A biochar material and its preparation method
By synthesizing a porous carbon layer on the surface of silicon nitride fine powder and using a combination of aluminosilicate, gel matrix and carboxymethyl cellulose, the problem of ash accumulation and slag formation during the combustion of bamboo chip-based biochar materials was solved, improving combustion thermal efficiency and fixing carbon content, and achieving stable combustion.
Patent Information
- Application Number
- CN202611548652.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
Bamboo-based biochar materials are prone to ash accumulation and slag formation during combustion, resulting in low combustion thermal efficiency and hindering their further development.
By synthesizing a porous carbon layer on the surface of silicon nitride fine powder and utilizing the three-dimensional network structure formed by aluminosilicate and gel matrix, combined with carboxymethyl cellulose as a binder, biochar materials were prepared, which improved their thermal conductivity and fixed carbon content, reduced oxygen diffusion rate, and increased ash melting temperature.
It significantly improves the combustion thermal efficiency and fixed carbon content of biochar materials, ensures continuous and stable combustion, avoids melting and sticking and slagging in the furnace, and achieves high-efficiency combustion.
Abstract
Description
Technical Field
[0001] This invention relates to the field of biochar fuel technology, specifically to a biochar material and its preparation method. Background Technology
[0002] Bamboo chips are a new type of energy-saving and environmentally friendly material made from bamboo processing waste. They belong to the category of filler additives, and their dry matter contains higher levels of cellulose, hemicellulose, and lignin than traditional hardwood chips. About 30% of the waste from bamboo processing can be converted into bamboo chips, which can be processed into fuel pellets, bamboo powder, and other products. Bamboo chip biochar materials have been widely used in various industries as a new commercial energy source. They have high density, high calorific value, regular shape, and good fluidity, which facilitates automatic combustion control and can save enterprises a lot of energy costs.
[0003] Biochar materials are made from bamboo processing waste as raw materials. After medium- and low-temperature carbonization, the material is ground into powder, extruded with a molding agent, and then dried and carbonized again. Compared with other biochar materials, it has the advantages of high bulk density, high calorific value, safer storage, and more complete combustion. Compared with coal and other fossil fuels, it has multiple advantages: carbon reduction and environmental protection: the carbon dioxide produced by biochar combustion can be reabsorbed by plant growth; reduced pollutants: replacing coal can effectively reduce the emission of sulfur dioxide and nitrogen oxides; renewable resources: coal is a finite fossil fuel, while biochar is a renewable resource with wide availability and greater sustainability; improved combustion performance: co-firing biochar with coal can improve overall combustion efficiency, making the fuel easier to ignite and burn more completely. It is widely used in industrial settings such as steel smelting, copper smelting, and cement kilns, using biochar materials as fuel to partially replace fossil fuels and develop renewable low-carbon biochar fuels.
[0004] Bamboo-based biochar materials are prone to ash accumulation and slag formation during combustion, which hinders the combustion process and results in low combustion thermal efficiency. This drawback seriously restricts the further development and utilization of bamboo-based biochar materials as fuel.
[0005] There is an urgent need to develop a biomass char industrial fuel that uses bamboo processing waste as raw material and has high fixed carbon, high calorific value, high bulk density, and high combustion thermal efficiency. Summary of the Invention
[0006] This invention provides a biochar material and its preparation method, which solves the problem that bamboo-based biochar materials are prone to ash accumulation and slag formation during combustion, which hinders the combustion process and leads to low combustion thermal efficiency.
[0007] The technical solution of the present invention: A method for preparing biochar material includes the following steps: S1. After removing sand and impurities from bamboo shavings and drying them, the bamboo shavings are carbonized once to obtain carbonized bamboo shavings; the carbonized bamboo shavings are then crushed to obtain carbonized bamboo shaving powder. S2. Mix the bamboo shavings powder that has been carbonized once, the forming agent and the sintering aid, extrude and form, then dry and carbonize again, cool to room temperature, grind and sieve to obtain biochar material; The sintering aid is obtained by mixing and reacting composite fine powder, polyvinyl alcohol and chitosan; The composite fine powder is obtained by synthesizing a porous carbon layer on the surface of silicon nitride fine powder, and then loading aluminosilicate with carboxymethyl cellulose.
[0008] Further, in step S1, the drying specifically involves drying at 100-110°C until the moisture content of the bamboo chips is 6-10%.
[0009] Further, in step S1, the primary carbonization specifically involves: heating to 200-300℃ at 3-5℃ / min and holding for 2-3 hours, then heating to 400-450℃ at 4-6℃ / min and holding for 1-2 hours.
[0010] Furthermore, in step S1, the bamboo shavings that have undergone primary carbonization are crushed to 3-5 mm.
[0011] Further, in step S2, the mass ratio of the primary carbonized bamboo shavings powder, forming agent, and sintering aid is 100:(3-5):(1-2).
[0012] Further, in step S2, the extrusion molding specifically involves: stirring at 800-1000 r / min for 8-12 min, followed by extrusion molding at 20-25 MPa and 80-100℃ for 1-2 min.
[0013] Further, in step S2, the drying process specifically involves drying at 90-110℃ for 5-10 minutes.
[0014] Further, in step S2, the secondary carbonization specifically involves heating to 800-900℃ at a rate of 4-6℃ / min and performing secondary carbonization for 1-2 hours.
[0015] Furthermore, in step S2, the mesh size of the grinding and sieving screen is 100-200 mesh.
[0016] Furthermore, in step S2, the molding agent is a water-soluble phenolic resin.
[0017] Furthermore, the sintering aid is specifically prepared by the following steps: A1. Place silicon nitride fine powder in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, remove it and dry it until the water evaporates. Place it in a tube furnace, introduce nitrogen gas, and carbonize it at 700-800℃ for 3-4 hours. Remove it, cool it to room temperature, wash it, and dry it until the water evaporates to obtain porous carbon-coated silicon nitride fine powder. A2. Mix porous carbon-coated silicon nitride fine powder and carboxymethyl cellulose solution, stir at 30-50℃ and 80-100r / min for 20-30min, add aluminosilicate, continue stirring for 20-30min, filter, and dry until the water evaporates to obtain composite fine powder; A3. Dissolve chitosan and polyvinyl alcohol in an aqueous acetic acid solution, stir at 95-100℃ and 200-220r / min until completely dissolved, cool to room temperature, add glutaraldehyde and composite fine powder, stir at 1000-1500r / min for 5-10min, wash and dry to obtain sintering aid.
[0018] Furthermore, in the A1 reaction process described above, glucose and potassium hydroxide solution are mixed to form a mixed solution. Silicon nitride fine powder is impregnated into the mixed solution, so that glucose and activator potassium hydroxide are coated and adsorbed on the surface of silicon nitride fine powder. After sintering and carbonization, glucose is decomposed by heat to form a carbon layer. Potassium hydroxide, as an activator, is decomposed by heat and overflows in the form of gas, leaving pores on the surface of the carbon layer, thereby forming channels on the surface of the carbon layer. This achieves the synthesis of a porous carbon layer on the surface of silicon nitride fine powder, resulting in porous carbon layer coated silicon nitride fine powder.
[0019] Furthermore, during the A2 reaction process described above, carboxymethyl cellulose is adsorbed onto the surface of the porous carbon layer-coated silicon nitride fine powder, imparting excellent adhesion properties, thereby enabling aluminosilicate to be loaded onto the surface of the porous carbon layer-coated silicon nitride fine powder, resulting in composite fine powder.
[0020] Furthermore, in the A3 reaction process described above, polyvinyl alcohol and chitosan serve as gel matrices, and the composite fine powder is added to the gel matrix to achieve the embedding of the composite fine powder into the gel matrix, thereby obtaining a sintering aid.
[0021] Further, in step A1, the mass ratio of the silicon nitride fine powder, glucose, potassium hydroxide and deionized water is (2-2.5):(1-1.2):(1.2-1.5):(50-60).
[0022] Further, in step A2, the mass ratio of the porous carbon layer coated silicon nitride fine powder, aluminosilicate and carboxymethyl cellulose solution is (2-2.3):(0.3-0.5):100.
[0023] Further, in step A3, the mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde and composite fine powder is (3.8-4):(3.8-4):(90-100):(0.01-0.02):(2-2.3).
[0024] The present invention has the following beneficial effects: (1) In the technical solution of the present invention, a porous carbon layer is synthesized on the surface of silicon nitride fine powder. On the one hand, silicon nitride fine powder has high thermal conductivity and high temperature resistance. When added to biochar material, silicon nitride constructs a three-dimensional thermally conductive network, which accelerates the heat transfer of the green body and conducts the heat of the combustion zone to the interior of the biochar material. The biochar material quickly reaches the ignition temperature and the combustion is continuous and stable, thereby improving the combustion thermal efficiency of the biochar material. On the other hand, the porous carbon layer synthesized on the surface of silicon nitride fine powder can capture the gaseous state generated during the secondary carbonization of bamboo shavings. Tar and hydrocarbon volatiles are retained inside the porous carbon pores and undergo high-temperature pyrolysis to transform into solid fixed carbon. This recovers carbon elements that would otherwise escape and increases the fixed carbon content of biochar materials, thereby improving their combustion efficiency. Furthermore, the porous carbon layer contains tortuous and interwoven microporous channels, which can extend the oxygen diffusion path. During the secondary carbonization process, bamboo powder can reduce the oxygen diffusion rate, reduce the formation of silicon dioxide oxide film on the silicon nitride surface, maintain thermal conductivity, and improve the combustion thermal efficiency of biochar materials.
[0025] (2) In the technical solution of the present invention, aluminosilicate is loaded onto the porous carbon layer coated with silicon nitride fine powder by carboxymethyl cellulose. On the one hand, during the combustion process of biomass char material, aluminosilicate can react with the low melting point free alkali metal salt contained in the biomass char material to form aluminosilicate with a higher melting point, which increases the melting temperature of ash and keeps the ash in a loose powder form after combustion, avoiding melting adhesion, covering of carbon particles, and slagging in the furnace, which affects the combustion thermal efficiency of biomass char material. On the other hand, carboxymethyl cellulose, as a binder, can load active aluminosilicate onto the surface of porous carbon layer coated with silicon nitride fine powder, avoiding the agglomeration and precipitation of active aluminosilicate. In addition, during the secondary carbonization process of bamboo chip powder, carboxymethyl cellulose is decomposed by heat and volatilized in gaseous form, generating mesoporous channels in situ, increasing the reaction sites of active aluminosilicate and low melting point free alkali metal salt, increasing the melting temperature of ash and improving the combustion thermal efficiency of biomass char material.
[0026] (3) In the technical solution of the present invention, polyvinyl alcohol and chitosan are used as gel matrix, and composite fine powder is embedded in the gel matrix. On the one hand, the gel formed by polyvinyl alcohol and chitosan has a three-dimensional network structure, which can be uniformly dispersed in the biochar material. During the secondary carbonization process of bamboo powder, the three-dimensional network structure of the gel carbonizes to form a porous carbon network, which works with the porous carbon layer to capture the gaseous tar and hydrocarbon small molecule volatiles generated during the secondary carbonization of bamboo powder, recover the carbon elements that would otherwise escape and lose, and improve the fixed carbon content of the biochar material. On the other hand, the porous carbon network formed by gel carbonization can accelerate oxygen transport, promote the complete combustion of biochar material, and improve the combustion thermal efficiency of biochar material. In addition, the composite fine powder with high thermal conductivity is embedded in the three-dimensional network structure of the gel system, which makes the gel have high thermal conductivity, thereby accelerating the heat transfer of the green body and transferring the heat of the combustion zone to the interior of the biochar material. The biochar material quickly reaches the ignition temperature and the combustion is continuous and stable, thereby improving the combustion thermal efficiency of the biochar material.
[0027] (4) In the technical solution of the present invention, bamboo shavings are removed from sand and gravel, dried, and then carbonized once to obtain primary carbonized bamboo shavings; the primary carbonized bamboo shavings are crushed to obtain primary carbonized bamboo shaving powder; the primary carbonized bamboo shaving powder, molding agent and sintering aid are mixed, extruded and shaped, then dried, carbonized a second time, cooled to room temperature, ground and sieved to obtain biochar material with high combustion efficiency. Detailed Implementation
[0028] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0029] The raw materials used in the embodiments of this invention are shown below, and all reagents used are analytical grade.
[0030] The molding agent is water-soluble phenolic resin, product number P875865, with a solid content of 70%; silicon nitride fine powder, product number S817703, with a particle size of 1-3μm; sodium carboxymethyl cellulose, product number C6332; chitosan, product number C660110, with a degree of deacetylation ≥85%; polyvinyl alcohol, product number 767382, and Mw9000-10000 were purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0031] Aluminosilicate: An aluminosilicate with a silicon to aluminum molar ratio of 1:1, with a density of 3.247 g / cm³. 3 Melting point 1545℃.
[0032] The bamboo shavings are from moso bamboo, with a particle size of 20-40 mesh.
[0033] Example 1: A method for preparing biochar material, comprising the following steps: S1. Remove sand and impurities from bamboo shavings, dry them at 100-110℃ until the moisture content of the bamboo shavings is 6%, raise the temperature to 200℃ at 3℃ / min and keep it at that temperature for 2 hours, raise the temperature to 400℃ at 4℃ / min and keep it at that temperature for 1 hour to obtain primary carbonized bamboo shavings; crush the primary carbonized bamboo shavings to 3-5mm to obtain primary carbonized bamboo shavings powder. S2. Mix the primary carbonized bamboo shavings powder, water-soluble phenolic resin and sintering aid in a mass ratio of 100:3:1, stir at 800 r / min for 8 min, extrude at 20 MPa and 80℃ for 1 min, dry at 90℃ for 5 min, heat to 800-900℃ at 4℃ / min for secondary carbonization for 1 h, cool to room temperature, and grind through a 100-mesh sieve to obtain biochar material. The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide, and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. Then, it was placed in a tube furnace, nitrogen gas was introduced, and it was carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide, and deionized water was 2:1:1.2:50. A2. Porous carbon-coated silicon nitride fine powder and a 1% carboxymethyl cellulose solution were mixed and stirred at 30℃ and 80r / min for 20min. Aluminosilicate was added and stirring was continued for 20min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain composite fine powder. The mass ratio of porous carbon-coated silicon nitride fine powder, aluminosilicate, and carboxymethyl cellulose solution was 2:0.3:100. A3. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 95°C and 200 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1000 r / min for 5 min. After washing three times with deionized water, the mixture was dried in an oven at 80°C for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 3.8:3.8:90:0.01:2.
[0034] Example 2, a method for preparing biochar material, comprising the following steps: S1. Remove sand and gravel impurities from bamboo shavings, dry them at 100-110℃ until the moisture content of the bamboo shavings is 8%, raise the temperature to 250℃ at 4℃ / min and hold for 2.5h, raise the temperature to 430℃ at 5℃ / min and hold for 1.5h to obtain primary carbonized bamboo shavings; crush the primary carbonized bamboo shavings to 4mm to obtain primary carbonized bamboo shaving powder. S2. The primary carbonized bamboo shavings powder, water-soluble phenolic resin and sintering aid are mixed in a mass ratio of 100:4:1.5, stirred at 900 r / min for 10 min, extruded at 23 MPa and 90℃ for 1.5 min, dried at 100℃ for 8 min, heated to 850℃ at 5℃ / min for secondary carbonization for 1.5 h, cooled to room temperature, and ground through a 150 mesh sieve to obtain biochar material. The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide, and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. It was then placed in a tube furnace, nitrogen gas was introduced, and carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide, and deionized water was 2.3:1.1:1.3:55. A2. Porous carbon-coated silicon nitride fine powder and a 1% (w / w) carboxymethyl cellulose solution were mixed and stirred at 40℃ and 90 r / min for 25 min. Aluminosilicate was added, and stirring was continued for another 25 min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain composite fine powder. The mass ratio of porous carbon-coated silicon nitride fine powder, aluminosilicate, and carboxymethyl cellulose solution was 2.2:0.3:100. A3. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 98℃ and 210 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1300 r / min for 8 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain the sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 3.9:3.9:95:0.015:2.2.
[0035] Example 3, a method for preparing biochar material, comprising the following steps: S1. Remove sand and gravel impurities from bamboo shavings, dry them at 110℃ until the moisture content of the bamboo shavings is 10%, raise the temperature to 300℃ at 5℃ / min and keep it at that temperature for 3 hours, raise the temperature to 450℃ at 6℃ / min and keep it at that temperature for 2 hours to obtain primary carbonized bamboo shavings; crush the primary carbonized bamboo shavings to 5mm to obtain primary carbonized bamboo shavings powder. S2. The primary carbonized bamboo shavings powder, water-soluble phenolic resin and sintering aid are mixed in a mass ratio of 100:5:2, stirred at 1000 r / min for 12 min, extruded at 25 MPa and 100℃ for 2 min, dried at 110℃ for 10 min, heated to 900℃ at 6℃ / min for secondary carbonization for 2 h, cooled to room temperature, and ground through a 200 mesh sieve to obtain biochar material. The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. It was then placed in a tube furnace, nitrogen gas was introduced, and it was carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide and deionized water was 2.5:1.2:1.5:60. A2. Porous carbon-coated silicon nitride fine powder and a 1% (w / w) carboxymethyl cellulose solution were mixed and stirred at 50℃ and 100 r / min for 30 min. Aluminosilicate was added, and stirring was continued for another 30 min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain composite fine powder. The mass ratio of porous carbon-coated silicon nitride fine powder, aluminosilicate, and carboxymethyl cellulose solution was 2.3:0.5:100. A3. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 100℃ and 220 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1500 r / min for 10 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 4:4:100:0.02:2.3.
[0036] Comparative Example 1 The only difference between this comparative example and Example 3 is the preparation of the sintering aid, as detailed below: The sintering aid is prepared by the following steps: A1. Porous carbon-coated silicon nitride fine powder and a 1% (w / w) carboxymethyl cellulose solution were mixed and stirred at 50℃ and 100 r / min for 30 min. Aluminosilicate was added, and stirring was continued for another 30 min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain composite fine powder. The mass ratio of silicon nitride fine powder, aluminosilicate, and carboxymethyl cellulose solution was 2.3:0.5:100. A2. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 100℃ and 220 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1500 r / min for 10 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 4:4:100:0.02:2.3.
[0037] Comparative Example 2 The only difference between this comparative example and Example 3 is the preparation of the sintering aid, as detailed below: The sintering aid is prepared by the following steps: A1. Porous carbon powder (pore size 150nm, product number P698902, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.) and a 1% carboxymethyl cellulose solution were mixed and stirred at 50℃ and 100r / min for 30min. Aluminosilicate was added, and stirring was continued for 30min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain a composite fine powder. The mass ratio of porous carbon powder, aluminosilicate, and carboxymethyl cellulose solution was 2.3:0.5:100. A2. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 100℃ and 220 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1500 r / min for 10 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 4:4:100:0.02:2.3.
[0038] Comparative Example 3 The only difference between this comparative example and Example 3 is the preparation of the sintering aid, as detailed below: The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. It was then placed in a tube furnace, nitrogen gas was introduced, and it was carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide and deionized water was 2.5:1.2:1.5:60. A2. Porous carbon-coated silicon nitride fine powder and deionized water are mixed and stirred at 50℃ and 100r / min for 30min. Aluminosilicate is added and stirring is continued for 30min. After filtration, the mixture is dried in an oven at 100℃ until the water evaporates to obtain composite fine powder. The mass ratio of porous carbon-coated silicon nitride fine powder, aluminosilicate and deionized water is 2.3:0.5:100. A3. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 100℃ and 220 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1500 r / min for 10 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 4:4:100:0.02:2.3.
[0039] Comparative Example 4 The only difference between this comparative example and Example 3 is the preparation of the sintering aid, as detailed below: The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. It was then placed in a tube furnace, nitrogen gas was introduced, and it was carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide and deionized water was 2.5:1.2:1.5:60. A2. Porous carbon-coated silicon nitride fine powder and a 1% carboxymethyl cellulose solution were mixed and stirred at 50℃ and 100r / min for 30min. After filtration, the mixture was dried in an oven at 100℃ until the moisture evaporated to obtain composite fine powder. The mass ratio of porous carbon-coated silicon nitride fine powder to carboxymethyl cellulose solution was 2.3:100. A3. Chitosan and polyvinyl alcohol were dissolved in a 3% (w / w) aqueous acetic acid solution and stirred at 100℃ and 220 r / min until completely dissolved. After cooling to room temperature, glutaraldehyde and composite fine powder were added, and the mixture was stirred at 1500 r / min for 10 min. After washing three times with deionized water, the mixture was dried in an oven at 80℃ for 1 h to obtain a sintering aid. The mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde, and composite fine powder was 4:4:100:0.02:2.3.
[0040] Comparative Example 5 The only difference between this comparative example and Example 3 is the preparation of the sintering aid, as detailed below: The sintering aid is prepared by the following steps: A1. Silicon nitride fine powder was placed in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, it was removed and dried in an oven at 100°C until the moisture evaporated. It was then placed in a tube furnace, nitrogen gas was introduced, and it was carbonized at 700°C for 3 hours. After removal, it was cooled to room temperature, washed three times with deionized water, and dried in an oven at 100°C until the moisture evaporated to obtain porous carbon-coated silicon nitride fine powder. The mass ratio of silicon nitride fine powder, glucose, potassium hydroxide and deionized water was 2.5:1.2:1.5:60. A2. Mix porous carbon-coated silicon nitride fine powder with a 1% carboxymethyl cellulose solution, stir at 50℃ and 100r / min for 30min, add aluminosilicate, continue stirring for 30min, filter, and dry in an oven at 100℃ until the moisture evaporates to obtain composite fine powder, i.e., sintering aid; the mass ratio of porous carbon-coated silicon nitride fine powder, aluminosilicate, and carboxymethyl cellulose solution is 2.3:0.5:100.
[0041] The performance of the biochar materials prepared in Examples 1-3 and Comparative Examples 1-5 was then tested.
[0042] The fixed carbon content of the biochar materials prepared above was tested using a muffle furnace (Shanghai Kailang Instrument Equipment Factory, SX2-4-10) and a drying oven (Wujiang Minxin Drying Oven and Electric Furnace Manufacturing Co., Ltd., MX841-6). The higher calorific value was determined using an oxygen bomb calorimeter in accordance with the standard GB / T30727-2014 "Determination of Calorific Value of Solid Biomass Fuels".
[0043] As shown in Table 1 below.
[0044] Table 1 Performance testing of biochar materials prepared in Examples 1-3 and Comparative Examples 1-5 project Fixed carbon content / % Caloric value (kcal / kg) Example 1 85.8 6562 Example 2 88.4 6582 Example 3 84.2 6560 Comparative Example 1 65.7 5845 Comparative Example 2 69.3 6021 Comparative Example 3 62.3 5961 Comparative Example 4 58.1 5262 Comparative Example 5 60.5 5453 As can be seen from the data in Table 1, the biochar materials prepared in Examples 1-3 have high combustion efficiency, high calorific value and fixed carbon content.
[0045] Comparative Example 1 showed that replacing the porous carbon layer-coated silicon nitride fine powder with a sintering aid prepared from silicon nitride fine powder resulted in a decrease in the performance of biochar materials. This demonstrates that the porous carbon layer synthesized on the surface of silicon nitride fine powder can capture gaseous tar and hydrocarbon volatiles generated during the secondary carbonization of bamboo shavings. The volatiles remain inside the pores of the porous carbon and undergo high-temperature pyrolysis to transform into solid fixed carbon, recovering the carbon elements that would otherwise escape and increasing the fixed carbon content of the biochar material, thereby improving the combustion efficiency of the biochar material. Furthermore, the porous carbon layer contains tortuous and interwoven microporous channels, which can extend the oxygen diffusion path. During the secondary carbonization process of bamboo shavings, it can reduce the oxygen diffusion rate, reduce the formation of silicon dioxide oxide film on the silicon nitride surface, maintain thermal conductivity, and improve the combustion thermal efficiency of the biochar material.
[0046] Comparative Example 2 showed that replacing porous carbon-coated silicon nitride fine powder with sintering aids prepared from porous carbon powder resulted in a decrease in the performance of biochar materials. This demonstrated that silicon nitride fine powder has high thermal conductivity and high temperature resistance. When added to biochar materials, silicon nitride constructs a three-dimensional thermally conductive network, accelerating heat transfer in the green body and conducting heat from the combustion zone to the interior of the biochar materials. The biochar materials quickly reach the ignition temperature, and combustion is continuous and stable, thereby improving the combustion thermal efficiency of the biochar materials.
[0047] Comparative Example 3, which used sintering aids without the addition of carboxymethyl cellulose to prepare biochar materials, showed a decline in performance. This demonstrates that carboxymethyl cellulose, as a binder, can load active aluminosilicates onto the porous carbon layer coating the surface of silicon nitride fine powder, preventing the agglomeration and precipitation of active aluminosilicates. Furthermore, during the secondary carbonization process of bamboo shavings, carboxymethyl cellulose decomposes upon heating and volatilizes in gaseous form, generating mesoporous channels in situ. This increases the reactive sites for the interaction between active aluminosilicates and low-melting-point free alkali metal salts, thereby increasing the melting temperature of ash slag and improving the combustion thermal efficiency of biochar materials.
[0048] Comparative Example 4, which used sintering aids prepared without aluminosilicates to prepare biochar materials, showed a decline in performance. This demonstrates that during the combustion process, aluminosilicates can react with low-melting-point free alkali metal salts contained within the biochar material to form aluminosilicates with higher melting points. This increases the melting temperature of the ash, allowing the ash to maintain a loose powder morphology after combustion. This prevents melting and adhesion, encapsulation of carbon particles, and slagging in the furnace, which would affect the combustion thermal efficiency of the biochar material.
[0049] Comparative Example 5: The sintering aid prepared by embedding composite fine powder into the gel matrix was used to prepare biochar materials. Its performance decreased, proving that the gel with a three-dimensional network structure formed by polyvinyl alcohol and chitosan can be uniformly dispersed in the biochar materials. During the secondary carbonization process of bamboo shavings, the three-dimensional network structure of the gel carbonizes to form a porous carbon network. This porous carbon layer works together to capture the gaseous tar and hydrocarbon volatiles generated during the secondary carbonization of bamboo shavings, recovering the carbon elements that would otherwise escape and increasing the fixed carbon content of the biochar materials. Furthermore, the porous carbon network formed by gel carbonization can accelerate oxygen transport, promote complete combustion of biochar materials, and improve the combustion thermal efficiency of biochar materials.
[0050] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0051] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. A method for preparing biochar material, characterized in that, Includes the following steps: S1. After removing sand and gravel impurities from bamboo shavings and drying them, the bamboo shavings are carbonized once to obtain carbonized bamboo shavings; the carbonized bamboo shavings are then crushed to obtain carbonized bamboo shaving powder. S2. Mix the bamboo shavings powder that has been carbonized once, the forming agent and the sintering aid, extrude and form, then dry and carbonize again, cool to room temperature, grind and sieve to obtain biochar material; The sintering aid is obtained by mixing and reacting composite fine powder, polyvinyl alcohol and chitosan; The composite fine powder is obtained by synthesizing a porous carbon layer on the surface of silicon nitride fine powder, and then loading aluminosilicate with carboxymethyl cellulose.
2. The method for preparing biochar material according to claim 1, characterized in that, The sintering aid is prepared by the following steps: A1. Place silicon nitride fine powder in a mixture of glucose, potassium hydroxide and deionized water. After impregnation, remove it and dry it until the water evaporates. Place it in a tube furnace, introduce nitrogen gas, and carbonize it at 700-800℃ for 3-4 hours. Remove it, cool it to room temperature, wash it, and dry it until the water evaporates to obtain porous carbon-coated silicon nitride fine powder. A2. Mix porous carbon-coated silicon nitride fine powder and carboxymethyl cellulose solution, stir at 30-50℃ and 80-100r / min for 20-30min, add aluminosilicate, continue stirring for 20-30min, filter, and dry until the water evaporates to obtain composite fine powder; A3. Dissolve chitosan and polyvinyl alcohol in an aqueous acetic acid solution, stir at 95-100℃ and 200-220r / min until completely dissolved, cool to room temperature, add glutaraldehyde and composite fine powder, stir at 1000-1500r / min for 5-10min, wash and dry to obtain sintering aid.
3. The method for preparing biochar material according to claim 2, characterized in that, In step A1, the mass ratio of the silicon nitride fine powder, glucose, potassium hydroxide and deionized water is (2-2.5):(1-1.2):(1.2-1.5):(50-60).
4. The method for preparing biochar material according to claim 2, characterized in that, In step A2, the mass ratio of the porous carbon layer coated silicon nitride fine powder, aluminosilicate and carboxymethyl cellulose solution is (2-2.3):(0.3-0.5):
100.
5. The method for preparing biochar material according to claim 2, characterized in that, In step A3, the mass ratio of chitosan, polyvinyl alcohol, aqueous acetic acid solution, glutaraldehyde and composite fine powder is (3.8-4):(3.8-4):(90-100):(0.01-0.02):(2-2.3).
6. The method for preparing biochar material according to claim 1, characterized in that, In step S1, the primary carbonization specifically involves: heating to 200-300℃ at 3-5℃ / min and holding for 2-3 hours, then heating to 400-450℃ at 4-6℃ / min and holding for 1-2 hours.
7. The method for preparing biochar material according to claim 1, characterized in that, In step S1, the drying process specifically involves drying at 100-110℃ until the moisture content of the bamboo chips is 6-10%. In step S1, the bamboo shavings that have undergone primary carbonization are crushed to 3-5 mm.
8. The method for preparing biochar material according to claim 1, characterized in that, In step S2, the mass ratio of the primary carbonized bamboo shavings powder, forming agent, and sintering aid is 100:(3-5):(1-2); In step S2, the extrusion molding specifically involves: stirring at 800-1000 r / min for 8-12 min, followed by extrusion molding at 20-25 MPa and 80-100℃ for 1-2 min.
9. The method for preparing biochar material according to claim 1, characterized in that, In step S2, the drying process specifically involves drying at 90-110℃ for 5-10 minutes. In step S2, the secondary carbonization specifically involves heating to 800-900℃ at a rate of 4-6℃ / min and carbonizing for 1-2 hours. In step S2, the mesh size of the grinding and sieving screen is 100-200 mesh.
10. A biochar material prepared by the method of any one of claims 1-9.