Methods to reduce glass powder agglomeration during glass wafer polishing

By adding disodium ethylenediaminetetraacetate and potassium hydroxide to the polishing solution to adjust the pH, and combining this with the adsorption of urea and Zn2+ during the preparation process, the problems of micro-powder agglomeration and high roughness during glass wafer polishing were solved, achieving efficient polishing removal and surface quality improvement.

CN123107546APending Publication Date: 2026-11-17ZHEJIANG LANTE OPTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611327803.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously address the issues of glass powder agglomeration, high wafer roughness, and low material removal rate during glass wafer polishing.

Method used

By adding disodium ethylenediaminetetraacetate to the polishing solution and adjusting the pH to 9-9.5 with potassium hydroxide solution, combined with the use of urea for high-temperature slow-release of hydroxide ions, polyvinylpyrrolidone adsorption on the crystal surface, and Zn2+ adsorption on the CeO2 surface during the preparation process, a stable negative charge environment is formed, which inhibits the agglomeration of glass micropowder.

Benefits of technology

It effectively inhibits the agglomeration of glass micropowder, reduces wafer surface roughness, improves polishing removal rate, extends the service life of polishing fluid, and reduces scratches and pitting defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for reducing glass powder agglomeration during glass wafer polishing, relating to the field of chemical mechanical polishing (CMP) technology. The invention involves adding disodium ethylenediaminetetraacetate (EDTA) to the polishing slurry and adjusting the pH of the slurry to 9-9.5 with potassium hydroxide solution. The resulting glass polishing powder reduces primary powder agglomeration, enhances cutting activity, and optimizes surface charge properties. The combination of disodium EDTA complexes metal ions to eliminate ion bridging, and potassium hydroxide solution regulates the weak alkalinity to enhance electrostatic repulsion of particles. This dual mechanism synergistically inhibits glass powder agglomeration, increases the polishing removal rate, and reduces wafer surface roughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical mechanical polishing technology, specifically to a method for reducing the agglomeration of glass micropowder during the polishing process of glass wafers. Background Technology

[0002] With the rapid development of optical sensing and optical communication, the batch double-sided polishing process for large-size optical glass wafers has become widely adopted. Cerium oxide polishing slurry is a core consumable for achieving ultra-precision planarization of wafers, and the industry has conducted extensive research on slurry dispersion stability and improving polished product yield. Currently, improving particle agglomeration usually involves adjusting the pH with a single alkali. However, this system cannot eliminate metal impurity ions introduced by water sources and equipment wear. After long-term circulation, ion accumulation will continue to induce flocculation. Simply adding chelating agents or polymeric dispersants lacks a stable alkaline environment, resulting in insufficient electrostatic repulsion strength of particles. The dispersion effect decays rapidly with processing time, and the micron-sized hard particles formed by agglomeration participate in polishing with the slurry circulation, continuously scratching the wafer surface and significantly increasing the surface defect rate. At the same time, the proportion of effective free abrasive in the system decreases, the polishing removal rate continues to decline, the polishing slurry replacement cycle is shortened, and consumable and downtime costs increase significantly. Existing technologies cannot simultaneously achieve long-term anti-agglomeration, stable polishing efficiency, and ultra-low surface roughness. There is an urgent need to develop a control method adapted to the cyclic polishing of glass wafers and synergistically blocking multi-path agglomeration.

[0003] In existing technologies, relying solely on a single method for regulation cannot simultaneously eliminate multiple agglomeration inducing factors. Adjusting the pH of the polishing slurry only alleviates particle aggregation through electrostatic repulsion; pH adjusters lack chelating ability and cannot remove the continuously accumulating polyvalent metal ions within the system. These metal ions will form ion bridges through coordination, crosslinking cerium oxide abrasive and glass micropowder, continuously generating irreversible agglomerated particles. Ordinary cerium oxide has a high isoelectric point, and the electrostatic repulsion generated by adjusting the alkali is limited, insufficient to counteract the van der Waals attraction between particles, leading to soft agglomeration and sedimentation even after long-term cycling. A large number of composite agglomerated particles will encapsulate the internal nano-abrasives, obscuring cutting active sites, weakening the mechanical and chemical removal effects at the polishing interface, and reducing the material removal rate. Simultaneously, hard agglomerated particles continuously scrape the wafer, causing scratches and pitting, and uneven slurry dispersion leads to inconsistent cutting rates, disrupting microscopic planar uniformity, ultimately significantly increasing the surface roughness of the glass wafer and increasing surface defects in the product. Summary of the Invention

[0004] The purpose of this invention is to provide a method for reducing the agglomeration of glass powder during glass wafer polishing, thereby solving the following technical problems: Existing glass wafer polishing processes suffer from problems such as glass powder agglomeration, high wafer roughness, and low material removal rate.

[0005] The objective of this invention can be achieved through the following technical solutions: A method to reduce the agglomeration of glass micropowder during glass wafer polishing involves adding disodium ethylenediaminetetraacetate to the polishing solution and adjusting the pH of the polishing solution to 9-9.5 with potassium hydroxide solution.

[0006] As a further aspect of the present invention: the polishing liquid is composed of glass polishing micro powder and deionized water in a mass ratio of 5-15:95-85.

[0007] As a further aspect of the present invention, the method for preparing the glass polishing micro powder includes the following steps: CeO2 powder and deionized water were added to a beaker and ultrasonically dispersed for 10-20 min. Zn(CH3COOH)2 was added and stirred for 2-3 h. The mixture was then dried and calcined to obtain glass polishing micro powder.

[0008] As a further aspect of the present invention: the ratio of CeO2 powder, deionized water and Zn(CH3COOH)2 is 8-12g:90-110mL:0.24-0.96g; The drying and calcination process includes: after the reaction is completed, the reaction solution is placed in an oven at 85-95℃ to evaporate to dryness, and then the dried sample is placed in a muffle furnace at 300℃ for 3 hours to obtain glass polishing micro powder.

[0009] As a further aspect of the present invention, the method for preparing the CeO2 powder includes the following steps: A1, cerium nitrate hexahydrate, polyvinylpyrrolidone and deionized water were added to a hydrothermal reactor for dispersion, urea solution was added for dispersion, the temperature was raised to 95-105℃ and kept at that temperature for 3.5-4.5h, washed and dried to obtain the cerium-based precursor; A2. Add the cerium-based precursor and hydrogen peroxide aqueous solution to a beaker, heat to 70-80℃ and stir for 1.5-2.5h, dry and anneal to obtain CeO2 powder.

[0010] As a further aspect of the present invention: in step A1, the ratio of cerium nitrate hexahydrate, polyvinylpyrrolidone, deionized water, and urea solution is 2.9-3.0g: 4.4-4.6g: 45-55mL: 84-86mL; the concentration of the urea solution is 29wt%. The washing and drying process includes: after the reaction is completed, the reaction solution is centrifuged, the solid precipitate is washed 3-5 times with anhydrous ethanol and deionized water, and then dried in a drying oven at 60-80℃ until constant weight to obtain the cerium-based precursor.

[0011] As a further aspect of the present invention: in step A2, the ratio of cerium-based precursor to hydrogen peroxide aqueous solution is 2.8-3.2g:93-107mL, and the concentration of hydrogen peroxide aqueous solution is 0.75mol / L; The drying and annealing process includes: after the reaction is completed, the reaction solution is centrifuged, the precipitate is dried at 60°C to constant weight, and then annealed at 500°C for 3.5-4.5 hours in a nitrogen atmosphere to obtain CeO2 powder.

[0012] As a further aspect of the present invention: the ratio of polishing liquid to disodium ethylenediaminetetraacetate is 1L:2g; the concentration of potassium hydroxide solution is 42wt%.

[0013] As a further aspect of the present invention: the polishing slurry is suitable for glass wafers with diameters of Φ100, 200, and 300 mm.

[0014] The beneficial effects of this invention are: 1. In the process of preparing glass polishing micropowder, this invention utilizes the high-temperature slow-release of hydroxide ions from urea to slowly precipitate cerium ions, while polyvinylpyrrolidone adsorbs onto the grain surface to form spatial barriers, preventing the formation of hard agglomerates from instantaneous large-scale precipitation. This results in a cerium-based precursor with uniform particle size and few primary agglomerates, laying the foundation for low-defect glass polishing micropowder; hydrogen peroxide removes cerium ions from the crystal surface. 3+ Oxidation to highly polishable Ce 4+ Nitrogen gas is used for calcination at 500℃ in the absence of air to remove impurities and prevent grain sintering and agglomeration. This enhances the chemical cutting ability of the glass polishing powder, makes the powder loose and easily dispersed, and improves the polishing removal rate. Zn is also used in the preparation of the glass polishing powder. 2+ The CeO2 adsorbs onto the surface and is calcined at low temperature to generate a thin layer of ZnO, which lowers the isoelectric point of the powder. In the weakly alkaline polishing solution, the particles carry a strong negative charge, which greatly enhances electrostatic repulsion. This inhibits the agglomeration of glass micropowder from the source and reduces the agglomeration of glass micropowder during the glass wafer polishing process. At the same time, it moderately reduces the hardness of the abrasive, reduces wafer scratches, and reduces surface roughness.

[0015] 2. This invention utilizes disodium ethylenediaminetetraacetate (EDTA) to form a stable, water-soluble cyclic chelate with polyvalent metal ions, eliminating the metal ion bridging effect and preventing the continuous generation of harmful agglomerated large particles during the cycle. This significantly extends the lifespan of the polishing slurry, maintains a low-agglomeration state throughout the process, and prevents metal ion flocculation and precipitation from adhering to the wafer surface, reducing pitting and crater defects and lowering surface roughness. The polishing slurry is stabilized to a weakly alkaline state using potassium hydroxide solution, allowing zinc-doped cerium oxide and glass micropowder to carry a large amount of negative charge, relying on electrostatic repulsion to inhibit particle adsorption and agglomeration. The disodium EDTA complexes calcium, magnesium, and iron metal ions in the system, eliminating ion bridging and flocculation. The combination of these two mechanisms, with electrostatic dispersion and impurity blocking working simultaneously, effectively inhibits complex agglomeration for a long time, balancing polishing efficiency and wafer surface quality. Detailed Implementation

[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] In this application, the polyvinylpyrrolidone is PVP-K30, CAS number 9003-39-8, selected from Wuhan Xinli Biotechnology Co., Ltd., with a purity of 99.9%.

[0018] Example 1

[0019] A method for reducing glass powder agglomeration during glass wafer polishing includes the following steps: S1. Preparation of glass polishing micro powder Weigh 2.9 g of cerium nitrate hexahydrate, 4.4 g of polyvinylpyrrolidone and 45 mL of deionized water and add them to a hydrothermal reactor. Stir at room temperature for 10 min, then add 84 mL of 29 wt% urea solution and stir for 50 min. Heat to 95 °C and keep warm for 3.5 h. After the reaction is complete, centrifuge the precipitate, wash it three times with anhydrous ethanol and then three times with deionized water. Then dry it in a 60 °C drying oven to constant weight to obtain the cerium-based precursor. Weigh 2.8g of cerium-based precursor and 93mL of 0.75mol / L hydrogen peroxide aqueous solution and add them to a beaker. Heat to 70℃ and stir for 1.5h. After the reaction is complete, centrifuge the reaction solution, take the precipitate and dry it at 60℃ to constant weight. Then anneal it at 500℃ for 3.5h in a nitrogen atmosphere to obtain CeO2 powder. Weigh 8g of CeO2 powder and 90mL of deionized water into a beaker, sonicate for 10min, add 0.24g of Zn(CH3COOH)2, stir for 2h, after the reaction is complete, put the reaction solution into an oven at 85℃ to evaporate to dryness, and then put the dried sample into a muffle furnace at 300℃ for 3h to obtain glass polishing micro powder.

[0020] S2. Preparation of polishing fluid for glass wafer polishing

[0021] Add 5g of glass polishing powder and 95g of deionized water to a mixing tank and stir for 10 minutes to obtain a polishing solution. Add 2g of disodium ethylenediaminetetraacetate to 1L of polishing solution, stir for 10min, adjust the pH to 9 with potassium hydroxide solution, and after the adjustment is completed, stir and homogenize to obtain the polishing solution for glass wafer polishing.

[0022] Example 2

[0023] A method for reducing glass powder agglomeration during glass wafer polishing includes the following steps: S1. Preparation of glass polishing micro powder Weigh 2.95 g of cerium nitrate hexahydrate, 4.5 g of polyvinylpyrrolidone and 50 mL of deionized water and add them to a hydrothermal reactor. Stir at room temperature for 15 min, add 85 mL of 29 wt% urea solution, stir for 60 min, raise the temperature to 100 °C and keep it at that temperature for 4 h. After the reaction is complete, centrifuge the precipitate, wash it 4 times with anhydrous ethanol and deionized water, and then dry it in a 70 °C drying oven to constant weight to obtain the cerium-based precursor. Weigh 3.0 g of cerium-based precursor and 100 mL of 0.75 mol / L hydrogen peroxide aqueous solution and add them to a beaker. Heat to 75 °C and stir for 2.0 h. After the reaction is complete, centrifuge the reaction solution, take the precipitate and dry it at 70 °C to constant weight. Then anneal it at 500 °C for 4.0 h in a nitrogen atmosphere to obtain CeO2 powder. Weigh 10g of CeO2 powder and 100mL of deionized water into a beaker, sonicate for 15min, add 0.6g of Zn(CH3COOH)2, stir for 2.5h, after the reaction is complete, put the reaction solution into an oven at 90℃ to evaporate to dryness, and then put the dried sample into a muffle furnace at 300℃ for 3h to obtain glass polishing micro powder.

[0024] S2. Preparation of polishing fluid for glass wafer polishing

[0025] Add 10g of glass polishing powder and 90g of deionized water to a mixing tank and stir for 15 minutes to obtain a polishing solution. Add 2g of disodium ethylenediaminetetraacetate to 1L of polishing solution, stir for 15min, adjust the pH to 9.3 with potassium hydroxide solution, and after the adjustment is completed, stir and homogenize to obtain the polishing solution for glass wafer polishing.

[0026] Example 3

[0027] A method for reducing glass powder agglomeration during glass wafer polishing includes the following steps: S1. Preparation of glass polishing micro powder Weigh 3.0 g of cerium nitrate hexahydrate, 4.6 g of polyvinylpyrrolidone and 55 mL of deionized water and add them to a hydrothermal reactor. Stir at room temperature for 20 min, add 86 mL of 29 wt% urea solution, stir for 70 min, raise the temperature to 105 °C and keep it at that temperature for 4.5 h. After the reaction is complete, centrifuge the precipitate, wash it 5 times with anhydrous ethanol and deionized water, and then dry it in an 80 °C drying oven to constant weight to obtain the cerium-based precursor. Weigh 3.2g of cerium-based precursor and 107mL of 0.75mol / L hydrogen peroxide aqueous solution and add them to a beaker. Heat to 80℃ and stir for 2.5h. After the reaction is complete, centrifuge the reaction solution, take the precipitate and dry it at 80℃ to constant weight. Then anneal it at 500℃ for 4.5h in a nitrogen atmosphere to obtain CeO2 powder. Weigh 12g of CeO2 powder and 110mL of deionized water into a beaker, sonicate for 20min, add 0.96g of Zn(CH3COOH)2, stir for 3h, after the reaction is complete, put the reaction solution into an oven at 95℃ to evaporate to dryness, and then put the dried sample into a muffle furnace at 300℃ for 3h to obtain glass polishing micro powder.

[0028] S2. Preparation of polishing fluid for glass wafer polishing

[0029] Add 15g of glass polishing powder and 85g of deionized water to a mixing tank and stir for 20 minutes to obtain a polishing solution. Add 2g of disodium ethylenediaminetetraacetate to 1L of polishing solution, stir for 20min, adjust the pH to 9.5 with potassium hydroxide solution, and after adjustment, stir and homogenize to obtain the polishing solution for glass wafer polishing.

[0030] Comparative Example 1

[0031] The difference between this comparative example and Example 3 is that Zn(CH3COOH)2 was not added in step S1, while the other components are exactly the same.

[0032] Comparative Example 2

[0033] The difference between this comparative example and Example 3 is that disodium ethylenediaminetetraacetate was not added in step S3, while the other components are exactly the same.

[0034] Comparative Example 3

[0035] The difference between this comparative example and Example 3 is that in step S3, potassium hydroxide solution was not used to adjust the pH, while the other components are exactly the same.

[0036] Performance testing

[0037] The polishing slurries for polishing glass wafers prepared in Examples 1-3 and Comparative Examples 1-3 were put into a polishing machine to polish glass wafers with a diameter of Φ200mm. After polishing, the glass wafers are cleaned and dried. The mass of the glass wafers before and after polishing is weighed using an analytical balance. The material removal rate is calculated based on the mass difference of the glass wafers before and after polishing. The surface roughness of the polished glass wafer was measured using an atomic force microscope (AFM). The particle size distribution of the polishing slurries for glass wafer polishing prepared in Examples 1-3 and Comparative Examples 1-3 was determined according to the standard GB / T 32698-2016 "Determination of particle size distribution of precipitated hydrated silica in rubber compounding agents by laser diffraction". The test results are shown in the table below:

[0038] As shown in the table, the polishing slurry for glass wafer polishing prepared in this application exhibits a high material removal rate and low surface roughness on the polished glass wafers. The polishing slurry also possesses a strong negative Zeta potential. Compared to Comparative Examples 1-3, the pure CeO2 in Examples 1-3 has a higher isoelectric point and a lower absolute Zeta potential at pH 9-9.5, indicating weak electrostatic repulsion between particles. In the examples, the powder surface is coated with ZnO, resulting in a lower isoelectric point and a significantly increased negative charge density at the same pH, making the glass polishing micropowder less prone to adsorption and aggregation. The polishing slurry has fewer micron-sized agglomerates, and ZnO moderately softens the abrasive, resulting in lower wafer roughness and a higher material removal rate. The polishing slurry used for glass wafer polishing does not precipitate during long-term circulation, maintains a stable amount of effective abrasive, and has a slow decay in removal rate, preventing pitting defects caused by metal impurities on the wafer. The neutral environment results in less hydroxyl dissociation of particles and extremely low surface negative charge. Van der Waals forces dominate particle agglomeration, and the potassium hydroxide solution provides an alkaline environment, constructing a strong electrostatic repulsion barrier. Even without metal ions, the powder can be stably dispersed without large-scale sedimentation, significantly improving polishing uniformity.

[0039] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.

Claims

1. A method for reducing glass powder agglomeration during glass wafer polishing, characterized in that, Disodium ethylenediaminetetraacetate is added to the polishing solution used for glass wafer polishing, and the pH of the polishing solution is adjusted to 9-9.5 with potassium hydroxide solution.

2. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 1, characterized in that, The polishing fluid is composed of glass polishing micro powder and deionized water in a mass ratio of 5-15:95-85.

3. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 2, characterized in that, The preparation method of the glass polishing micro powder includes the following steps: CeO2 powder and deionized water were added to a beaker and ultrasonically dispersed for 10-20 min. Zn(CH3COOH)2 was added and stirred for 2-3 h. The mixture was then dried and calcined to obtain glass polishing micro powder.

4. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 3, characterized in that, The ratio of CeO2 powder, deionized water, and Zn(CH3COOH)2 is 8-12g:90-110mL:0.24-0.96g; The drying and calcination process includes: after the reaction is completed, the reaction solution is placed in an oven at 85-95℃ to evaporate to dryness, and then the dried sample is placed in a muffle furnace at 300℃ for 3 hours to obtain glass polishing micro powder.

5. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 3, characterized in that, The method for preparing the CeO2 powder includes the following steps: A1, cerium nitrate hexahydrate, polyvinylpyrrolidone and deionized water were added to a hydrothermal reactor for dispersion, urea solution was added for dispersion, the temperature was raised to 95-105℃ and kept at that temperature for 3.5-4.5h, washed and dried to obtain the cerium-based precursor; A2. Add the cerium-based precursor and hydrogen peroxide aqueous solution to a beaker, heat to 70-80℃ and stir for 1.5-2.5h, dry and anneal to obtain CeO2 powder.

6. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 5, characterized in that, In step A1, the ratio of cerium nitrate hexahydrate, polyvinylpyrrolidone, deionized water, and urea solution is 2.9-3.0 g : 4.4-4.6 g : 45-55 mL : 84-86 mL; the concentration of the urea solution is 29 wt%. The washing and drying process includes: after the reaction is completed, the reaction solution is centrifuged, the solid precipitate is washed 3-5 times with anhydrous ethanol and deionized water, and then dried in a drying oven at 60-80℃ until constant weight to obtain the cerium-based precursor.

7. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 5, characterized in that, In step A2, the ratio of cerium-based precursor to hydrogen peroxide aqueous solution is 2.8-3.2 g: 93-107 mL, and the concentration of hydrogen peroxide aqueous solution is 0.75 mol / L. The drying and annealing process includes: after the reaction is completed, the reaction solution is centrifuged, the precipitate is dried at 60-80℃ to constant weight, and then annealed at 500℃ for 3.5-4.5h in a nitrogen atmosphere to obtain CeO2 powder.

8. The method for reducing glass powder agglomeration during glass wafer polishing according to claim 1, characterized in that, The ratio of polishing slurry to disodium ethylenediaminetetraacetate was 1L:2g; the concentration of potassium hydroxide solution was 42wt%.