A water-based adhesive, its preparation method and application

By constructing a hydrogen-bonded interpenetrating polymer network on the lithium battery separator, the problems of bonding strength and toughness of the lithium battery separator under high temperature and high pressure are solved, thereby improving the safety and cycle stability of the battery.

CN123107579APending Publication Date: 2026-11-17SHENZHEN HAOFEI IND CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611468660.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium battery separators made of polyolefins have poor thermal stability and are prone to oxidation and degradation, which causes the ceramic coating to peel off and crack under high temperature and high pressure, leading to micro-short circuits in the battery and affecting safety and cycle stability.

Method used

A composite dispersant system is polymerized in an oxygen-free environment to construct a hydrogen-bonded interpenetrating polymer network, forming a high-temperature resistant and highly adhesive water-based binder. This binder is then coated onto the diaphragm surface to enhance the adhesion strength and toughness of the ceramic coating.

Benefits of technology

It improves the stability and safety of lithium batteries under high temperature and high pressure, reduces the risk of micro-short circuits, and enhances the cycle stability and safety of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses an aqueous binder, its preparation method, and its application in ceramic separators for lithium-ion batteries. The aqueous binder comprises a composite dispersant, hard monomers, soft monomers, functional monomers, an initiator, and water; the composite dispersant is selected from at least two of polyvinyl alcohol, polyethylene glycol, polypropylene glycol, polyvinylpyrrolidone, and cellulose derivatives. This invention employs a multi-component dispersant compound system, constructing a double interpenetrating hydrogen-bonded polymer network through in-situ polymerization. Relying on the synergistic effect of multiple dispersants, a robust bonding network is built, allowing the high-temperature thermal shrinkage rate of the separator to be controlled within 3%, while maintaining stable permeability and good uniformity. This binder can stabilize the coating structure, inhibit coating cracking and peeling under high-temperature conditions, ensure lithium-ion conductivity and separator mechanical properties, reduce the risk of micro-short circuits in the battery, effectively improve the cycle stability and safety of lithium batteries, and meet the application requirements of high-energy-density, long-life lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium battery technology, and more specifically, to an aqueous binder, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, with their comprehensive advantages of high energy density, long cycle life, and environmental friendliness, have been widely used in key fields such as new energy vehicles, large-scale energy storage power stations, smart portable terminals, power tools, and aerospace. Among these, the separator, as a crucial component of lithium-ion batteries, not only provides a channel for lithium-ion transport but also prevents contact between the positive and negative electrodes. However, in current technology, approximately 90% of battery abuse incidents originate from internal short circuits caused by separator failure. Traditional polyolefin separators, due to their low melting point, pose a risk of thermal runaway in lithium-ion batteries and also exhibit poor rate performance.

[0003] To address these issues, existing technologies typically employ a method of coating the surface of polyolefin separators with inorganic ceramic microparticles (such as alumina, boehmite, and silica). An adhesive is then used to fix these microparticles to the separator surface, leveraging their high melting point to enhance the separator's thermal stability. Among these, polyacrylate binders, as the core category of waterborne binders for lithium-ion battery ceramic separators, have become the mainstream choice due to their highly tunable molecular structure, excellent affinity with ceramic particles and the base membrane, and superior film-forming properties. However, existing waterborne polyacrylate binders suffer from the following technical drawbacks: First, these binders contain carboxyl and ester groups, making them susceptible to oxidative degradation and molecular chain breakage under high voltage conditions of 4.5V and above, particularly by high-valence transition metal ions and free radicals generated at the positive electrode. This leads to decreased cohesive strength. Second, these binders have limited high-temperature resistance. At temperatures above 100℃, the increased thermal motion of their molecular chains weakens the interfacial forces between them and the ceramic particles and base membrane, resulting in decreased interfacial bonding stability. The combined effect of these problems causes the peel strength of the ceramic separator to decline rapidly with the number of cycles, leading to the detachment and cracking of the ceramic coating. Coating failure not only causes the separator to lose its reinforcing and protective function against the base film, but the detached coating debris may also cause micro-short circuits inside the battery, severely restricting the safe and stable application of lithium batteries in high-end scenarios such as new energy vehicles and energy storage power stations. Summary of the Invention

[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide a high-temperature resistant, high-adhesion water-based adhesive for lithium battery ceramic separators and its preparation method, so as to improve the stability of ceramic separators under high-temperature environments and their coating and adhesion to ceramics.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] On one hand, the present invention provides an aqueous binder comprising a composite dispersant, a hard monomer, a soft monomer, a functional monomer, an initiator, and water;

[0007] The composite dispersant is selected from at least two of polyvinyl alcohol and its derivatives, polyethylene glycol and its derivatives, polypropylene glycol and its derivatives, polyvinylpyrrolidone and its derivatives, and cellulose derivatives; the composite dispersant molecules are linked with monomer copolymer segments, which intertwine with the monomer copolymer segments to form an interpenetrating polymer network structure.

[0008] The mass ratio of the composite dispersant, hard monomer, soft monomer, functional monomer and initiator is 6-23:2-18:2-18:80-120:0.3-2.5.

[0009] Preferably, the composite dispersant is selected from a mixture of polyvinyl alcohol and its derivatives and polyvinylpyrrolidone and its derivatives.

[0010] Preferably, the mass ratio of polyvinyl alcohol and its derivatives to polyvinylpyrrolidone and its derivatives is 1:0.01 to 1:1, and more preferably 1:0.2 to 1:0.6.

[0011] Preferably, the functional monomer is selected from a combination of carboxyl monomers and amide monomers.

[0012] Furthermore, based on the total mass of the two, the mass ratio of the carboxyl monomer to the amide monomer is 80:20 to 50:50, preferably 70:30 to 60:40.

[0013] Furthermore, the carboxyl monomer is selected from at least one of acrylic acid, methacrylic acid, and itaconic acid; the amide monomer is selected from at least one of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide.

[0014] Secondly, the present invention provides a method for preparing an aqueous adhesive, comprising the following steps: By weight, 6-23 parts of composite dispersant, 0.1-1 parts of initiator and 300-500 parts of water are mixed in a reactor under mechanical stirring at 100-300 rpm to obtain a homogeneous solution. Nitrogen gas is continuously introduced to remove oxygen and ensure that the reaction system is in an oxygen-free environment. The composite dispersant is composed of at least two dispersant components. The system was then heated to 65–70°C, and a mixed monomer solution consisting of 2–18 parts hard monomer, 2–18 parts soft monomer, 80–120 parts functional monomer, and 0.5–1.5 parts initiator was added dropwise to the reaction system at a uniform rate. After the addition was completed, the polymerization reaction was maintained at this temperature for 1.5–4 hours. After polymerization, the temperature was raised to 75–80°C and maintained for 2–4 hours for curing. The system was then cooled to 40–45°C, the pH was adjusted to 8±1, and the mixture was filtered to obtain an aqueous binder.

[0015] On the other hand, the present invention provides a lithium-ion battery separator, the lithium-ion battery separator comprising the aqueous binder as described above.

[0016] On the other hand, the present invention provides a lithium-ion battery, the lithium-ion battery comprising the lithium-ion battery separator as described above.

[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention employs a compound dispersant system. Under oxygen-free conditions, it suppresses viscosity abrupt changes caused by monomer polymerization through steric hindrance, ensuring a stable and controllable solution polymerization process. Furthermore, multiple dispersants synergistically participate in graft copolymerization, constructing a hydrogen-bonded interpenetrating polymer network, giving the adhesive coating both excellent bonding strength and toughness. This adhesive ensures the reliability of ceramic coating adhesion while maintaining good lithium-ion conductivity and preserving the excellent mechanical properties of the separator. It effectively alleviates coating peeling and cracking failures under high temperature and high voltage conditions, reduces the risk of micro-short circuits in the battery, and significantly improves the cycle stability and safety of lithium batteries, meeting the development needs of high energy density and long cycle life in lithium batteries. Detailed Implementation

[0018] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0019] This invention provides an aqueous adhesive comprising a composite dispersant, a hard monomer, a soft monomer, a functional monomer, an initiator, and water.

[0020] The composite dispersant is selected from at least two of polyvinyl alcohol and its derivatives, polyethylene glycol and its derivatives, polypropylene glycol and its derivatives, polyvinylpyrrolidone and its derivatives, and cellulose derivatives; the composite dispersant molecules are linked with monomer copolymer segments, which intertwine with the monomer copolymer segments to form an interpenetrating polymer network structure.

[0021] The mass ratio of the composite dispersant, hard monomer, soft monomer, functional monomer and initiator is 6-23:2-18:2-18:80-120:0.3-2.5.

[0022] When any one dispersant component is weighed as 1 part, the remaining dispersant components are each weighed independently as 0.01 to 1 part.

[0023] Through extensive experimentation, the inventors discovered that the combined use of multiple dispersants, on the one hand, suppresses viscosity abrupt changes caused by monomer polymerization due to steric hindrance, ensuring a stable and controllable solution polymerization process; on the other hand, the composite dispersant molecular chains are rich in active sites that can be hydrogen-absorbed, generating active free radicals under the action of initiators. This triggers graft copolymerization of soft and hard monomers with functional monomers, forming graft copolymers with the dispersant molecular chains as the main chain and acrylate copolymers as the side chains, constructing a second polymer network. Simultaneously, the hydroxyl groups carried by the dispersant can form numerous intermolecular hydrogen bonds with polar groups such as carboxyl and amide groups on the copolymer chains, constructing physical crosslinking points. These points interact with the first copolymer network formed by monomer copolymerization, ultimately forming a semi-interpenetrating or interpenetrating polymer network structure, significantly improving the overall network structure stability of the binder.

[0024] In some embodiments, the dispersant is selected from water-soluble polymers, wherein the polyvinyl alcohol derivative is preferably acetylated modified polyvinyl alcohol, cationic modified polyvinyl alcohol, or silane modified polyvinyl alcohol; the polyethylene glycol derivative is preferably methoxy-terminated polyethylene glycol; the polypropylene glycol derivative is preferably a polyoxyethylene-polyoxypropylene block copolymer; the polyvinylpyrrolidone derivative is preferably a vinylpyrrolidone-vinyl acetate copolymer; and the cellulose derivative is preferably hydroxypropyl methylcellulose, sodium carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, or methylcellulose.

[0025] In some embodiments, the hard monomer includes one or more of acrylonitrile, styrene, isobornyl methacrylate, vinyl acetate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, tetrahydrofurfuryl methacrylate, isobornyl acrylate, n-butyl methacrylate, and isobutyl methacrylate.

[0026] In some embodiments, the soft monomer is one or more of ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, isooctyl acrylate, hexyl methacrylate, ethylene tert-carbonate, tetrahydrofurfuryl acrylate, lauryl acrylate, lauryl methacrylate, isodecyl acrylate, or ethoxyethoxyethyl acrylate.

[0027] In some embodiments, the functional monomer includes one or more of carboxyl monomers, hydroxyl monomers, amide monomers, epoxy monomers, acetoacetate monomers, multifunctional crosslinking monomers, and diene monomers.

[0028] The carboxyl monomers include acrylic acid, methacrylic acid, and itaconic acid; the hydroxyl monomers include 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate, and 4-hydroxybutyl acrylate; the amide monomers include acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide; the epoxy monomers include glycidyl methacrylate; the acetoacetate monomers include ethyl acetoacetate methacrylate; the multifunctional crosslinking monomers include divinylbenzene, tripropylene glycol diacrylate, pentaerythritol triacrylate, and polyethylene glycol diacrylate; and the diene monomers include isoprene.

[0029] In a preferred embodiment, the functional monomer is a combination of carboxyl monomers and amide monomers, with the mass ratio of carboxyl monomers to amide monomers being 80:20 to 50:50 based on their total mass.

[0030] In this invention, hard monomers, soft monomers, and functional monomers copolymerize to form polymer chains. The functional monomers provide a large number of polar functional groups, constructing a hydrogen-bonded cross-linking network. Hard monomers regulate the rigidity of the coating film, while soft monomers improve the flexibility of the coating, preventing the film from becoming too brittle and cracking. This invention relies on in-situ grafting of a composite dispersant to form an interpenetrating network structure, combined with a high proportion of functional monomers to construct a high-density hydrogen-bonded network. Therefore, the amount of hard monomers can be reduced, with a small amount used to regulate the rigidity of the copolymer segments. This ensures high-temperature resistance and high adhesion performance while also maintaining the stability of the binder solution.

[0031] In some embodiments, the initiator is a water-soluble initiator, including one or more of ammonium persulfate, sodium persulfate, and potassium persulfate.

[0032] In a specific embodiment, the preparation method of the above-mentioned water-based adhesive includes the following steps:

[0033] By weight, 6-23 parts of composite dispersant, 0.1-1 parts of initiator and 300-500 parts of water are mixed in a reactor under mechanical stirring at 100-300 rpm to obtain a homogeneous solution. Nitrogen gas is continuously introduced to remove oxygen and ensure that the reaction system is in an oxygen-free environment. The composite dispersant is composed of at least two dispersant components. The system was then heated to 65–70°C, and a mixed monomer solution consisting of 2–18 parts hard monomer, 2–18 parts soft monomer, 80–120 parts functional monomer, and 0.2–1.5 parts initiator was added dropwise to the reaction system at a uniform rate. After the addition was completed, the polymerization reaction was maintained at this temperature for 1.5–4 hours. After polymerization, the temperature was raised to 75–80°C and maintained for 2–4 hours to fully eliminate residual monomers and improve the polymer network structure. Subsequently, the system was cooled to 40–45°C, and an alkaline solution was added to adjust the pH of the system to 8±1. The mixture was then filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms. This binder is an aqueous dispersion.

[0034] Preferably, the alkaline solution is one or more of sodium hydroxide, lithium hydroxide, potassium hydroxide, sodium bicarbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate solution.

[0035] Typically, the water mentioned above is deionized water.

[0036] This invention employs a pre-feeding polymerization system with a compound dispersant, enabling simultaneous stable and controllable polymerization and the construction of a high-performance network structure in an oxygen-free water environment. During the polymerization reaction, the water-soluble initiator generates a large number of aqueous primary free radicals upon heating. The compound dispersant is pre-dissolved completely in the aqueous phase, and its molecular chains are rich in highly active hydrogen sites. The aqueous primary free radicals preferentially capture active hydrogens from the dispersant molecular chains, forming stable macromolecular chain free radical active sites. The activated dispersant molecular chains can initiate the polymerization reaction of unsaturated monomers in situ, grow grafted branches, and construct a graft copolymer second network, which interpenetrates with the first network formed by the homopolymerization of monomers. Simultaneously, the intermolecular hydrogen bonds formed between polar groups within the system constitute physical cross-linking sites, ultimately constructing a dense and stable hydrogen-bonded reinforced interpenetrating polymer network.

[0037] In a specific embodiment, a lithium-ion battery separator is provided, the separator comprising a base film, one or both sides of which are coated with an aqueous binder; the aqueous binder is the aqueous binder of the present invention; specifically, the amount of aqueous binder coated on the base film can be 0.3 g / m³. 2 ~0.7g / m 2 This is to ensure that the prepared lithium-ion battery separator has better electrochemical performance.

[0038] In some embodiments, the membrane substrate may be a conventional membrane, including single-layer PP (polypropylene), single-layer PE (polyethylene), double-layer PP / PE, double-layer PP / PP, and triple-layer PP / PE / PP membranes.

[0039] In a specific embodiment, a lithium-ion battery is provided, the lithium-ion battery including a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator is the lithium-ion battery separator described above.

[0040] The method for preparing batteries using the separator provided by this invention can be a conventional method in the prior art, and will not be described in detail here.

[0041] The present invention is further described below through embodiments, but these embodiments are only for illustrating the present invention and not for limiting the present invention.

[0042] Example 1

[0043] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0044] Example 2

[0045] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyethylene glycol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0046] Example 3

[0047] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polypropylene glycol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0048] Example 4

[0049] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts hydroxypropyl methylcellulose, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0050] Example 5

[0051] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts of acetylated modified PVA, 6 parts of polyvinylpyrrolidone, 0.2 parts of ammonium persulfate, and 400 parts of deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts of acrylonitrile, 4 parts of n-butyl acrylate, 61.8 parts of acrylic acid, 41.2 parts of acrylamide, and 0.25 parts of ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0052] Example 6

[0053] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinylpyrrolidone, 6 parts polyethylene glycol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0054] Example 7

[0055] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinylpyrrolidone, 6 parts polypropylene glycol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0056] Example 8

[0057] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinylpyrrolidone, 6 parts hydroxyethyl cellulose, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0058] Example 9

[0059] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyethylene glycol, 6 parts polypropylene glycol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0060] Example 10

[0061] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyethylene glycol, 6 parts hydroxyethyl cellulose, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0062] Example 11

[0063] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 8 parts polyvinyl alcohol, 8 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0064] Example 12

[0065] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 13.2 parts polyvinyl alcohol, 2.8 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0066] Example 13

[0067] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 15.0 parts of polyvinyl alcohol, 1.0 parts of polyvinylpyrrolidone, 0.2 parts of ammonium persulfate, and 400 parts of deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts of acrylonitrile, 4 parts of n-butyl acrylate, 61.8 parts of acrylic acid, 41.2 parts of acrylamide, and 0.25 parts of ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0068] Example 14

[0069] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 103 parts acrylic acid, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was then filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0070] Example 15

[0071] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 103 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was then filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0072] Example 16

[0073] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 103 parts hydroxyethyl methacrylate, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0074] Example 17

[0075] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 103 parts tripropylene glycol diacrylate, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was then filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0076] Example 18

[0077] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts hydroxyethyl methacrylate, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0078] Example 19

[0079] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 82.4 parts acrylic acid, 20.6 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0080] Example 20

[0081] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 72.1 parts acrylic acid, 30.9 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0082] Example 21

[0083] This embodiment provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 10 parts polyvinyl alcohol, 6 parts polyvinylpyrrolidone, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 51.5 parts acrylic acid, 51.5 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0084] Comparative Example 1

[0085] This comparative example provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 0.2 parts ammonium persulfate and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0086] Comparative Example 2

[0087] This comparative example provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 16 parts polyvinyl alcohol, 0.2 parts ammonium persulfate, and 400 parts deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts acrylonitrile, 4 parts n-butyl acrylate, 61.8 parts acrylic acid, 41.2 parts acrylamide, and 0.25 parts ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0088] Comparative Example 3

[0089] This comparative example provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 16 parts of polyvinylpyrrolidone, 0.2 parts of ammonium persulfate, and 400 parts of deionized water were mixed in a reactor under mechanical stirring at 250 rpm to obtain a homogeneous solution, and nitrogen gas was continuously introduced to maintain an oxygen-free environment. The system was heated to 65°C, and a mixed solution prepared by 8 parts of acrylonitrile, 4 parts of n-butyl acrylate, 61.8 parts of acrylic acid, 41.2 parts of acrylamide, and 0.25 parts of ammonium persulfate was added dropwise to the reactor. The polymerization reaction was maintained at this temperature for 2 hours. The temperature was then raised to 80°C and maintained for 4 hours. Subsequently, the temperature was lowered to 40°C, and sodium hydroxide solution was added to adjust the pH to 8. The mixture was filtered to obtain the high-temperature resistant, high-adhesion waterborne binder for ceramic diaphragms.

[0090] Comparative Example 4

[0091] This comparative example provides an aqueous adhesive, the preparation method of which includes the following steps: By weight, 400 parts deionized water and 0.45 parts ammonium persulfate were added to a reactor and stirred until homogeneous. Then, a monomer mixture (60 parts acrylonitrile, 20 parts n-butyl acrylate, 20 parts acrylic acid, and 10 parts acrylamide) was added dropwise, stirred, and a protective atmosphere was introduced. Next, 10 parts polyvinyl alcohol and 6 parts polyvinylpyrrolidone were added, and the mixture was heated to 80°C and maintained at that temperature for 4 hours. After the reaction, the pH of the system was adjusted to 8, and the mixture was filtered to obtain the binder solution. This comparative example could not form a dispersant-grafted interpenetrating polymer network structure.

[0092] The diaphragm binders obtained in Examples 1-21 and Comparative Examples 1-4 were used to prepare ceramic slurries: 100g of boehmite ceramic powder was weighed, 120g of deionized water was added, and the mixture was stirred at 300rpm for 60min; then 20g of diaphragm binder (solid content of 20wt%) was added, and the mixture was stirred at 300rpm for 30min to obtain a uniform ceramic coating slurry.

[0093] The above-mentioned ceramic slurry was coated on both sides of the polyethylene membrane using a wire bar coater. After drying, a ceramic coating layer with a thickness of 1-2 μm was formed, and the corresponding modified composite membrane was obtained.

[0094] All performance tests were conducted in a constant temperature and humidity environment (temperature 23.0±2.0℃, relative humidity 50.0±10.0%).

[0095] 1. Initial 180° peel strength test

[0096] Cut the diaphragm into rectangular specimens with a width of 25.0 mm and a length of 150.0 mm. Using 25.0 μm thick acrylic double-sided adhesive, smoothly adhere the ceramic-coated surface of the diaphragm to the surface of a 304 stainless steel plate that has been wiped clean with acetone. Use a 2.0 kg standard pressure roller to roll back and forth three times at a speed of 300.0 mm / min, ensuring no air bubbles on the bonding surface. Mount the specimen onto a universal testing machine (range ≥ 500 N), set the peel angle to 180° and the tensile rate to 300.0 mm / min for testing. Collect the average peel force in the stable peel section of at least 100.0 mm, according to the formula:

[0097] Peel strength (N / m) = Average peel force (N) ÷ Specimen width (m)

[0098] Each sample was tested in parallel for 3 groups, and the average value was taken as the final peel strength.

[0099] 2. Peel retention rate after aging

[0100] Cut 25.0 mm × 150 mm samples from the prepared ceramic separator; immerse a portion of the sample completely in lithium battery electrolyte, seal and place in a 65℃ oven for 72 hours; remove the sample and wipe off the surface electrolyte with clean filter paper, then equilibrate for 30 minutes in an environment with a temperature of 23.0 ± 2.0℃ and a relative humidity of 50.0 ± 10.0%. Using the same sample preparation method and testing machine parameters as the initial peel strength, test the 180° peel strength after aging. The peel retention rate is calculated as follows: Peel retention rate (%) = Aging peel strength ÷ Initial peel strength × 100%; each group of samples was tested in triplicate, and the average value was taken.

[0101] 3. High-temperature heat shrinkage test

[0102] The diaphragm sample was cut into specimens of 100 mm (Transverse Direction, TD) × 80 mm (Machine Direction, MD). Using a vernier caliper with an accuracy of 0.02 mm, a line with a length of 80.0 mm was marked at the center of the specimen in both the MD and TD directions. The specimen was placed flat in a forced-air drying oven lined with a polytetrafluoroethylene pad and heat-treated at 150.0℃ for 60.0 min. After removal, it was placed in a standard testing environment to cool to room temperature, and the remaining length of the marked line segment was measured again.

[0103] Formulas for calculating longitudinal / transverse heat shrinkage rate:

[0104] In the formula: L0 is the length of the mark before heat treatment; L1 is the length of the mark after heat treatment; each group of samples is tested in parallel 3 times, and the arithmetic mean is taken.

[0105] 4. Air permeability test

[0106] Three parallel samples were cut at 150mm intervals along the longitudinal direction of the diaphragm. The air permeability of the diaphragm was measured using a Golley air permeability tester, and the air permeation time was recorded. The average value of the three test results was taken as the air permeability performance data of the diaphragm.

[0107] The membrane performance test results corresponding to Examples 1-21 and Comparative Examples 1-4 are shown in Table 1.

[0108] Table 1

[0109] Table 1 shows that the modified diaphragms prepared in the various embodiments of the present invention possess excellent adhesion stability, high-temperature dimensional stability, and uniform air permeability. Their performance balance is significantly superior to that of the comparative examples. This is primarily due to the dense and stable interpenetrating network structure synergistically constructed by the combination of multiple dispersants and monomer polymerization. The combination of multiple dispersants exhibits a significant synergistic effect, endowing the modified diaphragms of the present invention with excellent comprehensive performance. It can stably control the high-temperature thermal shrinkage rate of the coating within 3%, effectively enhancing the overall heat resistance and confinement capacity of the coating and the diaphragm substrate, significantly improving the high-temperature dimensional stability of the diaphragm. Furthermore, the dense and regular network structure does not block the diaphragm pores and has no significant negative impact on the diaphragm's permeability, thus maintaining the diaphragm's excellent and uniform air permeability characteristics for a long time.

[0110] It should be noted that, based on the explanations and descriptions in the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some equivalent modifications and alterations to the present invention should also be within the scope of protection of the claims of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the invention.

Claims

1. A water-based adhesive, characterized in that, It includes composite dispersants, hard monomers, soft monomers, functional monomers, initiators, and water; The composite dispersant is selected from at least two of polyvinyl alcohol and its derivatives, polyethylene glycol and its derivatives, polypropylene glycol and its derivatives, polyvinylpyrrolidone and its derivatives, and cellulose derivatives. The composite dispersant molecules have monomer copolymer segments linked together, which intertwine with the monomer copolymer segments to form an interpenetrating polymer network structure.

2. The water-based adhesive according to claim 1, characterized in that, The mass ratio of the composite dispersant, hard monomer, soft monomer, functional monomer and initiator is 6-23:2-18:2-18:80-120:0.3-2.

5.

3. The water-based adhesive according to claim 1, characterized in that, The composite dispersant is selected from a combination of polyvinyl alcohol and its derivatives and polyvinylpyrrolidone and its derivatives.

4. The water-based adhesive according to claim 3, characterized in that, The mass ratio of polyvinyl alcohol and its derivatives to polyvinylpyrrolidone and its derivatives is 1:0.01 to 1:1, preferably 1:0.2 to 1:0.

6.

5. The water-based adhesive according to claim 1, characterized in that, The functional monomers are selected from a combination of carboxyl monomers and amide monomers.

6. The water-based adhesive according to claim 5, characterized in that, Based on the total mass of both, the mass ratio of the carboxyl monomer to the amide monomer is 80:20 to 50:50, preferably 70:30 to 60:

40.

7. The water-based adhesive according to claim 5, characterized in that, The carboxyl monomer is selected from at least one of acrylic acid, methacrylic acid, and itaconic acid; the amide monomer is selected from at least one of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide.

8. A method for preparing a water-based adhesive, characterized in that, Includes the following steps: By weight, 6-23 parts of composite dispersant, 0.1-1 parts of initiator and 300-500 parts of water are mixed in a reactor under mechanical stirring at 100-300 rpm to obtain a homogeneous solution. Nitrogen gas is continuously introduced to remove oxygen and ensure that the reaction system is in an oxygen-free environment. The composite dispersant is composed of at least two dispersant components. The system was then heated to 65–70°C, and a mixed monomer solution consisting of 2–18 parts hard monomer, 2–18 parts soft monomer, 80–120 parts functional monomer, and 0.2–1.5 parts initiator was added dropwise to the reaction system at a uniform rate. After the addition was completed, the polymerization reaction was maintained at this temperature for 1.5–4 hours. After polymerization, the temperature was raised to 75–80°C and maintained for 2–4 hours. The system was then cooled to 40–45°C, the pH was adjusted to 8±1, and the mixture was filtered to obtain an aqueous binder.

9. A lithium-ion battery separator, characterized in that, The lithium-ion battery separator comprises the aqueous binder as described in any one of claims 1-7 or the aqueous binder prepared by the preparation method as described in claim 8.

10. A lithium-ion battery, characterized in that, The lithium-ion battery includes the lithium-ion battery separator as described in claim 9.