A modified graphene lubricating oil additive and its preparation method

By introducing a hydrophobic polymer with a rigid twisted structure onto the surface of graphene, the problem of graphene's easy agglomeration in lubricating oil is solved, achieving long-term stable dispersion and friction-reducing and anti-wear effects of modified graphene, making it suitable for lubricating oil additives.

CN123107745APending Publication Date: 2026-11-17LIAONING QIZHONG LUBRICATING OIL MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611310240.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Graphene tends to agglomerate and has poor dispersion stability in lubricating oil. Existing modification methods have the risk of desorption or complex reactions, making it difficult to maintain a nanoscale dispersion in lubricating oil for a long time.

Method used

A tetrahydroxy aromatic monomer containing a spirocyclic structure and a tetrahalogenated terephthalonitrile are reacted with graphene oxide in a polar aprotic organic solvent to generate rigid twisted polymer chains through in-situ polycondensation. These chains are covalently bonded to the graphene surface to form a steric hindrance layer, thereby improving dispersibility.

Benefits of technology

This method enables graphene to be monodispersed or few-layered in lubricating oil for extended periods, reducing the coefficient of friction and wear. Furthermore, the polymer chain exhibits good stability, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107745A_ABST
    Figure CN123107745A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lubricant additive technology, specifically to a modified graphene lubricant additive and its preparation method. The method includes: S1: Weighing a measured amount of a tetrahydroxy aromatic monomer containing a spirocyclic structure, a tetrahalophthalonitrile, and a polar aprotic organic solvent; S2: Dissolving the tetrahydroxy aromatic monomer containing a spirocyclic structure and the tetrahalophthalonitrile in the polar aprotic organic solvent to obtain a mixed solution; S3: Adding an alkaline catalyst and graphene oxide to the mixed solution and performing ultrasonic dispersion treatment to obtain a mixed system; S4: Heating the mixed system to the reaction temperature, maintaining the temperature and stirring to carry out an in-situ polycondensation reaction, and after the reaction is completed, cooling and separating to obtain a solid product; S5: Washing and drying the solid product to obtain the modified graphene lubricant additive. According to the technical solution provided by the embodiments of this invention, the modified graphene lubricant additive has good dispersibility and can effectively reduce friction and wear.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lubricant additive technology, specifically to a modified graphene lubricant additive and its preparation method. Background Technology

[0002] Lubricating oil is hailed as the "blood" of the machinery industry, its main functions being to reduce friction between mechanical parts, decrease wear, aid heat dissipation, and prevent corrosion. As modern machinery increasingly demands high speed, heavy load, and high temperature, the performance requirements for lubricating oils are also rising. Adding high-performance additives to base oils is one effective way to improve the overall performance of lubricating oils. Graphene, as a two-dimensional carbon nanomaterial, has been considered a highly promising lubricating oil additive in recent years due to its extremely high mechanical strength, excellent thermal conductivity, and self-lubricating properties. Theoretical and preliminary experimental studies have shown that graphene nanosheets can form a physical protective film on the surface of friction pairs, and through interlayer slippage and filling repair effects, can significantly reduce the coefficient of friction and wear rate.

[0003] However, a key bottleneck in the practical application of graphene lies in its poor dispersion stability. Due to the strong van der Waals forces and π-π stacking interactions between graphene sheets, it is prone to agglomeration and sedimentation in non-polar lubricating oil bases, making it difficult to maintain a nanoscale dispersion state for a long time. Once agglomerated, graphene not only loses its nanoscale effect but may also exacerbate wear by forming abrasive particles.

[0004] Based on this, various modification strategies have been implemented in existing technologies, including the physical adsorption of surfactants, the reduction treatment of graphene oxide, and the grafting of small organic molecules or polymers through covalent bonds. However, physical adsorption methods are subject to desorption risks and lack stability; while traditional covalent modification can improve dispersibility to some extent, it usually involves complex multi-step reactions, and the grafted molecular chains are highly flexible and easily coil and entangle in oil media, which can lead to the re-aggregation of the modified graphene. Summary of the Invention

[0005] In view of the bottleneck problems of graphene's tendency to agglomerate and poor dispersion stability in lubricating oil in the prior art, this application discloses a method for preparing a modified graphene lubricating oil additive, comprising: S1: Weigh out a fixed amount of tetrahydroxy aromatic monomer containing a spirocyclic structure, tetrahalogenated terephthalonitrile, and polar aprotic organic solvent according to the preset stoichiometric ratio. S2: Dissolve a tetrahydroxy aromatic monomer containing a spirocyclic structure and a tetrahalogenated terephthalonitrile in a polar aprotic organic solvent to obtain a mixed solution; S3: Add an alkaline catalyst and graphene oxide to the mixed solution, and perform ultrasonic dispersion treatment to obtain a mixed system; S4: Heat the mixture to the reaction temperature, keep it at the temperature and stir to carry out the in-situ polycondensation reaction. After the reaction is completed, cool and separate the mixture to obtain the solid product. S5: The solid product is washed and dried to obtain a modified graphene lubricant additive.

[0006] Furthermore, the tetrahydroxy aromatic monomer containing a spirocyclic structure in step S1 includes, but is not limited to, 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane.

[0007] Furthermore, in step S1, the tetrahalogenated terephthalonitrile includes, but is not limited to, tetrafluoroterephthalonitrile.

[0008] Furthermore, the polar aprotic organic solvents in step S1 include, but are not limited to, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

[0009] Furthermore, the alkaline catalyst in step S3 is an alkali metal carbonate, which includes, but is not limited to, alkali metal carbonates. , , .

[0010] Furthermore, in step S2, the molar ratio of the tetrahydroxy aromatic monomer and the tetrahalogenated terephthalonitrile is 1:1.

[0011] Furthermore, in step S3, the molar ratio of the alkaline catalyst to the tetrahydroxy aromatic monomer is 3:1.

[0012] Furthermore, the ultrasonic dispersion treatment time in step S3 is 1 to 4 hours; the reaction temperature in step S4 is 50 to 80°C; and the heat preservation and stirring time is 48 to 96 hours.

[0013] Furthermore, the washing and drying steps in step S5 are as follows: Washing was performed with dichloromethane for 20–40 minutes. The material is dried under vacuum at a temperature of 50–120°C for 10–15 hours. A second aspect of this application mentions a modified graphene lubricant additive, prepared using the method described in the first aspect above.

[0014] The beneficial effects of this application are as follows: This invention relates to the field of lubricant additive technology, specifically to a modified graphene lubricant additive and its preparation method. The method uses a tetrahydroxy aromatic monomer containing a spirocyclic structure, a tetrahalogenated terephthalonitrile, and a polar aprotic organic solvent as raw materials. The tetrahydroxy aromatic monomer and the tetrahalogenated terephthalonitrile are dissolved in the polar aprotic organic solvent, and then an alkaline catalyst and graphene oxide are added. The mixture is then subjected to ultrasonic dispersion, heating and holding at a constant temperature to carry out an in-situ polycondensation reaction. After cooling, separation, washing, and drying, the modified graphene lubricant additive is obtained.

[0015] This invention uses 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spiral bis-indane, tetrafluoroterephthalonitrile, and graphene oxide as raw materials, and N,N-dimethylformamide as a solvent. Through the condensation reaction of tetrafluoroterephthalonitrile with hydroxyl groups, a hydrophobic polymer is in situ bonded to the graphene surface. Because the polymer molecular chain contains a spiro atom center and lacks freely rotating single bonds in the main chain, the molecular configuration is distorted and exhibits extremely high rigidity. The irregular and distorted polymer segments are difficult to stack, thus forming steric hindrance between graphene sheets. This significantly improves the dispersion performance of the modified graphene in lubricating oil, allowing it to maintain a monodisperse or few-layer dispersion state for a long time. The uniformly dispersed modified graphene can fully penetrate the contact area of ​​the friction pair, utilizing the interlayer slip properties and high mechanical strength of graphene itself to form a protective film, thereby effectively reducing the coefficient of friction and wear volume.

[0016] Furthermore, this invention also provides a modified graphene lubricating oil additive prepared by the above-described method. The surface-bonded polymer molecular chains contain spiroatomic centers and lack freely rotating single bonds in the main chain, resulting in a twisted and rigid molecular configuration. These twisted segments are difficult to stack, allowing the additive to maintain a stable dispersion in base oils and enabling the preparation of lubricating oils with friction-reducing and anti-wear properties. This invention introduces a rigid, twisted, hydrophobic polymer onto the graphene surface through in-situ polycondensation. The covalent bonding of this polymer ensures the stability of the additive. Simultaneously, the one-pot in-situ polymerization modification method provides mild reaction conditions, simple operation, and readily available raw materials, making it suitable for industrial production. This comprehensively improves the dispersibility, stability, and friction-reducing and anti-wear properties of graphene in lubricating oils. Attached Figure Description

[0017] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings.

[0018] Figure 1 This is a process flow diagram of a method for preparing a modified graphene lubricating oil additive mentioned in this invention. Detailed Implementation

[0019] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention, but the description is not intended to limit the present invention.

[0020] Therefore, refer to Figure 1 This application discloses a method for preparing a modified graphene lubricating oil additive, comprising: S1: Weigh out a fixed amount of tetrahydroxy aromatic monomer containing a spirocyclic structure, tetrahalogenated terephthalonitrile, and polar aprotic organic solvent according to the preset stoichiometric ratio. It should be noted that in this technical solution, the tetrahydroxy aromatic monomer containing a spirocyclic structure in step S1 includes, but is not limited to, 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-helical bis-indane (hereinafter referred to as TTSBI). The core structural feature of TTSBI is that a spiro atom connects two indane rings, forming a three-dimensional twisted rigid framework. The molecular structure of TTSBI contains a spiro atom and four phenolic hydroxyl groups. Among them, the spiro atom endows the final polymer chain with a rigid twisted configuration, while the four phenolic hydroxyl groups provide the reaction sites required for the condensation reaction with tetrahaloterephthalonitrile.

[0021] This application mentions that the polymer chain formed by the condensation reaction of TTSBI with tetrahalophthalonitrile has specific structural features. The TTSBI molecular structure contains a spiro atom center, through which two indene rings are connected. This structural feature ensures that after the TTSBI undergoes condensation reaction with tetrahalophthalonitrile, the resulting polymer molecular chain retains the spiro atom center and lacks freely rotating single bonds on the main chain. This results in a distorted configuration and extremely high rigidity in the polymer molecule.

[0022] It should be noted that the polymer molecular chains, due to their irregular and twisted configuration, are difficult to stack. Therefore, when these polymer molecules are bonded to the graphene surface through in-situ polycondensation, the polymer chains grafted onto the graphene surface form a spatial barrier layer. This barrier layer effectively prevents the graphene sheets from re-aggregating due to van der Waals forces and π-π stacking. Compared to existing methods that graft flexible polymer chains, which tend to coil and entangle in oil media and fail to form stable spatial barriers, leading to the re-aggregation of modified graphene, the rigid and twisted polymer chains in this invention lack freely rotating single bonds. Their twisted configuration is fixed, preventing close stacking through conformational adjustments, thus creating a persistent steric hindrance effect on the graphene surface.

[0023] This invention introduces rigid, twisted polymer segments containing spiroatomic centers and lacking freely rotatable single bonds in the main chain. Utilizing the difficulty of stacking these irregularly twisted configurations, graphene achieves long-term dispersion in lubricating oil. The resulting modified graphene maintains a monodisperse or few-layer dispersion state in lubricating oil for extended periods, exhibiting significant dispersibility. Based on uniform dispersion, graphene fully leverages its interlayer slip properties and high mechanical strength to form a protective film on the friction pair surface, effectively reducing the coefficient of friction and wear volume. Furthermore, this modification process employs in-situ polycondensation, where the polymer is firmly bonded to the graphene surface via covalent bonds, avoiding desorption problems associated with physical adsorption and ensuring the long-term stability of the additive.

[0024] In this technical solution, the tetrahalogenated terephthalonitrile in step S1 includes, but is not limited to, tetrafluoroterephthalonitrile (TFTN).

[0025] The molecular structure of tetrafluoroterephthalonitrile contains four fluorine atoms and two cyano groups. The two cyano groups are located at positions 1 and 4 of the terephthalonitrile, and the four fluorine atoms are located at positions 2, 3, 5, and 6.

[0026] The tetrafluoroterephthalonitrile molecule mentioned in this application can provide the leaving group required for nucleophilic substitution reactions. Under basic conditions, the phenolic hydroxyl group of TTSBI is deprotonated by potassium carbonate to generate a phenoxy anion. This phenoxy anion acts as a nucleophile, attacking the carbon atom attached to the fluorine atom on the benzene ring of tetrafluoroterephthalonitrile. The fluorine atom then leaves as a leaving group, forming a carbon-oxygen covalent bond.

[0027] On the other hand, TFTN can activate the carbon-fluorine bonds on the benzene ring. The two cyano groups attached to the benzene ring of tetrafluoroterephthalonitrile are strong electron-withdrawing groups. These groups reduce the electron cloud density on the benzene ring through electron-withdrawing inductive effect and conjugation effect, especially making the carbon atom attached to the fluorine atom electron-deficient. This reduces the activation energy of the reaction when the phenoxy anion launches a nucleophilic attack on the carbon atom, allowing the condensation reaction to proceed under mild conditions of 50-80°C.

[0028] It should be noted that, based on the aforementioned synergistic effect, the activation effect of the cyano group on the benzene ring ensures that all four fluorine atoms possess high reactivity, thereby guaranteeing the smooth progress of the polycondensation reaction between TTSBI and tetrafluoroterephthalonitrile. Furthermore, the para-dicyano structure of tetrafluoroterephthalonitrile allows it to form a linear polymer chain during polycondensation with TTSBI. This polymer chain retains the spiro atom center of TTSBI while further enhancing the rigidity of the main chain due to the rigid benzene ring structure of tetrafluoroterephthalonitrile. This results in the polymer segments ultimately grafted onto the graphene surface exhibiting the rigid twisted configuration required by the specifications. This rigid twisted configuration makes it difficult for the polymer segments to stack and entangle, thereby forming a steric hindrance layer between the graphene sheets and achieving long-term dispersion of graphene in lubricating oil.

[0029] In this technical solution, the polar aprotic organic solvents in step S1 include, but are not limited to, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).

[0030] It should be noted that the preparation method mentioned in this application uses TTSBI, tetrafluoroterephthalonitrile and graphene oxide as raw materials, and N,N-dimethylformamide as solvent, to achieve modification through the polycondensation reaction of tetrafluoroterephthalonitrile and hydroxyl groups.

[0031] For example, DMF is chosen as the organic solvent. The DMF molecule contains a carbonyl group with lone pair electrons, enabling it to interact with cations via dipole-dipole interactions. Simultaneously, the DMF molecule does not contain ionizable hydrogen atoms. These structural features give DMF both high polarity and aproticity. High polarity allows DMF to effectively dissolve TTSBI and tetrafluoroterephthalonitrile through dipole-dipole interactions, ensuring uniform dispersion of the reactants at the molecular level and providing a homogeneous reaction environment for the polycondensation reaction. Aproticity prevents DMF from providing hydrogen bonds to phenoxy anions, thus avoiding hydrogen bonding with the phenoxy anions generated from TTSBI in the reaction system and maintaining the high reactivity of this nucleophile.

[0032] This application selects DMF as a polar aprotic organic solvent. Through the synergistic effect of its polarity and aproticity, it simultaneously solves the problems of reactant dissolution, nucleophile activity retention, and transition state stability, providing a suitable medium environment for the polycondensation reaction between TTSBI and tetrafluoroterephthalonitrile, enabling the polycondensation reaction to proceed efficiently under homogeneous and mild conditions.

[0033] S2: Dissolve the tetrahydroxy aromatic monomer containing a spirocyclic structure and the tetrahalogenated terephthalonitrile in a polar aprotic organic solvent to obtain a mixed solution; in this technical solution, the molar ratio of the tetrahydroxy aromatic monomer and the tetrahalogenated terephthalonitrile in step S2 is 1:1.

[0034] It should be noted that condensation polymerization is a stepwise polymerization, where polymer chains grow through repeated condensation between the functional groups of bifunctional monomers. When the molar ratio of the functional groups of the two monomers is strictly equal, all functional groups participate in the polymerization reaction, and the degree of polymerization of the condensation product reaches its maximum value. When the molar ratio deviates from the equimolar ratio, the monomer with fewer functional groups is exhausted first, the growth of the polymer chain is forced to stop, and the degree of polymerization decreases accordingly. The modification effect of this invention relies on the formation of an effective steric hindrance layer on the graphene surface by the polymer chain, which requires the polymer chain to have sufficient length and molecular weight. A 1:1 molar ratio enables the condensation polymerization reaction to achieve the highest degree of polymerization, and the resulting polymer chain length is sufficient to form a stable steric hindrance layer between graphene sheets, preventing the aggregation and stacking of graphene and achieving its long-term stable dispersion in lubricating oil.

[0035] S3: Add an alkaline catalyst and graphene oxide to the mixed solution, and perform ultrasonic dispersion treatment to obtain a mixed system; In this technical solution, the alkaline catalyst in step S3 is an alkali metal carbonate, which includes, but is not limited to, alkali metal carbonates. , , The molar ratio of the alkaline catalyst to the tetrahydroxy aromatic monomer is 3:1.

[0036] It should be noted that this application uses alkali metal carbonates to abstract protons from the phenolic hydroxyl groups of TTSBI, converting them into nucleophilic phenol-oxygen anions, thereby enabling the polycondensation reaction to start and continue. In addition, it can neutralize the hydrogen fluoride removed during the polycondensation reaction, preventing the accumulation of HF from increasing the acidity of the reaction system and inhibiting the deprotonation of the phenolic hydroxyl groups, while also avoiding corrosion of the reaction equipment by HF.

[0037] For example, It can capture the proton from the hydroxyl group of TTSBI phenol and convert it into a phenol-oxygen anion. This phenol-oxygen anion acts as a nucleophile to attack the carbon atom attached to the fluorine atom on the benzene ring of tetrafluoroterephthalonitrile, thus enabling the condensation reaction to start and continue.

[0038] On the other hand, for every new CO bond formed in the condensation polymerization reaction, one molecule of HF is removed. The HF generated in the reaction is neutralized to prevent the accumulation of HF from increasing the acidity of the reaction system and inhibiting the deprotonation of phenolic hydroxyl groups, while simultaneously pulling the reaction equilibrium toward polymer formation.

[0039] It should be noted that alkali metal carbonates are moderately strong bases, strong enough to abstract a proton from the phenolic hydroxyl group (the pKa of the phenolic hydroxyl group is approximately 10, while the pKa of the conjugate acid of the alkali metal carbonate is approximately 10.3). However, their basicity is weaker than that of alkali metal hydroxides, such as NaOH and KOH, and they will not trigger the hydrolysis of the cyano group in the tetrafluoroterephthalonitrile molecule. Secondly, alkali metal carbonates have a certain solubility in polar aprotic organic solvents, allowing them to be uniformly dispersed in the reaction system as dissolved or fine suspended particles, providing a heterogeneous or quasi-homogeneous alkaline environment. Thirdly, the reaction of alkali metal carbonates with the byproduct HF from the polycondensation reaction produces alkali metal fluoride KF and bicarbonate. These byproducts are insoluble in organic solvents and can be separated from the target product by filtration after the reaction.

[0040] In step S3 of this application, ultrasonic dispersion is performed for 1-4 hours, preferably 2 hours. The technical significance of this operation is as follows: Graphene oxide exists in powder form when added to the reaction system. Its layers exhibit van der Waals forces and π-π stacking interactions, making it prone to agglomeration in solvents and difficult to spontaneously disperse. This application utilizes the cavitation effect generated by ultrasound in a liquid to create a locally high-temperature, high-pressure microenvironment. Simultaneously, the shock waves and microjets generated by the collapse of cavitation bubbles provide mechanical energy, exfoliating the graphene oxide aggregates into single-layer or few-layer graphene oxide sheets, thus uniformly dispersing them in the reaction system. After ultrasonic dispersion, the specific surface area of ​​graphene oxide increases significantly, and the oxygen-containing functional groups (hydroxyl, carboxyl, epoxy, etc.) on its surface are fully exposed in the reaction system, providing more bonding sites for the polymer chains generated by the condensation reaction, thereby increasing the grafting density of the polymer on the graphene surface.

[0041] In addition, ultrasonic dispersion also uniformly introduces TTSBI, tetrafluoroterephthalonitrile, and alkaline catalyst into the nanoscale space between graphene oxide sheets, enabling in-situ polycondensation reactions to occur simultaneously on the surface and between layers of graphene, achieving uniform coating of graphene by polymer chains.

[0042] The ultrasonic dispersion treatment time was set to 1-4 hours, based on the following criteria. When the ultrasonic time is less than 1 hour, the degree of exfoliation of graphene oxide is insufficient, and some graphene oxide still exists in the form of aggregates. Its effective specific surface area is not fully exposed, and the number of grafting sites of polymer chains is limited, resulting in no significant improvement in the dispersion performance of modified graphene. When the ultrasonic time exceeds 4 hours, the graphene oxide sheets may develop structural defects due to prolonged high-energy ultrasonic treatment. These defects will weaken the mechanical strength of graphene and affect its performance as a friction-reducing and wear-resistant component.

[0043] In this application, the solubility and dispersion of alkali metal carbonates in polar aprotic organic solvents are directly affected by their particle size in the reaction system. Ultrasonic dispersion exfoliates agglomerated graphene oxide into nanoscale sheets, while simultaneously breaking down the alkali metal carbonate particles and uniformly dispersing them in the reaction system. This allows the catalyst to enter the nanoscale spaces between the graphene oxide sheets, catalyzing the in-situ polycondensation reaction of TTSBI and tetrafluoroterephthalonitrile within these spaces, achieving uniform grafting of polymer chains between and on the surface of the graphene layers. The final product contains modified graphene coated with a sufficient amount of uniformly rigid, twisted polymer chains. These polymer chains form a steric hindrance layer in the lubricating oil, achieving long-term stable dispersion and friction-reducing / wear-resistant effects for the graphene.

[0044] S4: Heat the mixture to the reaction temperature, keep it warm and stir to carry out in-situ polycondensation reaction, cool and separate the mixture after the reaction to obtain the solid product; the reaction temperature in step S4 is 50-80℃; the stirring time is 48-96h.

[0045] It should be noted that condensation polymerization is a reversible equilibrium reaction, where polymer chains grow gradually through repeated condensation between functional groups. Reaction temperature affects the polymerization rate and equilibrium position. When the temperature is below 50℃, the thermal kinetic energy of the reactant molecules is insufficient, reducing the frequency of nucleophilic attack of the phenoxy anion on the carbon atom of the tetrafluoroterephthalonitrile benzene ring, resulting in a slow condensation polymerization rate that cannot reach a sufficient degree of polymerization within a limited time. While temperatures above 80℃ can increase the reaction rate, the polar aprotic organic solvent DMF used in the instructions has a boiling point of 153℃. Although prolonged heating above 80℃ remains within a safe range, higher temperatures may increase the risk of side reactions or adversely affect the stability of oxygen-containing functional groups on the graphene oxide surface.

[0046] It should be noted that under the above temperature conditions, the polycondensation reaction has sufficient reaction time to allow the two monomers to gradually condense into polymer chains with sufficient molecular weight. If the reaction time is less than 48 hours, the polycondensation reaction has not yet reached equilibrium, and the molecular weight of the polymer chain is insufficient to form an effective steric hindrance layer between the graphene sheets. If the reaction time exceeds 96 hours, the reaction has already reached equilibrium, and further extending the time has limited effect on increasing the degree of polymerization, but instead increases the production cycle and energy consumption costs.

[0047] S5: The solid product is washed and dried to obtain a modified graphene lubricant additive.

[0048] In this technical solution, the washing and drying steps in step S5 are as follows: dichloromethane is used for stirring and washing, and the washing time is 20-40 minutes, preferably 30 minutes; In this invention, dichloromethane is used to stir and wash the solid product for 20-40 minutes. After the polycondensation reaction is completed, in addition to the target product modified graphene, unreacted monomers and catalyst residues remain in the product system. The reaction produces KF and other byproducts, as well as oligomers. Dichloromethane can dissolve unreacted TTSBI and tetrafluoroterephthalonitrile monomers, as well as low molecular weight polymer oligomers, while also providing good dispersion for the target product, modified graphene. Stirring and washing for 20-40 minutes ensures sufficient contact between the washing solvent and the product, allowing soluble impurities to dissolve from the solid product. Too short a washing time results in insufficient dissolution of impurities, while too long a washing time reduces production efficiency and provides no additional benefit.

[0049] Drying is carried out under vacuum conditions at a temperature of 50–120°C, preferably 80°C, for a time of 10–15 hours, preferably 12 hours.

[0050] The negative pressure environment used in vacuum drying lowers the boiling points of the solvent and water, allowing residual dichloromethane and moisture to be removed from the product at lower temperatures. Drying at low temperatures avoids thermal damage to the polymer chain structure and functional groups on the graphene oxide surface that could be caused by high-temperature processing, while maximizing the protection of the dispersed structure and surface chemistry of the modified graphene. A drying time of 10–15 hours ensures that residual solvents are fully removed under vacuum and low-temperature conditions, preventing any potential adverse effects of residual solvents on the performance of lubricating oil additives.

[0051] This application uses 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane (TTSBI), tetrafluoroterephthalonitrile (TFTN), and graphene oxide as raw materials, and N,N-dimethylformamide as a solvent. Through a polycondensation reaction between the hydroxyl groups of TFTN and TTSBI, a hydrophobic polymer generated in situ is covalently grafted onto the surface of graphene oxide to obtain modified graphene. The polymer molecular chain contains a helical atom center and lacks freely rotating single bonds in the main chain, resulting in a rigidly twisted molecular configuration. The twisted and irregular chain segments are difficult to stack and entangle, thus forming a steric hindrance layer between the graphene sheets, achieving long-term stable dispersion of the modified graphene in lubricating oil. Based on the above structural characteristics, the modified graphene lubricating oil additive prepared by the present invention has good dispersibility. In the contact area of ​​the friction pair, it can give full play to the interlayer slip characteristics and high mechanical strength of graphene to form a protective film to reduce the friction coefficient and wear volume.

[0052] Compared with existing technologies, this application introduces a hydrophobic polymer with a rigid, twisted structure onto the surface of graphene through in-situ polycondensation. This polymer chain, containing a spiro atom center and lacking freely rotating single bonds, exhibits a twisted, rigid configuration. The twisted chain segments are difficult to stack and entangle, avoiding aggregation between grafted chains. This allows the modified graphene to maintain stable dispersion in lubricating oil for extended periods, significantly improving the additive's dispersion performance. Furthermore, the modified graphene of this application disperses uniformly in lubricating oil, enabling it to penetrate more fully into the contact area of ​​the friction pair. Utilizing its interlayer slip properties and high mechanical strength, it forms a protective film, significantly reducing the coefficient of friction and wear volume.

[0053] The method described in this invention involves in-situ polymerization modification under mild reaction conditions, requiring no complex post-processing steps, and using readily available raw materials, making it suitable for industrial production. The polymer is firmly bonded to the graphene surface via covalent bonds, making it difficult to desorb, and the resulting additive exhibits excellent thermal stability and long-term storage stability.

[0054] The second aspect of this application provides a modified graphene lubricant additive prepared using the above-described method. The polymer molecular chains bonded to the surface of this additive have spiro atom centers, the main chain lacks freely rotating single bonds, and the molecular configuration is twisted and rigid. These twisted chain segments are difficult to stack, allowing the modified graphene to remain monodisperse or few-layer dispersed in the base oil. This modified graphene lubricant additive can be used in lubricant preparation, achieving friction reduction and anti-wear functions by being added to the base oil.

[0055] To better understand the technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings.

[0056] The present invention will be further described below with reference to specific embodiments, but this does not limit the present invention in any way.

[0057] This series of examples uses TTSBI and TFTN as monomers, potassium carbonate as catalyst, and graphene oxide as modified filler. By controlling key parameters such as solvent dosage, monomer ratio, solvent type, graphene oxide ratio and addition amount, reaction temperature, and reaction time, a series of modified polymer precursor materials are prepared. Each example strictly follows the single variable principle, and the remaining process parameters are consistent with the original examples.

[0058] Example 1 (Adjusting the amount of DMF solvent: 20 mL); Place 20 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder (GO) to a flask and ultrasonically disperse it for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0059] Example 2 (Original Baseline Example); Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter, and place the filter cake in an 80 ℃ vacuum oven to dry for 12 hours. Collect and seal for later use.

[0060] Example 3 (Adjusting DMF solvent volume: 35 mL, intermediate gradient); Place 35 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0061] Example 4 (Adjusting the amount of DMF solvent: 50 mL); Place 50 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0062] Example 5 (adjusting the ratio of TTSBI to TFTN to 1:2); Place 30 mL of DMF in a 100 mL three-necked flask. Add 1.705 g (5 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF (the molar ratio of TTSBI to TFTN is 1:2). After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 hours using an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 hours. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0063] Example 6; (Adjusting the ratio of TTSBI to TFTN to 2:1, with an intermediate gradient); Place 30 mL of DMF in a 100 mL three-necked flask. Add 6.82 g (20 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF (the molar ratio of TTSBI to TFTN is 2:1). After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 hours using an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 hours. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0064] Example 7 (adjusting the ratio of TTSBI to TFTN to 4:1). Place 30 mL of DMF in a 100 mL three-necked flask. Add 13.64 g (40 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF (the molar ratio of TTSBI to TFTN is 4:1). After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 hours using an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 hours. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0065] Example 8 (Solvent type control: DMAC); Place 30 mL of DMAC in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMAC. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0066] Example 9 (adjusting the mass ratio of TTSBI to graphene oxide to 6:1, with GO added at 0.3g). Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g of TTSBI and 2.01 g of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 0.3 g of graphene oxide powder (TTSBI to graphene oxide mass ratio approximately 6:1) to a flask, then ultrasonically disperse in an ultrasonic cleaner for 2 h. The mixture is then heated to 60 °C and stirred at this temperature for 72 h. After the reaction is complete, the resulting suspension is allowed to cool naturally to room temperature and filtered to obtain a dark brown solid. The obtained product is then added to an excess of… Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0067] Example 10 (adjusting the mass ratio of TTSBI to graphene oxide to 1:1, with GO addition of 3.4g, and an intermediate gradient). Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g of TTSBI and 2.01 g of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). 3.4 g of graphene oxide powder (TTSBI to graphene oxide mass ratio approximately 1:1) was added to a flask and ultrasonically dispersed in an ultrasonic cleaner for 2 h. The mixture was then heated to 60 °C and stirred at this temperature for 72 h. After the reaction was complete, the resulting suspension was allowed to cool naturally to room temperature and filtered to obtain a dark brown solid. An excess of [amount missing] was added to [amount missing] Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0068] Example 11 (adjusting the mass ratio of TTSBI to graphene oxide to 3:2, with GO added at 2g). Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 2 g of graphene oxide powder (TTSBI to graphene oxide mass ratio approximately 3:2) to a flask and ultrasonically disperse in an ultrasonic cleaner for 2 h. Then, heat to 60 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0069] Example 12 (Reaction temperature controlled: 90°C, intermediate gradient); Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 90 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0070] Example 13 (Reaction temperature controlled: 120°C); Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 120 °C and maintain stirring at this temperature for 72 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0071] Example 14 (Reaction time controlled: 18h); Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 18 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0072] Example 15 (Controlled reaction time: 48h, intermediate gradient); Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 48 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0073] Example 16; Place 30 mL of DMF in a 100 mL three-necked flask. Add 3.41 g (10 mmol) of TTSBI and 2.01 g (10 mmol) of TFTN to the flask and dissolve them in DMF. After complete dissolution, take 4.14 g (30 mmol). Add 1 g of graphene oxide powder to a flask and ultrasonically disperse for 2 h in an ultrasonic cleaner. Then, heat to 60 °C and maintain stirring at this temperature for 96 h. After the reaction is complete, allow the resulting suspension to cool naturally to room temperature and filter to obtain a dark brown solid. Add excess [amount of product] to [amount of product]. Stir and wash for 30 minutes, filter the cake and dry it in an 80 ℃ vacuum oven for 12 hours. Collect and seal for later use.

[0074] Obviously, the above are merely examples for clear illustration and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

[0075] Application Implementation Process The prepared modified graphene lubricating oil additive was added to the lubricating oil base oil in a certain amount to prepare a lubricating oil with an additive content of 0.05 wt%. The mixing process was as follows: pre-stirring at 3000 r / min for 40 min at 30℃, followed by ultrasonic dispersion at 20 kHz for 75 min. The friction performance was tested using an MS-10A four-ball friction testing machine, following the GB / T3142-2019 standard, with a load of 460 N, a rotation speed of 1450 rpm, a temperature of 520 ℃, and a time of 10 seconds.

[0076] The results are shown in Table 1 below. The base oil of the Xintai No. 6 lubricating oil used has a coefficient of friction of 0.084 and a wear scar diameter of 0.338 mm. Lubricating oils containing this additive can significantly reduce the coefficient of friction at the friction interface, decreasing it by 50% during friction, demonstrating excellent friction-reducing properties and making it suitable as a lubricating oil additive.

[0077] Table 1 Comparison of Physicochemical Data of Lubricating Oils In the description of this invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0078] In this specification, the terms "a," "some," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that example or example that is included in at least one or more examples of the invention. The illustrative expressions of the above terms in this specification do not necessarily refer to the same example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more examples or examples. Moreover, those skilled in the art can combine and integrate the different examples and features described in this specification without contradiction.

[0079] It is understood that the above is exemplary and should not be construed as a limitation of the present invention. Those skilled in the art can make modifications, alterations, substitutions and variations to the above within the scope of the present invention.

Claims

1. A method for preparing a modified graphene lubricating oil additive, characterized in that, include: S1: Weigh out a fixed amount of tetrahydroxy aromatic monomer containing a spirocyclic structure, tetrahalogenated terephthalonitrile, and polar aprotic organic solvent according to the preset stoichiometric ratio. S2: Dissolve the tetrahydroxy aromatic monomer containing the spirocyclic structure and the tetrahalogenated terephthalonitrile in the polar aprotic organic solvent to obtain a mixed solution; S3: Add an alkaline catalyst and graphene oxide to the mixed solution, and perform ultrasonic dispersion treatment to obtain a mixed system; S4: Heat the mixture to the reaction temperature, keep it warm and stir to carry out in-situ polycondensation reaction, cool and separate the mixture after the reaction is completed to obtain a solid product; S5: The solid product is washed and dried to obtain a modified graphene lubricant additive.

2. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The tetrahydroxy aromatic monomer containing a spirocyclic structure mentioned in step S1 includes, but is not limited to, 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane.

3. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The tetrahalogenated terephthalonitrile mentioned in step S1 includes, but is not limited to, tetrafluoroterephthalonitrile.

4. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The polar aprotic organic solvents mentioned in step S1 include, but are not limited to, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

5. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The alkaline catalyst mentioned in step S3 is an alkali metal carbonate, which includes, but is not limited to, alkali metal carbonates. , , .

6. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The molar ratio of the tetrahydroxy aromatic monomer and the tetrahalogenated terephthalonitrile in step S2 is 1:

1.

7. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, In step S3, the molar ratio of the alkaline catalyst to the tetrahydroxy aromatic monomer is 3:

1.

8. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The ultrasonic dispersion treatment in step S3 takes 1 to 4 hours; the reaction temperature in step S4 is 50 to 80°C; and the heat preservation and stirring time is 48 to 96 hours.

9. The method for preparing a modified graphene lubricating oil additive according to claim 1, characterized in that, The washing and drying steps in step S5 are as follows: Washing was performed with dichloromethane for 20–40 minutes. Drying is carried out under vacuum conditions at a temperature of 50–120°C for 10–15 hours.

10. A modified graphene lubricating oil additive, characterized in that, It is prepared by the preparation method described in any one of claims 1-9.