A method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus
By co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus, the problem of unstable phosphorus enrichment in steel slag was solved, achieving efficient phosphorus recovery and solid waste resource utilization, and improving the comprehensive utilization rate of steel slag.
Patent Information
- Application Number
- CN202611616617.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing single solid waste modification methods are difficult to simultaneously achieve phosphorus enrichment in steel slag and slag property control, resulting in low comprehensive utilization rate of steel slag, low phosphorus recovery rate, and insufficient industrial adaptability.
Red mud and biomass ash were combined at a mass ratio of (1~4):1 to modify molten steel slag. The modification temperature and cooling regime were controlled. After grinding, the mixture was mixed with an acidic solution for selective leaching. The pH value was controlled at 3.5~5.0 to recover phosphorus products.
It achieves highly efficient and selective leaching of phosphorus, with a phosphorus leaching rate of over 84% and an iron leaching rate of less than 10%. At the same time, it realizes the synergistic resource utilization of red mud, biomass ash and steel slag, reducing environmental risks and ecological damage from the mining of natural minerals.
Smart Images

Figure CN123108213A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical waste resource utilization technology, and in particular relates to a method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus. Background Technology Steel slag is a major solid waste generated during the steelmaking process, but its comprehensive utilization rate has long been low, and large-scale stockpiling not only occupies land but also poses pollution risks. At the same time, steel slag contains approximately 1% to 5% P2O5, and with the increasing scarcity of natural phosphate rock resources, recovering phosphorus from steel slag has significant resource value.
[0002] Phosphorus in steel slag mainly exists as a solid solution of 2CaO·SiO2-3CaO·P2O5. This solid solution can be selectively leached using a weakly acidic citric acid solution, achieving a phosphorus dissolution rate of 85.1% at pH 5, while the iron dissolution rate is only 6.7%, demonstrating good selectivity. However, because this solid solution is dispersed in the steel slag, direct acid leaching is not ideal for phosphorus extraction. Therefore, it is necessary to modify the steel slag to promote the enrichment of phosphorus-containing solid solutions.
[0003] Existing technologies mostly employ single solid wastes to modify molten steel slag. Red mud and biomass ash are two commonly used modifiers. Red mud, a highly alkaline residue from alumina extraction from bauxite, is rich in Fe2O3, Al2O3, SiO2, and Na2O, exhibiting high reactivity. Biomass ash, sourced from biomass power plants, typically contains over 10% K2O and a certain amount of CaO. While both can promote the enrichment of phosphorus-containing solid solutions to some extent when used for steel slag modification, they each have significant limitations: when red mud is used alone, its high Fe2O3 content readily reacts with CaO to form calcium ferrite, consuming active CaO and hindering the full enrichment of phosphorus-containing solid solutions; when biomass ash is used alone, its high K and Na content can excessively reduce slag viscosity, accelerating furnace lining erosion, and its dispersed sources and high collection costs make large-scale application difficult.
[0004] Therefore, existing single solid waste modification methods are difficult to simultaneously achieve the enrichment of phosphorus-containing solid solutions and the regulation of slag properties, and generally suffer from problems such as unstable effects, difficulty in controlling alkalinity, and insufficient industrial adaptability. Summary of the Invention
[0005] In view of the above problems, this application provides a method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus. This invention solves at least one of the following problems: low comprehensive utilization rate of steel slag, low phosphorus recovery rate from steel slag, difficulty in balancing phosphorus enrichment and process stability when using red mud or biomass ash alone to modify steel slag, and difficulties in the co-utilization of industrial solid wastes such as red mud, biomass ash, and steel slag.
[0006] This invention provides a method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus, comprising the following steps: (1) Red mud and biomass ash are added to molten steel slag for modification treatment, wherein the mass ratio of red mud to biomass ash is (1~4):1; (2) The modified steel slag is cooled and ground to obtain modified steel slag powder; (3) The modified steel slag powder is mixed with an acidic solution for selective leaching. The pH value is controlled at 3.5~5.0 during the leaching process. After the leaching is completed, the solid and liquid are separated to obtain leaching residue and phosphorus-containing leachate. (4) Separate and recover phosphorus products from the phosphorus-containing leachate.
[0007] In some embodiments, the biomass ash includes at least one of corn stalk ash, wheat stalk ash, rice husk ash, and cotton stalk ash.
[0008] In some embodiments, in step (1), the total amount of red mud and biomass ash added per 1 kg of steel slag is 80~300 g.
[0009] In some embodiments, in step (1), 100-200g of red mud and 50-100g of biomass ash are added per 1kg of steel slag.
[0010] In some embodiments, step (1) is carried out in an air atmosphere, and the temperature of the modification treatment is 1500~1600℃, and the holding time is 30~90min.
[0011] In some embodiments, before step (1), the red mud is crushed and ground to a particle size ≤75μm, the biomass ash is passed through a 100-mesh sieve, and the steel slag is crushed, ball-milled, and then passed through a 200-mesh sieve.
[0012] In some embodiments, in step (2), the cooling of the modified steel slag includes: cooling to 1350°C at a cooling rate of 6~12°C / min and holding for 30~90min, and then water quenching to room temperature.
[0013] In some embodiments, in step (2), the particle size of the modified steel slag powder is ≤48μm.
[0014] In some embodiments, during selective leaching in step (3), the solid-liquid ratio of the modified steel slag powder to the acidic solution is 1:10~1:50 kg / L, the leaching temperature is 20~60℃, and the leaching time is 30~90min.
[0015] In some embodiments, the acidic solution is an aqueous solution of citric acid, and the concentration of the aqueous solution of citric acid is 0.3~1.5 mol / L.
[0016] In some embodiments, in step (4), an alkaline precipitant is added to the phosphorus-containing leachate to adjust the pH to 7.5-9.0, and phosphorus products are precipitated.
[0017] In some embodiments, the main components of the red mud include, by mass percentage: Fe2O3: 30%~60%, Al2O3: 10%~20%, SiO2: 10%~20%, CaO: 2%~8%.
[0018] In some embodiments, the main components of the biomass ash include, by mass percentage: SiO2: 30%~60%, K2O: 5%~20%, CaO: 5%~15%, MgO: 2%~8%.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects: 1. This invention combines red mud and biomass ash in a mass ratio of (1~4):1 for the modification of molten steel slag. The Na2O and Al2O3 components in the red mud reduce the viscosity of the molten steel slag and promote ion diffusion, while the K2O in the biomass ash induces the crystal transformation and volume growth of phosphorus-containing solid solutions. The synergistic effect of these two components enhances the enrichment of phosphorus-containing solid solutions in the steel slag. Based on this, the modified steel slag is cooled and ground, then mixed with an acidic solution for selective leaching. The pH value is controlled at 3.5~5.0, which helps to achieve efficient phosphorus leaching while inhibiting iron leaching. The phosphorus leaching rate can reach over 84%, while the iron leaching rate is less than 10%. Simultaneously, using red mud and biomass ash instead of natural minerals as modifiers helps reduce the environmental risks associated with solid waste storage and mitigates the ecological damage caused by natural mineral mining. Finally, phosphorus products are recovered from the phosphorus-containing leachate, achieving phosphorus resource recovery.
[0020] 2. This invention, through the synergistic control of key process parameters such as the ratio of red mud to biomass ash, modification temperature, cooling regime, grinding particle size and leaching conditions, is conducive to promoting the directional enrichment and growth of phosphorus-containing solid solutions and provides a relatively stable process window for the efficient and selective leaching of phosphorus.
[0021] 3. This invention simultaneously realizes the synergistic resource utilization of three major solid wastes: red mud, steel slag, and biomass ash. Red mud and steel slag are the main solid wastes in the metallurgical industry, while biomass ash is a major byproduct of biomass power plants. All three can be transformed into high-value-added products and recyclable secondary resources through this method, forming a closed loop of "solid waste synergy - phosphorus resource recovery - product reuse," which helps reduce dependence on natural phosphate rock resources.
[0022] 4. The process flow of this invention is simple, mainly involving conventional unit operations such as high-temperature melting, grinding and acid leaching. It has low equipment requirements, good process controllability, and is easy to realize industrial production. Attached Figure Description
[0023] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 This is a process flow diagram of the method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus according to the present invention. Figure 2 The image shows the XRD pattern of the modified steel slag in Example 1 of this invention. Figure 3 The images show the XRD patterns of the leaching residues after steel slag leaching in Example 1 and Comparative Examples 1-3 of this invention. Detailed Implementation
[0024] The embodiments of the technical solution of this application will be described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are intended to cover non-exclusive inclusion.
[0026] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.
[0027] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0028] A specific embodiment of the present invention provides a method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus, comprising the following steps: (1) Red mud and biomass ash are added to molten steel slag for modification treatment, wherein the mass ratio of red mud to biomass ash is (1~4):1; (2) The modified steel slag is cooled and ground to obtain modified steel slag powder; (3) The modified steel slag powder is mixed with an acidic solution for selective leaching. The pH value is controlled at 3.5~5.0 during the leaching process. After the leaching is completed, the solid and liquid are separated to obtain leaching residue and phosphorus-containing leachate. (4) Separate and recover phosphorus products from the phosphorus-containing leachate.
[0029] By combining red mud and biomass ash for the upgrading of molten steel slag, and supplementing it with selective leaching with acidic solution and recovery of phosphorus products, it is beneficial to achieve selective separation of phosphorus while promoting the enrichment of phosphorus-containing solid solutions in steel slag, and simultaneously achieve the synergistic treatment of three types of solid waste: red mud, biomass ash and steel slag.
[0030] In some embodiments, the mass ratio of red mud to bioash can be, for example, 1:1, 2:1, 3:1, 4:1, or a value within the range obtained by any combination of the above two values.
[0031] In some embodiments, in step (1), the total amount of red mud and biomass ash added is 80-300 g per 1 kg of steel slag. This provides sufficient active components for the modification reaction while also taking into account the cost of the modifier.
[0032] In some embodiments, in step (1), 100-200g of red mud and 50-100g of biomass ash are added per 1kg of steel slag. This helps to achieve a balance between synergistic modification effect and cost control while maintaining reactivity.
[0033] Optionally, 150-200g of red mud and 50-80g of biomass ash may be added to every 1kg of steel slag.
[0034] Optionally, in step (1), the red mud and biomass ash are pre-mixed evenly before being added, or added sequentially and stirred thoroughly. By controlling the feeding method, the two modifiers can be evenly dispersed and fully reacted in the slag, which is beneficial to exert their synergistic modifying effect and improve the uniformity of modification.
[0035] In some embodiments, step (1) is carried out in an air atmosphere, the temperature of the modification treatment is 1500~1600℃, and the holding time is 30~90min. This is conducive to the full melting of steel slag and maintaining suitable fluidity, allowing the active components in red mud and biomass ash to fully diffuse and participate in the reaction, and promoting the formation of phosphorus-containing solid solutions.
[0036] Optionally, the temperature of the modification treatment is 1500~1550℃ and the holding time is 60~90min. Within this temperature and time range, the fluidity of the steel slag melt is more suitable, which is conducive to the full diffusion of active components and their participation in the reaction.
[0037] In some embodiments, the temperature of the modification treatment may be, for example, 1500°C, 1520°C, 1550°C, 1580°C, 1600°C, or a value within the range obtained by any combination of the above two values.
[0038] In some embodiments, before step (1), the red mud is crushed and ground to a particle size ≤75μm, the biomass ash is passed through a 100-mesh sieve, and the steel slag is crushed, ball-milled, and then passed through a 200-mesh sieve. This is beneficial for improving the dispersion uniformity of the modifier in the molten slag, increasing the reaction interface, and providing favorable conditions for subsequent synergistic modification reactions.
[0039] In some embodiments, the moisture content of the dried red mud is ≤2%; unburned carbon particles are removed from the biomass ash before sieving; and the steel slag is converter steel slag or electric furnace steel slag.
[0040] In some embodiments, in step (2), the cooling of the modified steel slag includes: cooling to 1350°C at a cooling rate of 6~12°C / min and holding at that temperature for 30~90min, followed by water quenching to room temperature. This is beneficial for controlling the crystal transformation and growth process of phosphorus-containing solid solutions and promoting further enrichment of phosphorus in the solid solution.
[0041] In some embodiments, water mist cooling is used in step (2). This can achieve relatively stable cooling in the early stage of the modification, providing a basis for subsequent cooling processes.
[0042] In some embodiments, in step (2), the particle size of the modified steel slag powder is ≤48μm. This can increase the solid-liquid contact area and improve the leaching rate and leaching volume of phosphorus during subsequent acid leaching.
[0043] In some embodiments, during selective leaching in step (3), the solid-liquid ratio of the modified steel slag powder to the acidic solution is 1:10~1:50 kg / L, the leaching temperature is 20~60℃, and the leaching time is 30~90min. This provides relatively stable process conditions for the selective leaching of phosphorus.
[0044] In some embodiments, step (3) of the selective leaching process is carried out under stirring, optionally with mechanical stirring assistance, at a stirring speed of 300-500 rpm. This can enhance solid-liquid mass transfer and improve leaching efficiency.
[0045] In some embodiments, the acidic solution is an aqueous solution of citric acid, with a concentration of 0.3~1.5 mol / L. This is beneficial for inhibiting the dissolution of iron while leaching phosphorus; and citric acid is a biodegradable organic acid, which can reduce the environmental impact of the leaching process and the risk of equipment corrosion.
[0046] The P2O5 mass fraction in the leaching residue obtained in step (3) is ≤0.30%, and it can be returned to the sintering or steelmaking process as a metallurgical flux.
[0047] In some embodiments, in step (4), an alkaline precipitant is added to the phosphorus-containing leachate to adjust the pH to 7.5-9.0, and phosphorus products are precipitated. This allows phosphorus to precipitate from the solution, providing conditions for the separation and recovery of phosphorus products. The phosphorus-containing leachate can be concentrated and used directly as liquid phosphate fertilizer or phosphorus chemical raw material.
[0048] In some embodiments, the phosphorus product obtained in step (4) has a P2O5 mass fraction of 22% to 30% and is used as a phosphate fertilizer or phosphate raw material.
[0049] In some embodiments, the alkaline precipitant includes at least one of lime milk, ammonia water, or sodium hydroxide solution. A suitable precipitating agent is selected based on actual process conditions and cost factors.
[0050] In some embodiments, the main components of the red mud include, by mass percentage: Fe2O3: 30%~60%, Al2O3: 10%~20%, SiO2: 10%~20%, CaO: 2%~8%.
[0051] In some embodiments, the main components of the biomass ash include, by mass percentage: SiO2: 30%~60%, K2O: 5%~20%, CaO: 5%~15%, MgO: 2%~8%.
[0052] The components of red mud, such as Fe2O3, Al2O3, SiO2, CaO, and Na2O, along with the components of biomass ash, such as SiO2, K2O, CaO, and MgO, can form a complex regulatory effect in molten steel slag. Na2O and Al2O3 in red mud help reduce the viscosity of the molten steel slag and promote ion diffusion; K2O in biomass ash can directionally induce the crystal transformation and volume growth of phosphorus-containing solid solutions. This synergistic effect promotes the enrichment of phosphorus-containing solid solutions while simultaneously utilizing the moderate viscosity-enhancing effect of Al2O3 in red mud to offset the excessive viscosity reduction caused by alkali metal oxides in biomass ash. This approach balances phosphorus enrichment and slag property regulation to a certain extent, providing a relatively stable mineral phase basis for subsequent selective leaching.
[0053] In some embodiments, the red mud is Bayer process red mud or sintered process red mud, and its drying temperature is 105~120℃. The particle size requirement after grinding is to pass through a 200-mesh sieve. Controlling the quality of raw materials reduces process fluctuations caused by excessive moisture and excessively large particle sizes.
[0054] Biomass ash includes at least one of corn stalk ash, wheat stalk ash, rice husk ash, or cotton stalk ash. The applicability of the process to biomass fuels in different regions will be expanded.
[0055] In summary, this invention promotes the enrichment of phosphorus-containing solid solutions and the efficient and selective leaching and recovery of phosphorus by synergistic modification of steel slag with red mud and biomass ash. At the same time, it realizes the synergistic treatment and resource utilization of three types of solid waste: red mud, steel slag and biomass ash. Moreover, the process is simple and easy to industrialize.
[0056] The method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus according to the present invention will be described below with reference to specific embodiments.
[0057] Example 1 This embodiment provides a method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus.
[0058] Raw materials: Bayer process red mud was used, dried to a moisture content of ≤2%, and crushed and ground to a particle size of ≤75μm; biomass ash was corn stalk combustion ash, sieved through a 100-mesh sieve to remove unburned carbon particles; steel slag was converter steel slag, crushed, ball-milled, and sieved through a 200-mesh sieve for later use. The chemical composition of converter steel slag, red mud, and biomass ash is shown in Table 1.
[0059] A method for co-modifying steel slag with red mud and biomass ash to recover phosphorus, such as... Figure 1 As shown, the specific steps include the following: (1) Take 1 kg of converter steel slag, add 150 g of red mud and 50 g of biomass ash to each 1 kg of steel slag, and add red mud and biomass ash to the molten converter steel slag, wherein the mass ratio of red mud to biomass ash is 3:1; under air atmosphere, control the modification temperature to 1550℃ and keep it at that temperature for 60 min.
[0060] (2) The modified steel slag is cooled to 1350℃ by water mist at a rate of 6~12℃ / min and kept at that temperature for 60min. Then it is cooled to room temperature by water quenching. The cooled modified steel slag is crushed and ball-milled to obtain modified steel slag powder.
[0061] (3) Selective leaching was carried out by mixing modified steel slag powder with citric acid solution. The concentration of citric acid solution was 0.8 mol / L, the solid-liquid ratio of modified steel slag powder to citric acid solution was 1:20 kg / L, the leaching temperature was 25℃, and the leaching time was 60 min. During the leaching process, dilute citric acid was used to adjust the pH value to be stable at 3.8~4.2. The leaching process was carried out under stirring conditions at a stirring speed of 400 rpm. After leaching, the residue is separated by pressure filtration to obtain leaching residue and phosphorus-containing leachate. The leaching residue contains 0.21% P2O5 (mass fraction) and 18.5% iron (calculated as Fe2O3), which can be returned to the sintering batch as a metallurgical flux.
[0062] (4) Add lime water to the phosphorus-containing leachate to adjust the pH to 8.2, and calcium phosphate precipitate is generated. The precipitate is filtered by plate and frame filter, washed and dried at 80°C to obtain the phosphorus product.
[0063] The test results showed that the P2O5 concentration in the leachate was 3.75 g / L, and the leachate volume was 9.5L. Therefore, the total P2O5 in the leachate was 35.6g, the total P2O5 in the modified steel slag was 41.2g, and the phosphorus leaching rate was 86.4%. The iron leaching rate (calculated as Fe ions) was 8.1%. The P2O5 content in the phosphorus product was 26.8% (mass fraction).
[0064] Example 2 The difference from Example 1 is as follows: In step (1), 1 kg of converter steel slag is taken, and red mud and biomass ash are added sequentially to the molten converter steel slag according to the ratio of 200 g of red mud and 80 g of biomass ash per 1 kg of steel slag, and the mixture is stirred thoroughly. The mass ratio of red mud to biomass ash is 2.5:1. In step (3), the concentration of citric acid solution is 0.8 mol / L, the solid-liquid ratio of modified steel slag powder to citric acid solution is 1:25 kg / L, and the leaching time is 80 min. The rest is the same as in Example 1. The leaching rate of phosphorus was 88.7%, and the leaching rate of iron was 7.9%. The P2O5 content in the phosphorus product was 27.4% (mass fraction).
[0065] Example 3 The difference from Example 1 is as follows: In step (1), the red mud is sintered red mud, and the biomass ash is rice straw combustion ash. 1 kg of converter steel slag is taken, and red mud and biomass ash are added at a ratio of 100 g of red mud and 100 g of biomass ash per 1 kg of steel slag (mass ratio 1:1). The mixture is then placed in an induction furnace and heated to 1550℃ to melt. In step (3), the concentration of citric acid solution is 0.6 mol / L, the solid-liquid ratio of modified steel slag powder to citric acid solution is 1:15 kg / L, the leaching temperature is 40℃, and the leaching time is 50 min. The rest is the same as in Example 1.
[0066] The phosphorus leaching rate was 84.9%, and the iron leaching rate was 8.8%. The P2O5 content in the phosphorus product was 25.1% (mass fraction).
[0067] Comparative Example 1 The difference from Example 1 is that no modification treatment is performed; instead, the converter slag is directly crushed, ball-milled, and then selectively leached according to the leaching conditions of Example 1.
[0068] The test results showed that the phosphorus leaching rate was 61.2% and the iron leaching rate was 16.5%.
[0069] Comparative Example 2 The difference from Example 1 is that in step (1), 1 kg of converter steel slag is taken, and red mud is added to the molten converter steel slag at a ratio of 200 g per kg of steel slag. No biomass ash is added. The rest is the same as in Example 1.
[0070] Tests showed that the phosphorus leaching rate was 70.5% and the iron leaching rate was 10.8%.
[0071] Comparative Example 3 The difference from Example 1 is that in step (1), 1 kg of converter steel slag is taken, and biomass ash is added to the molten converter steel slag at a ratio of 200 g of biomass ash per 1 kg of steel slag. No red mud is added. The rest is the same as in Example 1.
[0072] The test results showed that the phosphorus leaching rate was 72.3% and the iron leaching rate was 10.2%.
[0073] Detection methods The phosphorus and iron content in the leachate and modified steel slag was determined by inductively coupled plasma optical emission spectrometry (ICP-OES); solid samples were analyzed after acid dissolution treatment. The P2O5 and iron ion concentrations in the leachate were directly measured by ICP-OES, and the leachate volume was measured using a graduated cylinder or flow meter. The phosphorus leaching rate was calculated as the ratio of the mass of phosphorus in the leachate to the total mass of phosphorus in the modified steel slag, and the iron leaching rate was calculated using the same method. The P2O5 content in the phosphorus products was determined by the quinoline phosphomolybdate gravimetric method or spectrophotometry, and the iron content was determined by potassium dichromate titration or ICP-OES.
[0074] Table 1
[0075] Comparative Example 1, without modification treatment, showed a phosphorus leaching rate of 61.2% and an iron leaching rate of 16.5% after direct acid leaching. The C2S-C3P solid solution in the unmodified steel slag was relatively dispersed, resulting in limited phosphorus extraction efficiency during direct acid leaching, and a large amount of iron minerals were simultaneously dissolved, leading to poor selectivity.
[0076] Comparative Example 2, using only red mud modification, achieved a phosphorus leaching rate of 70.5% and an iron leaching rate of 10.8%; Comparative Example 3, using only biomass ash modification, achieved a phosphorus leaching rate of 72.3% and an iron leaching rate of 10.2%. Compared to Comparative Example 1, the phosphorus leaching rate was higher and the iron leaching rate was lower after single modification, indicating that single solid waste modification can promote the enrichment of phosphorus-containing solid solutions and improve leaching selectivity to some extent; however, the phosphorus leaching rate is still below 80%, and there is still room for improvement in the enrichment of phosphorus-containing solid solutions.
[0077] Examples 1-3 employed a combined modification of red mud and biomass ash, with a mass ratio ranging from 1 to 4:1. In Example 1, the phosphorus leaching rate was 86.4%, and the iron leaching rate was 8.1%; in Example 2, the phosphorus leaching rate was 88.7%, and the iron leaching rate was 7.9%; in Example 3, the phosphorus leaching rate was 84.9%, and the iron leaching rate was 8.8%. Compared to Comparative Examples 1-3, the phosphorus leaching rate in Examples 1-3 was significantly increased, while the iron leaching rate was decreased. These data indicate that the combined modification of red mud and biomass ash is superior to single modification schemes in increasing phosphorus leaching rate and reducing iron leaching rate.
[0078] Combination Figure 2 and Figure 3 The XRD analysis results showed that the diffraction signal of phosphorus-containing solid solution (C2S-C3P) in the synergistically modified steel slag was enhanced, while the signal of this solid solution in the leaching residue was weakened, and the signal of iron phase minerals still maintained a certain intensity, which supported the above results of phosphorus selective leaching from the perspective of mineral phase.
[0079] In summary, this invention promotes the enrichment of phosphorus-containing solid solutions and the efficient and selective leaching and recovery of phosphorus by synergistic modification of steel slag with red mud and biomass ash. At the same time, it realizes the synergistic treatment and resource utilization of three types of solid waste: red mud, steel slag and biomass ash. Moreover, the process is simple and easy to industrialize.
[0080] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for co-modifying steel slag with red mud and biomass ash and selectively leaching phosphorus, characterized in that, Includes the following steps: (1) Red mud and biomass ash are added to molten steel slag for modification treatment, wherein the mass ratio of red mud to biomass ash is (1~4):1; (2) The modified steel slag is cooled and ground to obtain modified steel slag powder; (3) The modified steel slag powder is mixed with an acidic solution for selective leaching. The pH value is controlled at 3.5~5.0 during the leaching process. After the leaching is completed, the solid and liquid are separated to obtain leaching residue and phosphorus-containing leachate. (4) Separate and recover phosphorus products from the phosphorus-containing leachate.
2. The method according to claim 1, characterized in that, In step (1), the total amount of red mud and biomass ash added per 1 kg of steel slag is 80~300 g.
3. The method according to claim 1 or 2, characterized in that, In step (1), 100-200g of red mud and 50-100g of biomass ash are added per 1kg of steel slag.
4. The method according to claim 1, characterized in that, Step (1) is carried out in an air atmosphere, and the temperature of the modification treatment is 1500~1600℃, and the holding time is 30~90min.
5. The method according to claim 1, characterized in that, Before step (1), the red mud is crushed and ground to a particle size ≤75μm, the biomass ash is passed through a 100-mesh sieve, and the steel slag is crushed, ball-milled, and then passed through a 200-mesh sieve.
6. The method according to claim 1, characterized in that, In step (2), the cooling of the modified steel slag includes: cooling to 1350°C at a cooling rate of 6~12°C / min and holding for 30~90min, and then water quenching to room temperature.
7. The method according to claim 6, characterized in that, In step (2), the particle size of the modified steel slag powder is ≤48μm.
8. The method according to claim 1, characterized in that, In step (3), during selective leaching, the solid-liquid ratio of the modified steel slag powder to the acidic solution is 1:10~1:50 kg / L, the leaching temperature is 20~60℃, and the leaching time is 30~90min; And / or, the acidic solution is an aqueous solution of citric acid, and the concentration of the aqueous solution of citric acid is 0.3~1.5 mol / L.
9. The method according to claim 1, characterized in that, In step (4), an alkaline precipitant is added to the phosphorus-containing leachate to adjust the pH to 7.5-9.0, and phosphorus products are obtained by precipitation.
10. The method according to claim 1, characterized in that, The main components of the red mud, by mass percentage, are: Fe2O3: 30%~60%, Al2O3: 10%~20%, SiO2: 10%~20%, CaO: 2%~8%; The main components of the biomass ash, by mass percentage, include: SiO2: 30%~60%, K2O: 5%~20%, CaO: 5%~15%, and MgO: 2%~8%.