 11.3 wt% Pigment 0wt%.
[0053] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0054] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0055] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0056] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0057] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0058] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0059] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.3 μm on the surface of the cast aluminum part.
[0060] Example 2 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 45wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 35wt% Diisopropyloxydi(ethoxyacetyl)titanium 5wt% Methyltrimethoxysilane 1.5wt% 2-Methoxyethanol 13.5wt% Pigment 0wt%.
[0061] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0062] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0063] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0064] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0065] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0066] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0067] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.0 μm on the surface of the cast aluminum part.
[0068] Example 3 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 55wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 25wt% Diisopropyloxydi(ethoxyacetyl)titanium 8wt% 2wt% methyltrimethoxysilane 2-Methoxyethanol 10wt% Pigment 0wt%.
[0069] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0070] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0071] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0072] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0073] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0074] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0075] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.6 μm on the surface of the cast aluminum part.
[0076] Example 4 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 52wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 25wt% Diisopropyloxydi(ethoxyacetyl)titanium 8wt% 2wt% methyltrimethoxysilane 2-Methoxyethanol 10wt% Zinc-aluminum paste pigment 3wt%.
[0077] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0078] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0079] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0080] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0081] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0082] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0083] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.9 μm on the surface of the cast aluminum part.
[0084] Example 5 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 50wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 30wt% Diisopropoxydi(ethoxyacetyl)titanium 7wt% Methyltrimethoxysilane 1.7wt% 2-Methoxyethanol 11.3 wt% Pigment 0wt%.
[0085] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0086] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0087] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0088] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0089] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0090] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0091] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 160°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.4 μm on the surface of the cast aluminum part.
[0092] Example 6 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 50wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 30wt% Diisopropoxydi(ethoxyacetyl)titanium 7wt% Methyltrimethoxysilane 1.7wt% 2-Methoxyethanol 11.3 wt% Pigment 0wt%.
[0093] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0094] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0095] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0096] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0097] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0098] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0099] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 220°C for 22 minutes, and then cooled to form a protective layer with a thickness of 6.3 μm on the surface of the cast aluminum part.
[0100] Example 7 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 50wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 30wt% Diisopropoxydi(ethoxyacetyl)titanium 7wt% Methyltrimethoxysilane 1.7wt% 2-Methoxyethanol 11.3 wt% Pigment 0wt%.
[0101] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0102] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0103] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0104] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0105] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0106] S6, The above-mentioned aluminum surface protection agent composition is applied to the dried aluminum surface by spraying. The viscosity of the aluminum surface protection agent composition is 8s (this viscosity is obtained by dilution).
[0107] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 4.7 μm on the surface of the cast aluminum part.
[0108] Example 8 The composition of the cast aluminum surface protective agent provided in this embodiment is as follows: 1-Methoxy-2-propanol 50wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 30wt% Diisopropoxydi(ethoxyacetyl)titanium 7wt% Methyltrimethoxysilane 1.7wt% 2-Methoxyethanol 11.3 wt% Pigment 0wt%.
[0109] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this embodiment includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0110] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0111] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0112] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0113] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0114] S6. The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 15s (this viscosity can be obtained after a period of use).
[0115] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 9.4 μm on the surface of the cast aluminum part.
[0116] Comparative Example 1 The composition of the cast aluminum surface protectant provided in this comparative example is as follows: 1-Methoxy-2-propanol 40wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 40wt% Diisopropyloxydi(ethoxyacetyl)titanium 4wt% 1 wt% methyltrimethoxysilane 2-Methoxyethanol 15wt% Pigment 0wt%.
[0117] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this comparative example includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0118] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0119] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0120] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0121] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0122] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0123] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 5.1 μm on the surface of the cast aluminum part.
[0124] Comparative Example 2 The composition of the cast aluminum surface protectant provided in this comparative example is as follows: 1-Methoxy-2-propanol 58wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 22wt% Diisopropoxydi(ethoxyacetyl)titanium 12wt% Methyltrimethoxysilane 0.5wt% 2-Methoxyethanol 7.5wt% Pigment 0wt%.
[0125] The method for protecting the surface of cast aluminum using the above-mentioned cast aluminum surface protective agent composition provided in this comparative example includes the following steps: S1, The cast aluminum part is shot peened for 3.5 minutes.
[0126] S2, the shot-peened aluminum casting is placed in a cleaning tank equipped with an ultrasonic device for ultrasonic cleaning treatment. The ultrasonic cleaning treatment temperature is 25°C and the time is 2.5 min.
[0127] S3, perform chromium-free passivation pretreatment on the cast aluminum parts after ultrasonic cleaning, specifically including: after degreasing and derusting the cast aluminum parts after ultrasonic cleaning, rinse them with running water, and then put them into a chromium-free passivation solution at a temperature of 25°C for 3 minutes.
[0128] S4. The pre-treated cast aluminum parts are washed with water to remove residues.
[0129] S5, the cast aluminum parts that have been washed with water are dried at a temperature of 100°C.
[0130] S6, The above-mentioned aluminum surface protection agent composition is applied to the surface of the dried aluminum part by spraying. The viscosity of the aluminum surface protection agent composition is 12s.
[0131] S7. The cast aluminum part with the above-mentioned cast aluminum surface protective agent composition applied is baked at a temperature of 190°C for 22 minutes, and then cooled to form a protective layer with a thickness of 4.7 μm on the surface of the cast aluminum part.
[0132] The protective layers prepared in Examples 1-8 and Comparative Examples 1-2 were subjected to neutral salt spray performance tests (GB / T 10125) and UV aging resistance tests (GB / T 23987.3). The specific test results are shown in Table 1.
[0133] Table 1. Test results of protective layer performance
[0134] Analysis of Table 1 shows that: The protective layer prepared in Examples 1-8 of this invention has a neutral salt spray resistance of ≥264h, which is much higher than the 120h requirement for neutral salt spray in existing cast aluminum anti-corrosion technology; moreover, it has an ultraviolet aging resistance of ≥240h, exhibiting excellent corrosion resistance.
[0135] Among them, the protective layers prepared in Examples 1-4 have a neutral salt spray resistance of ≥480h and a UV aging resistance of up to 500h, exhibiting superior overall performance in terms of protective layer thickness, neutral salt spray resistance, and UV aging resistance. In Example 5, the baking temperature was too low, and in Example 6, the baking temperature was too high, resulting in a decrease in both neutral salt spray resistance and UV aging resistance. In Example 7, the viscosity of the cast aluminum surface protective agent composition was too low, leading to a decrease in neutral salt spray performance. In Example 8, the viscosity of the cast aluminum surface protective agent composition was too high; although the neutral salt spray resistance and UV aging resistance were relatively good, the excessive thickness of the protective layer would severely affect the heat dissipation function of the cast aluminum parts.
[0136] Compared to Example 1, under the same conditions, the neutral salt spray and UV aging resistance properties decreased in Comparative Examples 1 and 2 after the formulation of the protective agent composition was changed.
[0137] Therefore, it can be seen that the cast aluminum surface protective agent composition and protection method provided by the present invention can solve the technical problem that related technologies cannot effectively prevent the cast aluminum surface from turning black due to mud and rainwater erosion under low cost and without affecting heat dissipation.
[0138] In the description of this specification, the references to terms such as "one embodiment / mode," "some embodiments / modes," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment / mode or example is included in at least one embodiment / mode or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment / mode or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments / modes or examples. Furthermore, without contradiction, those skilled in the art can combine and integrate the different embodiments / modes or examples described in this specification, as well as the features of different embodiments / modes or examples.
[0139] It should be noted that in this invention, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element. In this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise expressly specified.
[0140] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A composition of a surface protective agent for cast aluminum, characterized in that, It comprises the following components by weight: 1-Methoxy-2-propanol 45wt%~55wt% 3-(2,3-epoxypropoxy)propyltrimethoxysilane 25wt%~35wt% Diisopropoxydi(ethoxyacetyl)titanium 5wt%~10wt% Methyltrimethoxysilane 1.5wt%~2.5wt% 2-Methoxyethanol 10wt%~15wt% Pigment 0~4wt%.
2. The cast aluminum surface protective agent composition according to claim 1, characterized in that, The viscosity of the cast aluminum surface protective agent composition is 10~13s.
3. A method for protecting the surface of cast aluminum using the cast aluminum surface protective agent composition as described in claim 1, characterized in that, Includes the following steps: Pre-treatment of cast aluminum parts; The cast aluminum surface protective agent composition is applied to the pretreated surface of the cast aluminum part; The cast aluminum parts to which the protective agent composition is applied are post-treated to form a protective layer on the surface of the cast aluminum parts.
4. The method according to claim 3, characterized in that, The pretreatment includes chromium-free passivation and / or trivalent chromium passivation.
5. The method according to claim 3, characterized in that, The method of application includes spraying.
6. The method according to claim 5, characterized in that, The post-treatment includes baking the cast aluminum part to which the protective agent composition has been applied, wherein the baking temperature is 180~200℃ and the baking time is 20~25min.
7. The method according to claim 3, characterized in that, Before pretreatment of the cast aluminum parts, the method further includes: shot peening and ultrasonic cleaning of the cast aluminum parts.
8. The method according to claim 7, characterized in that, The shot peening treatment time is 3-4 minutes; and / or The ultrasonic cleaning temperature is 20~25℃, and the ultrasonic cleaning time is 2~3 minutes.
9. The method according to claim 3, characterized in that, After pretreatment of the cast aluminum part and before applying the cast aluminum surface protective agent composition to the surface of the pretreated cast aluminum part, the method further includes: washing and drying the pretreated cast aluminum part; wherein the drying temperature is 80~100℃.
10. The method according to claim 3, characterized in that, The thickness of the protective layer is 6~8μm.