3000m 3 Rapid recovery method for pipeline stroke in blast furnace
The blast furnace pipeline stroke recovery method, which combines graded response and multi-parameter coordination, solves the gas loss imbalance problem caused by blast furnace pipeline stroke, enabling rapid recovery of furnace conditions and stable production, and avoiding furnace temperature fluctuations and equipment damage.
Patent Information
- Application Number
- CN202611466520.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
The gas imbalance caused by the blast furnace pipeline is not standardized and parameter linkage is lacking in the current handling operation, which can easily cause furnace temperature fluctuations, deterioration of the gas column permeability, difficulty in quickly restoring the furnace condition, and the disconnect between slag and iron discharge and furnace operation, which prolongs the duration of the abnormality.
Based on the duration of pipeline operation, a graded response level is established, and parameters such as air volume, oxygen enrichment, pulverized coal injection, blast humidity, air temperature, and coke reheating are precisely matched. Combined with the control of slag and iron discharge in front of the furnace, a dual guarantee mechanism of multi-parameter coordination and furnace temperature baseline is constructed to restore the furnace thermal regime and gas flow distribution in stages and gradients.
It achieves rapid suppression of blast furnace pipeline travel and smooth recovery of furnace conditions, avoiding large fluctuations in furnace temperature and equipment damage, reducing losses from unplanned shutdowns, and improving production stability and safety.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of blast furnace abnormal condition handling technology, and more specifically, it relates to 3000m... 3 A rapid method for restoring the pipeline stroke of a blast furnace. Background Technology
[0002] Blast furnace pipeline flow is a typical gas imbalance fault that occurs during ironmaking due to the combined effects of multiple factors, including fluctuations in furnace charge quality, uneven charge distribution, abnormal furnace temperature, and untimely slag and iron discharge. Its core mechanism is the deterioration of permeability in localized charge columns within the furnace, leading to uneven resistance distribution. This causes the originally uniformly distributed gas flow to concentrate and rise at high speed along localized channels with lower resistance, forming a "pipeline-like" gas flow channel.
[0003] When a pipeline malfunction occurs, typical operating conditions include: severe fluctuations in air pressure, abnormal increases in pressure differential, sudden increases in localized temperature readings at multiple points on the furnace top, uneven distribution of gas at the furnace top, and a significant increase in heat load. This is accompanied by abnormal material flow rate and fluctuations in tuyeres' operating conditions. In severe cases, secondary malfunctions such as slag and iron buildup at the tuyeres and damage to furnace cooling equipment may occur. If not handled promptly or operated improperly, the high-speed gas flow will continuously scour the furnace charge, further damaging the permeability of the charge column, leading to more serious charge collapses, charge suspension, and even furnace hearth freezing. Ultimately, this forces an emergency shutdown, resulting in a significant decrease in blast furnace production efficiency and substantial economic losses.
[0004] Currently, the standardization of operations for handling blast furnace pipeline travel is low. There is a lack of tiered and quantified operational standards based on pipeline duration, and the handling process relies entirely on the foreman's personal experience. There are no unified operational guidelines for reducing blast volume, oxygen levels, pulverized coal injection, and coke replenishment. Different operators use significantly different methods, easily missing the optimal time for pipeline suppression. Furthermore, the handling operations suffer from insufficient coordination among multiple parameters. Adjustments to blast volume, oxygen enrichment, pulverized coal injection, blast humidity, and thermal regime are independent, lacking a linkage mechanism. Adjusting a single parameter can easily cause significant fluctuations in furnace temperature and further deterioration of the burden permeability, making it difficult to achieve a positive restoration of furnace conditions.
[0005] Furthermore, the slag and iron discharge process is disconnected from the furnace operation, and the impact of the slag and iron discharge rhythm at the furnace front on the permeability of the furnace charge column is completely ignored. When the pipeline malfunctions, the accumulation of slag and iron in the hearth will further worsen the gas flow distribution. If the slag and iron discharge rhythm does not match the furnace control operation, it will directly lead to a reduction in the pipeline treatment effect, or even induce a secondary pipeline malfunction.
[0006] After the pipeline travel is eliminated, the lack of clear operational guidelines for phased and gradual recovery leads to chaotic operation rhythms for increasing air volume, oxygen supply, and coal supply. When parameters are restored drastically at once, the airflow distribution inside the furnace changes rapidly, easily inducing pipeline travel again and prolonging the duration of abnormal furnace conditions. Existing handling methods often focus on quickly restoring air volume and suppressing pipeline travel, neglecting the control of the furnace temperature baseline. This can easily lead to serious accidents such as furnace cooling or even hearth freezing due to excessive air reduction and untimely heat replenishment, causing wider production interruptions and equipment damage.
[0007] Therefore, it is necessary to invent a standardized pipeline rapid recovery solution for daily blast furnace operation, uninterrupted smelting, and multi-process coordinated operation. This solution should accurately match the pipeline development level for appropriate measures, systematically repair the distribution of gas flow and thermal stability within the furnace, overcome various shortcomings of existing technologies, and support the stable and efficient operation of the blast furnace. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide a 3000m 3 The rapid recovery method for the pipeline stroke of a blast furnace is based on the pipeline duration as the core criterion. Combined with the quantitative thresholds of the material line, furnace top temperature, and heat load, the pipeline stroke is divided into three standard response levels and matched with precise quantitative operating parameters. This effectively solves the problems of traditional handling methods that rely on the foreman's experience and are rough in operation. It can quickly suppress the development of pipeline airflow and prevent the furnace condition from deteriorating.
[0009] The above-mentioned technical objective of the present invention is achieved through the following technical solution: A 3000m 3 The rapid recovery method for the pipeline stroke of a blast furnace is as follows.
[0010] Phase 1: Based on changes in wind pressure and differential pressure, three response levels are defined according to pipeline duration and supporting operating conditions. Each level is precisely matched with seven in-furnace coordinated parameters, including air volume, oxygen enrichment, pulverized coal injection, blast humidity, air temperature, coke reheating, and ore batch adjustment. Corresponding slag and iron discharge control standards are implemented simultaneously to quickly curb the development of pipeline airflow. Phase Two: After the pipeline travel characteristics have completely disappeared, the core references are the recovery status of the material line, furnace temperature level, permeability index, and heat load change trend. The six furnace parameters of air volume, oxygen enrichment, pulverized coal injection, blast humidity, blast temperature, and ore batch are adjusted in a step-by-step manner at nine time nodes. The adjustment range and observation interval of the parameters are strictly controlled to gradually restore the furnace thermal regime and material column permeability, ensuring that the furnace condition returns to normal smelting state smoothly. During the recovery process, if the physical heat of molten iron is <1480℃, all blasting and oxygen enrichment operations are immediately suspended, and coke is added first for supplemental heating. After the furnace temperature trend rises, the gradient recovery plan is continued.
[0011] In one embodiment, during the first stage, when the pipeline duration is 1-2 minutes, the material line is 1500-1900 mm, the furnace top temperature reaches a maximum of 380-450°C, and the heat load increases by 1800 × 10⁻⁶. 7 When J / h, it is determined to be a first-level pipeline stroke; When the pipeline duration is 2-3.5 minutes, the material line is 1900-2100 mm, the furnace top temperature reaches a maximum of 450-480℃, and the heat load increases by 3000×10⁻⁶. 7 When the speed is J / h, it is determined to be a secondary pipeline stroke; When the pipeline duration is 3.5-8 minutes, the material line is 2100-2500 mm, the furnace top temperature reaches a maximum of 480-660℃, and the heat load increases by 4500×10⁻⁶. 7 When the J / h of the air outlet fluctuates, it is determined to be a third-level duct stroke. In one embodiment, during the first stage, when in the primary duct travel, the airflow is reduced to 5600-5700 m³ / h. 3 / min, control the differential pressure target value <185kPa; maintain oxygen enrichment flow rate at 23000m 3 / h remains unchanged; hourly pulverized coal injection rate reduced to 56-58 t / h; blower humidity maintained at 12 g / m³ 3 The air temperature was kept constant at 1170℃; 1 ton of ore was removed to reduce the load on the material column; 2 tons of coke were added to the furnace for reheating to compensate for the heat loss of the downward material column in the furnace.
[0012] In one embodiment, during the first stage, when in the secondary duct travel, the airflow is reduced to 5400-5500 m³ / h. 3 / min, control the pressure difference target value <183kPa; reduce the oxygen enrichment flow rate to 22000m 3 / h; Hourly pulverized coal injection rate remains unchanged at 58t / h; Blower air humidity remains unchanged at 12g / m³ 3 The blast temperature was kept constant at 1170℃; 2t of ore was removed to reduce the load on the feed column; 3t of coke was added to the furnace for reheating, along with 0.6t of silica to improve the fluidity of slag and iron.
[0013] In one embodiment, during the first stage, when in the third-stage duct travel, the airflow is rapidly reduced to 5200-5300 m³ / h. 3 / min, control the differential pressure target value <181kPa; reduce the oxygen enrichment flow rate to 21000m 3 / h; the hourly pulverized coal injection rate was reduced to 56t / h; the blast humidity was reduced to 10g / m³; the blast temperature was maintained at 1170℃; 3t of ore was removed to minimize the load on the material column; 5t of coke was added to the furnace for reheating, along with 1t of silica, which significantly improved the fluidity of slag and iron.
[0014] In one embodiment, in the first stage, the tapping nozzle is drilled to shorten the tapping interval, increase the tapping frequency, ensure smooth discharge of slag and iron, and avoid slag and iron accumulation in the hearth, which would increase the load on the feed column.
[0015] In one embodiment, in the second stage, during the first hour, the reduced air volume is maintained, the blast humidity is reduced, and the blast temperature is increased to compensate for the heat in the hearth. The ore batch is kept in a state of ore withdrawal to reduce the load on the material column. The tapping hole is maintained in front of the furnace to maintain a normal tapping interval and ensure that slag and iron are discharged in a timely manner. During the second hour, all operating parameters from the first hour were kept unchanged, and data on air pressure, differential pressure, and furnace top temperature were continuously collected to confirm that the furnace condition was stable and that there were no signs of pipeline travel recurrence. In the third hour, after the physical heat of the molten iron recovers, the blast humidity is increased, the blast temperature is gradually reduced, and the hourly pulverized coal injection rate is gradually decreased to avoid the heat accumulation after the coke reaches the tuyeres. The blast volume is maintained, and the ore batch gradually recovers. The drilling taphole in front of the furnace is expanded, and overlapping tapping operations are started to accelerate the slag and iron discharge speed. Hours 4-6: Maintain stable blast humidity and constant blast temperature to prevent overheating of the furnace; reduce pulverized coal injection rate in advance to avoid heat accumulation after coke replenishment reaches the tuyeres; if the pressure differential shows signs of rising, reduce the blast rate slightly by 3-5 kPa at a time to ensure the material rate remains stable at over 7 batches / hour; ore batches recover steadily and heat load gradually decreases. Hours 7-8: Gradually increase the humidity of the blower, and increase the air volume and oxygen enrichment flow rate. Observe for 30 minutes or more after each adjustment. Fine-tune the material distribution matrix to increase the ore-coke angle difference by 2-4°, increase the proportion of central coke by 10-15%, and optimize the coal gas flow distribution pattern. 9th hour: All parameters gradually returned to the normal smelting benchmark range, the ore batch returned to normal, and all indicators of molten iron returned to normal levels.
[0016] In one embodiment, during the first and second stages, the adjusted airflow must not remain below 5550 m³ / h for an extended period. 3 / min, to ensure basic blast energy and maintain basic air permeability of the material column in the furnace.
[0017] In one embodiment, during the first and second stages, the interval between each air injection is no less than 5 to 6 minutes, and the air injection amplitude each time does not exceed 300 m. 3 / min, and the change in air pressure after adding air must not exceed 20 kPa.
[0018] In one embodiment, in the first and second stages, sufficient hearth heat is a prerequisite for all operations, with the physical heat of molten iron ≥1510°C.
[0019] In one embodiment, if the air permeability index is >100 in the first and second stages, the air supply operation is immediately suspended, the current air volume level is maintained, and the air supply process is continued after the air permeability of the material column is improved to a reasonable range.
[0020] In one embodiment, in the first and second stages, the oxygen enrichment recovery rhythm is synchronized with the air volume recovery rhythm, and the linkage between the oxygen enrichment rate and the pulverized coal ratio follows the principle that for every 10 kg / t increase in the pulverized coal ratio, the oxygen enrichment rate increases by 0.2% to 0.3%.
[0021] In one embodiment, during the first and second phases, the ore batch adjustment and air volume recovery are synchronized, with the air volume increasing by 100 m³ / s. 3 / min, the ore batch recovers by 0.5 to 1 t accordingly, to avoid the ore batch recovering too quickly and increasing the load on the material column.
[0022] In summary, the present invention has the following beneficial effects: This invention enables precise hierarchical control of pipeline travel: Based on the pipeline duration, this solution combines the material line, furnace top temperature, and heat load quantification thresholds to divide the pipeline travel into three standard response levels, matching precise quantified operating parameters. This effectively solves the problems of traditional handling methods relying on foreman experience and rough operation, and can quickly suppress the development of pipeline airflow and prevent the furnace condition from deteriorating continuously.
[0023] This invention constructs a dual guarantee mechanism of "one core, six linkages, and one guarantee" for multi-parameter coordination and furnace temperature baseline: using differential pressure as the core control criterion, it coordinates and controls six in-furnace parameters, including air volume, oxygen enrichment, pulverized coal injection, blast humidity, blast temperature, and ore batch, while simultaneously implementing slag and iron discharge guarantee measures in front of the furnace. It establishes a linkage and coupling logic between parameters, and simultaneously lowers oxygen enrichment, pulverized coal injection, and ore batch during the air reduction phase, in conjunction with blast humidity adjustment and coke reheating. At the same time, it takes "rather reduce air volume than let the furnace cool down" as a rigid operating baseline, setting a 1480℃ furnace temperature melting and cutting-off mechanism. It adjusts all parameters on the premise of sufficient furnace hearth heat, taking into account both the repair of the material column permeability and the stability of furnace hearth heat. This not only avoids large fluctuations in furnace temperature caused by the adjustment of a single parameter, but also fundamentally eliminates the risk of serious accidents such as furnace cooling and furnace hearth freezing.
[0024] This invention pioneers an integrated collaborative management and control model for both inside and outside the furnace: it innovatively incorporates the slag and iron removal operation in front of the furnace into the core system of pipeline handling. Based on the differentiated needs of the pipeline handling and recovery stages, it matches the diameter of the tap hole drill bit, the iron removal interval, and the timing of overlapping iron removal, so as to promptly remove the slag and iron accumulated in the hearth, improve the permeability of the material column from the bottom, and eliminate the root cause of pipeline recurrence. This invention significantly reduces the probability of secondary pipeline failures: it sets up a phased gradient recovery strategy lasting up to 9 hours, which closely matches the actual smelting cycle of the coke column descending from the furnace throat to the tuyeres. It strictly controls the recovery range and observation time of air volume, oxygen enrichment, pulverized coal injection, and ore batch. It uses stable pressure difference as a prerequisite for increasing air volume and uses the decline in heat load as a verification standard for furnace condition recovery. It smoothly repairs the furnace thermal regime and gas flow distribution, effectively avoiding secondary pipeline failures induced by excessively rapid air increase.
[0025] This invention eliminates all downtime losses and offers significant safety and economic benefits: throughout the entire handling and recovery process, the blast furnace maintains continuous smelting without the need for downtime treatment, thus avoiding unplanned downtime losses caused by pipeline deterioration; at the same time, the 1480℃ furnace temperature melting and cutting-off mechanism provides a safety net, preventing serious accidents such as furnace cooling and hearth freezing from the operational rules, significantly improving the safety redundancy of abnormal handling, and greatly reducing losses from accidental production stoppages.
[0026] This invention is highly reproducible and easy to promote in the industry: all operating parameters are derived from industrial practice verification in large blast furnaces, the standards are clear and easy for work teams to implement uniformly, and can be directly converted into standardized operation manuals for blast furnace positions, or embedded into the blast furnace automated control system to achieve intelligent control, adapting to the pipeline stroke handling needs of various large and medium-sized blast furnaces. Detailed Implementation
[0027] The present invention will now be described in detail with reference to the embodiments.
[0028] This invention proposes a 3000 m 3 A rapid recovery method for the piping stroke of a blast furnace, applicable to furnaces with a volume of 3000 m³. 3 A large blast furnace with a coke load of 4.9 t / t and a normal smelting baseline operating parameters of 5700-5800 m³ / h. 3 / min, pressure difference <188kPa, oxygen enrichment flow rate 23000m 3 / h, hourly pulverized coal injection rate 59t / h, blast humidity 10~13g / m 3 Air temperature 1170℃, heat load <8000×10 7 J / h, physical heat of molten iron 1510~1540℃, silicon content of molten iron 0.3%~0.5%.
[0029] The specific operation of this invention is as follows.
[0030] Phase 1: Tiered and coordinated emergency response for pipeline routes.
[0031] In the first phase, changes in air pressure and differential pressure are the core control criteria. Three response levels are established based on pipeline duration and associated operating conditions. Each level precisely matches seven in-furnace coordinated parameters: air volume, oxygen enrichment, pulverized coal injection, blast humidity, air temperature, coke reheating, and ore batch adjustment. Corresponding slag and iron discharge control standards are simultaneously implemented to quickly curb the development of pipeline airflow. During the handling process, general control rules are followed: differential pressure changes are used as the core criterion for determining the extent of air reduction, reducing airflow until the pipeline phenomenon is completely eliminated; oxygen enrichment and air volume are synchronized to reduce blast kinetic energy; pulverized coal injection is strictly matched to furnace temperature levels to avoid exacerbating furnace turbulence; ore batches are simultaneously reduced to alleviate the load on the material column; and the material distribution matrix is adjusted in a timely manner to guide the gas flow, thus controlling the pipeline's trajectory from multiple dimensions.
[0032] Phase 2: Gradual recovery operation performed hourly after pipeline elimination.
[0033] In the second stage, after the pipeline travel characteristics completely disappeared, the core references were the recovery status of the material line, furnace temperature level, permeability index, and heat load change trend. Six furnace parameters, including air volume, oxygen enrichment, pulverized coal injection, blast humidity, blast temperature, and ore batch, were adjusted in a step-by-step manner at nine time nodes. The adjustment range and observation interval of the parameters were strictly controlled. The coordinated recovery logic of "air volume first, oxygen enrichment second, pulverized coal injection matching, humidity and temperature adjustment, ore batch follow-up, pressure difference control, heat load verification, and furnace temperature bottoming out" was followed to gradually restore the furnace thermal regime and material column permeability, rebuild a reasonable gas flow distribution of "strong center and stable edge", and ensure that the furnace condition returned to normal smelting state smoothly. A 1480℃ furnace temperature melting mechanism was set up throughout the recovery process. If the physical heat of molten iron dropped below 1480℃, all blast and oxygen enrichment operations were immediately suspended, and coke was added first for supplemental heating. After the furnace temperature trend rebounded, the gradient recovery plan was continued.
[0034] In the first stage, when the pipeline duration is 1-2 minutes, the material line is 1500-1900 mm, the furnace top temperature reaches a maximum of 380-450℃, and the heat load increases by 1800×10⁻⁶. 7 When J / h, it is determined to be a first-level pipeline stroke; When the pipeline duration is 2-3.5 minutes, the material line is 1900-2100 mm, the furnace top temperature reaches a maximum of 450-480℃, and the heat load increases by 3000×10⁻⁶. 7 When the speed is J / h, it is determined to be a secondary pipeline stroke; When the pipeline duration is 3.5-8 minutes, the material line is 2100-2500 mm, the furnace top temperature reaches a maximum of 480-660℃, and the heat load increases by 4500×10⁻⁶. 7 When the working condition of the air outlet fluctuates (J / h), it is determined to be a third-level pipeline stroke.
[0035] Furthermore, in the first stage, when in the primary duct travel, the air volume is reduced to 5600-5700 m³ / h. 3 / min, control the differential pressure target value <185kPa (e.g., 183-185kPa); maintain oxygen enrichment flow rate at 23000m 3 / h remains unchanged; hourly pulverized coal injection rate reduced to 56-58 t / h; blower humidity maintained at 12 g / m³ 3 The air temperature was kept constant at 1170℃; 1 ton of ore was removed to reduce the load on the material column; 2 tons of coke were added to the furnace for reheating to compensate for the heat loss of the downward material column in the furnace.
[0036] In the first stage, when in the secondary pipeline travel, the air volume is reduced to 5400-5500 m³ / h. 3 / min, control the differential pressure target value <183kPa (e.g., 181-183kPa); reduce the oxygen enrichment flow rate to 22000m 3 / h; Hourly pulverized coal injection rate remains unchanged at 58t / h; Blower air humidity remains unchanged at 12g / m³ 3 The blast temperature was kept constant at 1170℃; 2t of ore was removed to reduce the load on the feed column; 3t of coke was added to the furnace for reheating, along with 0.6t of silica to improve the fluidity of slag and iron.
[0037] In the first stage, when in the third-stage duct travel, the air volume is rapidly reduced to 5200-5300 m³ / h. 3 / min, control the differential pressure target value <181kPa (e.g., 175-181kPa); reduce the oxygen enrichment flow rate to 21000m 3 / h; the hourly pulverized coal injection rate was reduced to 56t / h; the blast humidity was reduced to 10g / m³; the blast temperature was maintained at 1170℃; 3t of ore was removed to minimize the load on the material column; 5t of coke was added to the furnace for reheating, along with 1t of silica, which significantly improved the fluidity of slag and iron.
[0038] In the first stage, drilling the tapping hole shortens the tapping interval, increases the tapping frequency, ensures smooth discharge of slag and iron, and avoids slag and iron accumulation in the hearth, which increases the load on the material column.
[0039] In the second stage, during the first hour, the reduced air volume is maintained, the blast humidity is reduced, and the blast temperature is increased to compensate for the heat in the hearth. The ore batch is kept in a state of ore withdrawal to reduce the load on the material column. The tapping nozzle is maintained in front of the furnace, and the normal tapping interval is maintained to ensure timely discharge of slag and iron. During the second hour, all operating parameters from the first hour were kept unchanged, and data on air pressure, differential pressure, and furnace top temperature were continuously collected to confirm that the furnace condition was stable and that there were no signs of pipeline travel recurrence. In the third hour, after the physical heat of the molten iron recovers, the blast humidity is increased, the blast temperature is gradually reduced, and the hourly pulverized coal injection rate is gradually decreased to avoid the heat accumulation after the coke reaches the tuyeres. The blast volume is maintained, and the ore batch gradually recovers. The drilling taphole in front of the furnace is expanded, and overlapping tapping operations are started to accelerate the slag and iron discharge speed. Hours 4-6: Maintain stable blast humidity and constant blast temperature to prevent overheating of the furnace; reduce pulverized coal injection rate in advance to avoid heat accumulation after coke replenishment reaches the tuyeres; if the pressure differential shows signs of rising, reduce the blast rate slightly by 3-5 kPa at a time to ensure the material rate remains stable at over 7 batches / hour; ore batches recover steadily and heat load gradually decreases. Hours 7-8: Gradually increase the humidity of the blower, and increase the air volume and oxygen enrichment flow rate. Observe for 30 minutes or more after each adjustment. Fine-tune the material distribution matrix to increase the ore-coke angle difference by 2-4°, increase the proportion of central coke by 10-15%, and optimize the coal gas flow distribution pattern. 9th hour: All parameters gradually returned to the normal smelting benchmark range, the ore batch returned to normal, and all indicators of molten iron returned to normal levels.
[0040] Preferably, in the first and second stages, the adjusted air volume should not be lower than 5550 m3 / min for an extended period (generally 30 minutes) to ensure basic blast kinetic energy and maintain the basic permeability of the material column in the furnace.
[0041] Preferably, in the first and second stages, the ventilation operation must follow the principle of "small amplitude and frequent observation," with an interval of no less than 5 to 6 minutes between each ventilation operation, and the amplitude of each ventilation operation not exceeding 300 m. 3 / min, and the change in air pressure after adding air must not exceed 20 kPa, that is, the pressure difference change ≤20 kPa.
[0042] In the first and second stages, sufficient hearth heat is a prerequisite for all operations. The normal range of physical heat of molten iron is 1510-1540℃, with a control line of ≥1510℃. Adhering to the operating principle of "rather reduce blast than let the hearth cool down", a 1480℃ furnace temperature cutoff mechanism is set up. When the physical heat of molten iron continues to be lower than 1480℃ and the downward trend is not stopped, the blasting operation is immediately suspended, the smelting intensity is appropriately reduced, and coke is added simultaneously to replenish the hearth heat. The risk of hearth cooling and freezing is resolutely eliminated to ensure that the slag and iron have good fluidity.
[0043] In both the first and second stages, if the air permeability index is greater than 100, immediately suspend the air supply operation, maintain the current air volume level, and continue the air supply process only after the air permeability of the material column has improved to a reasonable range. The air permeability index corresponds to the blower humidity.
[0044] In both the first and second phases, the tapping operation strictly adheres to industry technical specifications, with the difference in iron quantity not exceeding 10% to 15% of the theoretical iron quantity, and the pass rate for tapping depth and the on-time tapping rate both needing to reach over 90%.
[0045] In the first and second stages, the oxygen enrichment recovery rhythm was synchronized with the air volume recovery rhythm, and the linkage between the oxygen enrichment rate and the pulverized coal ratio followed the following: for every 10 kg / t increase in the pulverized coal ratio, the oxygen enrichment rate increased by 0.2% to 0.3%.
[0046] In the first and second phases, the adjustment of the mine batch and the restoration of the ventilation volume are synchronized. For every 100 m³ increase in ventilation volume... 3 / min, the ore batch recovers by 0.5 to 1 t accordingly, to avoid the ore batch recovering too quickly and increasing the load on the material column.
[0047] In the first and second phases, the continuous decline of heat load is used as the core verification indicator for furnace condition recovery. If the heat load does not fall back to within 120% of the normal range, the production should not be increased significantly.
[0048] In the first and second stages, the material distribution matrix can be finely adjusted during the recovery stage to appropriately increase the ore-coke angle difference and the proportion of central coke, continuously suppress excess gas flow at the edge, and consolidate the reasonable coal and gas flow distribution pattern.
[0049] This invention comprehensively determines the severity of pipeline travel by collecting high-frequency real-time data on blast furnace cold air flow, differential pressure, furnace top temperature, heat load, material line depth, and furnace top gas distribution, combined with airflow distribution patterns observed by a furnace top camera. Using pipeline duration as the core grading criterion, and matching quantitative thresholds for operating conditions, pipeline travel is divided into three levels: Level 1, Level 2, and Level 3. Differentiated collaborative operations are implemented according to each level. After pipeline travel is eliminated, operating parameters are gradually adjusted back according to a preset hourly rhythm, constructing a multi-parameter collaborative recovery system that uses differential pressure as the core criterion, air volume as the leading parameter, six furnace parameters linked, and slag and iron discharge simultaneously guaranteed, thus achieving stable furnace condition recovery.
[0050] This invention uses changes in wind pressure and differential pressure as the core control basis, constructing two core operational logics: "tiered collaborative emergency response + hourly gradient recovery." Specifically, it divides the response level into three levels based on the duration of pipeline disruption, matching quantitative linkages with wind reduction, oxygen enrichment adjustment, pulverized coal injection reduction, blast humidity adjustment, coke reheating, and ore batch collaborative operation, while simultaneously implementing differentiated slag and iron management strategies before the furnace. After the pipeline disruption is eliminated, a 9-hour gradient recovery plan is implemented, systematically adjusting six major smelting parameters: wind volume, oxygen enrichment, pulverized coal injection, blast humidity, blast temperature, and ore batch, gradually restoring the furnace thermal regime and the permeability of the burden, thus fundamentally preventing the recurrence of pipeline disruption. This invention takes sufficient furnace temperature as a rigid bottom line, adhering to the principle of "rather reduce wind than let the furnace cool down" throughout the process, setting a 1480℃ furnace temperature melting mechanism, integrating multi-process collaborative linkage mechanisms, maintaining continuous blast furnace smelting without interruption, with a high degree of standardized operation, significantly shortening the duration of pipeline anomalies, and systematically preventing serious accidents such as furnace cooling, hearth freezing, and unplanned shutdowns, ensuring the long-term stable operation of the blast furnace.
[0051] This invention employs a standardized operating model of "tiered collaborative emergency response + hourly gradient recovery" to precisely match the development stage of pipeline travel. It coordinates and regulates the air supply system, heating system, pulverized coal injection oxygen enrichment system, blast humidity system, and furnace slag and iron discharge system. While maintaining continuous blast furnace smelting, it rapidly suppresses high-speed pipeline airflow, eliminates pipeline travel defects, and smoothly restores furnace conditions to normal levels, effectively preventing pipeline travel recurrence. At the same time, it firmly safeguards the furnace temperature safety baseline by setting a 1480℃ furnace temperature melting mechanism. Through the linkage of coke replenishment and blast reduction, it ensures sufficient heat in the hearth, and eliminates serious accidents such as furnace cooling and hearth freezing from the operational rules, minimizing production losses and safety risks caused by abnormal furnace conditions.
[0052] The technical solution of the present invention will be described below with reference to specific embodiments. Example 1
[0053] A steel plant 3200 m 3 A single-stage blast furnace with a coke load of 4.9 t / t and normal smelting baseline parameters of 5700–5800 m³ / h. 3 / min, pressure difference <188kPa, oxygen enrichment flow rate 23000 m 3 / h, hourly pulverized coal injection rate 59 t / h, blast air humidity 10~13g / m 3 Air temperature 1170℃, heat load <8000×10 7 J / h, physical heat of molten iron 1510~1540℃.
[0054] After the blast furnace shift started, abnormal conditions such as fluctuating air pressure and increasing differential pressure occurred. Based on the data on furnace top temperature distribution and heat load changes, it was determined that the problem was caused by a primary pipeline stroke. The pipeline duration was approximately 1.5 minutes, the material level was approximately 1750 mm, the highest furnace top temperature reached 380℃, and the heat load increase was approximately 1800 × 10⁻⁶. 7 J / h.
[0055] The specific steps for processing using the method described in this invention are as follows: Step 1: Collaborative emergency response for primary pipeline travel.
[0056] In accordance with the Level 1 pipeline response standard, immediately implement parameter adjustment operations: reduce the air volume to 5700 m³ / h. 3 / min, control the differential pressure target value <185 kPa; maintain oxygen enrichment flow rate at 23000 m³ / min. 3 / h remains unchanged; hourly pulverized coal injection rate is reduced from 59 t / h to 58 t / h; blast air humidity remains at 12 g / m 3 The blast temperature was maintained at 1170℃; 1 ton of ore was removed to reduce the load on the charge column; 2 tons of coke were added to the furnace for reheating to compensate for the heat loss of the descending charge column. The entire process strictly adhered to furnace temperature priority control, with real-time monitoring of the physical and thermal changes of the molten iron to ensure that the furnace temperature did not fall below the safe threshold of 1480℃.
[0057] Synchronous control measures in front of the furnace: Use a φ58mm drill bit to drill the iron tapping hole, shorten the iron tapping interval to 80% of the normal level, increase the iron tapping frequency, ensure smooth discharge of slag and iron, and avoid slag and iron accumulation in the hearth, which would increase the load on the material column.
[0058] Continuously observe the changes in furnace conditions: the fluctuation range of air pressure gradually narrows, the pressure difference tends to stabilize, and the furnace top temperature and heat load gradually decrease; after about 18 minutes, the pipeline travel characteristics completely disappear, and the furnace enters the hourly gradient recovery stage.
[0059] Step 2: Gradient recovery operation performed hourly after pipeline elimination.
[0060] After the pipeline is cleared, the parameters are returned step by step in strict accordance with the hourly recovery rhythm. The operation execution standards for each node are as follows: Hour 1: Airflow maintained at 5700m 3 / min, blower humidity reduced to 9g / m 3 The blast temperature was increased to 1180℃ to compensate for the heat in the hearth, the hourly coal ratio was controlled within 180kg / t, the ore batch was kept in a state of ore withdrawal to reduce the load on the material column, and a φ58mm drill bit was continuously used in front of the furnace to maintain a normal iron tapping interval and ensure timely discharge of slag and iron.
[0061] Hour 2: Maintain all operating parameters unchanged from Hour 1, continuously collect data on air pressure, differential pressure, and furnace top temperature, and confirm that there are no signs of pipeline travel recurrence.
[0062] Hour 3: After the molten iron's physical heat rises to 1520℃, gradually increase the blast humidity to 15g / m³. 3 The air temperature was gradually reduced to 1170℃, and the hourly coal injection rate was gradually decreased to avoid heat accumulation after the coking coal reached the tuyere area. The minimum air volume was maintained at 5550 m³ / h. 3 / min, the ore batch began to gradually recover; the drill bit in front of the furnace was replaced with a φ60mm large diameter drill bit, and the overlapping tapping operation was started to speed up the slag and iron discharge.
[0063] Hours 4-6: Blower humidity stabilizes at 15-20 g / m³ 3 Within the range, the blast temperature is kept constant at 1160℃ to prevent the furnace temperature from overheating; the amount of coal injected is reduced in advance to avoid heat accumulation after the coke is added to the tuyere area; if the pressure difference shows signs of rising, the blast is reduced slightly by 3 kPa at a time to ensure that the material rate is stable at more than 7 batches / hour; the ore batch is steadily restored to more than 90% of the normal level, and the heat load is gradually reduced to less than 120% of the normal range.
[0064] 7-8 hours: The humidity of the blower gradually increases to the upper limit of 20g / m³. 3 Steadily and gradually increase the air volume and oxygen enrichment flow rate, and synchronize the recovery rhythm of oxygen enrichment with the air volume. Observe for more than 30 minutes after each adjustment, and proceed with the next operation only after confirming that the pressure difference has not rebounded and the heat load continues to fall. The coal injection volume is adjusted back in sync with the increase of oxygen enrichment rate. The material distribution matrix is finely adjusted to expand the ore-coke angle difference by 2° and increase the proportion of central coke by 10% to continuously guide the central coal flow.
[0065] From the 9th hour onwards: all parameters gradually returned to the normal smelting baseline range, the ore batch size recovered to 88t; the hourly coal ratio stabilized at 165kg / t; and the air volume recovered to 5800m³. 3 / min; heat load drops to 7500×10 7 J / h; the physical heat of molten iron is stable at around 1520℃, the silicon content is stable at around 0.4%; the pressure difference is stable within 185kPa; the furnace condition has been fully restored to the normal smelting level.
[0066] No ventilation was interrupted during the entire pipeline treatment process. The pipeline movement was effectively suppressed within 18 minutes, and the furnace condition was restored to normal in a total of about 8 hours. The lowest physical heat of the molten iron during the entire treatment process was 1512℃, which was always higher than the melting threshold of 1480℃, and there were no significant fluctuations in furnace temperature. Compared with the traditional single ventilation reduction treatment method, the duration of the abnormality was shortened by nearly 40%, and no secondary failures such as pipeline recurrence, slag filling of the tuyeres, and furnace cooling occurred.
[0067] The cause of this example is: the coal injection rate was not adjusted in time before the end of the middle shift, resulting in a higher actual fuel ratio in the furnace and a stronger coal flow distribution; after the night shift took over, the upward trend of the furnace temperature was not accurately identified, and the high coal injection rate was maintained. After the furnace was changed, the blast kinetic energy fluctuated briefly, and the resistance of the local airflow channel continued to decrease, which eventually triggered the first-stage pipeline stroke.
[0068] The handling logic in this embodiment is as follows: the primary pipeline exhibits a minor anomaly, and the core of the handling is "precise air control and minor adjustments": by appropriately reducing airflow and lowering the pulverized coal injection rate, the impact force of the local high-speed airflow is quickly reduced; a small amount of supplemental heating is used to balance the heat loss of the downward-flowing charge column in the furnace; and conventional iron tapping at the furnace front ensures normal slag and iron discharge, preventing further deterioration of the charge column's permeability. Due to the early timing of the handling and the precise parameter adjustments, the pipeline travel was suppressed within a short period of time.
[0069] This embodiment does not blindly reduce the air volume significantly. Through the coordinated fine-tuning of air volume, pulverized coal injection, and ore batch, the development of pipelines is curbed without affecting normal smelting. The amount of coke replenishment is precisely adapted to the changes in furnace temperature, and the heat is compensated by the temporary increase in air temperature, so as not to cause large fluctuations in furnace temperature. Example 2
[0070] The 3200m as described in Example 1 3 The blast furnace experienced abnormal conditions during the transition period between high and low coal feed rates, including persistently high blast pressure and an increasing pressure differential. On-duty personnel attempted to reduce blast temperature and decrease blast volume, but the measures were insufficient, and the abnormal conditions continued to worsen. Based on real-time monitoring data, the problem was determined to be a secondary pipeline malfunction, lasting approximately 3.5 minutes, with a feed line length of approximately 1900 mm, a maximum furnace top temperature of 480°C, and a heat load increase of approximately 3000 × 10⁻⁶. 7 J / h.
[0071] The specific steps for processing using the method described in this invention are as follows: Step 1: Coordinated Emergency Response for Secondary Pipeline Flow Immediately implement the secondary pipeline coordinated operation parameters: reduce the air volume to 5500m³. 3 / min, control the differential pressure target value <183kPa; oxygen enrichment flow rate from 23000m 3 / h reduced to 22000m 3 / h; Hourly pulverized coal injection rate remains unchanged at 58t / h; Blower air humidity remains unchanged at 12g / m³ 3 The blast temperature was maintained at 1170℃; 2t of ore was removed to reduce the load on the feed column; 3t of coke was added to the furnace for reheating, along with 0.6t of silica to improve the fluidity of the slag and iron. The process adhered to the principle of prioritizing furnace temperature. When there was a conflict between differential pressure control and furnace temperature reduction, priority was given to ensuring sufficient heat in the hearth.
[0072] Synchronous upgrade and control measures at the furnace front: Maintain the φ58mm drill bit for drilling the iron tapping hole, increase the frequency of iron tapping, and shorten the iron tapping interval to 70% of the normal interval; when the slag and iron accumulation exceeds 50t, open the next iron tapping hole in advance to ensure timely discharge of slag and iron.
[0073] Continuous monitoring of furnace conditions: After the air volume is reduced, the pressure difference gradually decreases, and the upward trend of furnace top temperature and heat load is curbed; after about 25 minutes, the pipeline travel phenomenon is completely eliminated, and the furnace enters the hourly gradient recovery stage.
[0074] Step 2: Gradient recovery operation by hour after pipe removal Strictly follow the recovery rhythm standard to execute parameter callbacks. The specific operation is as follows: Hour 1: Maintain airflow at 5500m 3 / min, blower humidity reduced to 9g / m 3 The upper limit of the blast temperature is controlled at 1185℃ to compensate for the heat of the hearth, the hourly coal ratio is controlled within 182kg / t, and the ore batch is kept in the state of ore withdrawal; φ58mm drill bit is continuously used in front of the furnace to maintain the pace of iron tapping.
[0075] Hour 2: Keep all operating parameters unchanged from Hour 1, and continue to observe the changing trends of air pressure, differential pressure, and heat load to confirm that the furnace condition is stable.
[0076] Hour 3: After the molten iron's physical heat rises to 1515℃, the blast ventilation humidity is gradually increased to 15g / m³. 3 The air temperature gradually decreased to 1170℃, and the hourly pulverized coal injection rate was gradually reduced to avoid coking. The minimum air volume was maintained at 5550 m³ / h. 3 / min, the ore batch began to gradually recover; the furnace front was replaced with a φ63mm large-diameter drill bit, and overlapping iron tapping operation was performed.
[0077] Hours 4-6: Blower humidity stabilizes at 15-20 g / m³ 3 Within the range, the air temperature is kept constant at 1160℃; the amount of pulverized coal is reduced in advance to avoid the arrival of coking coal; when the pressure difference is too high, the air volume is reduced slightly by 4 kPa at a time to ensure that the material rate is stable at more than 7 batches / hour; the ore batch is steadily recovering and the heat load is gradually decreasing.
[0078] 7-8 hours: The humidity of the blower gradually increases to the upper limit of 20g / m³. 3 Steadily and slightly increase air volume and oxygen enrichment flow, and observe for more than 30 minutes after each adjustment; fine-tune the material distribution matrix to increase the ore-coke angle difference by 3°, increase the central coke ratio by 12%, and optimize the coal gas flow distribution pattern.
[0079] From the 9th hour onwards: all parameters gradually returned to the normal smelting baseline range, and the ore batch returned to normal; the hourly coal ratio stabilized at 168 kg / t; and the air volume recovered to 5800 m³ / t. 3 / min; heat load drops to 7800×10 7 J / h; All indicators of molten iron have returned to normal levels.
[0080] No ventilation was interrupted during the entire pipeline handling process. The pipeline travel was brought under control within 25 minutes, and the total time to restore the furnace to normal was approximately 8.5 hours. The lowest physical heat of the molten iron during the entire handling process was 1508℃, which did not trigger the 1480℃ melting mechanism. There were no problems such as large fluctuations in furnace temperature or poor slag and iron discharge. The pipeline travel did not recur afterward, and there was no risk of furnace cooling.
[0081] The cause of this embodiment is: during the transition period between high and low coal volumes, the distribution pattern of gas in the furnace is temporarily unbalanced; although the on-duty personnel identified the abnormally high air pressure, the reduction in air temperature and air volume was insufficient, and the gas imbalance continued to worsen, gradually developing into a secondary pipeline flow.
[0082] The handling logic of this embodiment is as follows: the secondary pipeline is in a moderate abnormality, and the core of the handling is "appropriate reduction of airflow and parameter linkage": while reducing airflow, the oxygen enrichment and pulverized coal injection are adjusted in a coordinated manner, starting from the two dimensions of blast kinetic energy and hearth thermal regime, to weaken the development momentum of pipeline airflow; with appropriate amount of coke and silica supplementation, the slag and iron flowability is improved; the iron tapping frequency in front of the furnace is increased to avoid slag and iron accumulation and deterioration of the material column permeability, and the pipeline development is controlled in a multi-dimensional coordinated manner.
[0083] This embodiment establishes a linkage adjustment logic for air volume, oxygen enrichment, pulverized coal injection, and ore batch, avoiding furnace temperature fluctuations caused by simply reducing air volume; the addition of silica effectively improves slag-iron fluidity, and combined with increased iron tapping at the furnace front, creates conditions for the subsequent stable recovery of furnace conditions. Example 3
[0084] Same as in Example 1, 3200m 3 In the first-stage blast furnace, a malfunction in the furnace taphole opening machine caused delays in taphole drilling, extending the actual tapping interval by 30 minutes compared to the normal interval. A total of one hour was spent without proper slag and iron discharge, resulting in a large accumulation of slag and iron in the hearth and a sharp deterioration in the permeability of the charge column, inducing severe pipe travel. The pipe travel lasted approximately 8 minutes, with a charge level of approximately 2100 mm. The highest furnace top temperature reached 660°C, and the heat load increased by approximately 4500 × 10⁻⁶. 7 J / h, the working condition of the air outlet fluctuated significantly.
[0085] The specific steps for processing using the method described in this invention are as follows: Step 1: Three-level pipeline coordinated emergency response In accordance with the Level 3 pipeline response standard, immediately execute parameter adjustment operations: rapidly reduce the air volume to 5300 m³ / h. 3 / min, control the differential pressure target value <181kPa; oxygen enrichment flow rate from 23000m 3 / h reduced to 21000m 3 / h; Hourly pulverized coal injection rate reduced to 56t / h; Blower air humidity reduced to 10g / m 3 The blast temperature was maintained at 1170℃; 3 tons of ore were removed to minimize the load on the feed column; 5 tons of coke were added to the furnace for reheating, along with 1 ton of silica, which significantly improved the fluidity of the slag and iron. The process strictly adhered to the bottom-line principle of furnace temperature control. Due to the heavy piping and significant reduction in blast, the risk of furnace temperature decline was high. Priority was given to ensuring adequate coke replenishment, while simultaneously compensating for heat loss by controlling the upper limit of blast temperature, resolutely maintaining the bottom line of preventing the furnace from cooling down.
[0086] Simultaneously, emergency measures were taken at the furnace front: the tapping machine malfunction was quickly repaired, the tapping hole was drilled with a φ58mm drill bit, and the overlapping tapping mode was immediately activated to minimize the tapping interval; the slag and iron accumulation was strictly monitored, and when the slag and iron accumulation exceeded 50t, the tapping hole diameter was appropriately enlarged to accelerate the slag and iron discharge speed.
[0087] Continuous and close monitoring of the furnace condition: The fluctuation range of air pressure gradually narrows, the pressure difference decreases accordingly, and the upward trend of furnace top temperature and heat load is curbed; after about 32 minutes, the pipeline travel characteristics completely disappear, and the furnace enters the hourly gradient recovery stage.
[0088] Step 2: Gradient recovery operation by hour after pipe removal Given the severity of this pipeline incident, the parameter recovery process will be slowed down appropriately, with the following procedures implemented at each time point: Hour 1: Airflow maintained at 5300m 3 / min, blower humidity reduced to 9g / m 3 The upper limit of the blast temperature is controlled at 1185℃, the hourly coal ratio is controlled within 180kg / t, and the maximum ore withdrawal range is maintained in the ore batch; the overlapping iron tapping rhythm is maintained in front of the furnace, and the slag and iron discharge is closely monitored.
[0089] Hour 2: Maintain all operating parameters unchanged from Hour 1, continuously monitor air pressure, differential pressure, heat load and furnace top airflow distribution data, and confirm that there are no signs of pipeline recurrence.
[0090] Hour 3: After the molten iron's physical heat rises to 1520℃, the blast air humidity is gradually increased to 15g / m³. 3 The air temperature gradually decreased to 1170℃, and the hourly pulverized coal injection rate was gradually reduced to avoid coking. The minimum air volume was maintained at 5550 m³ / h. 3 / min, the ore batch began to gradually recover; the furnace head was replaced with a φ63mm large-diameter drill bit, and iron was continuously tapped in overlapping manner.
[0091] Hours 4-6: Blower humidity stabilizes at 15-20 g / m³ 3Within the range, the air temperature is kept constant at 1160℃; the amount of pulverized coal is reduced in advance to avoid the arrival of coke replenishment; when the pressure difference is too high, the air is reduced slightly by 5 kPa at a time to ensure that the material speed is stable at more than 7 batches / hour; the ore batches are steadily recovering and the heat load is gradually decreasing; the material distribution matrix is slightly adjusted to increase the ore-coke angle difference by 4° and increase the proportion of central coke by 15% to enhance the airflow guidance effect.
[0092] 7-8 hours: The humidity of the blower gradually increases to the upper limit of 20g / m³. 3 Steadily and gradually increase the air volume and oxygen enrichment flow rate, and observe for more than 30 minutes after each adjustment; track the furnace temperature change data after the coke replenishment reaches the tuyere area in real time, and adjust the coal injection volume and air temperature in a timely manner to prevent the heat accumulation from causing the furnace temperature to overheat.
[0093] From the 9th hour onwards: all parameters gradually returned to the normal smelting baseline range, and the ore batch returned to normal; the hourly coal ratio stabilized at 170 kg / t; and the air volume recovered to 5800 m³ / t. 3 / min; heat load drops to 7600×10 7 J / h; All indicators of molten iron have returned to normal levels.
[0094] No ventilation shutdown occurred during the entire pipeline handling process. The pipeline travel was effectively suppressed within 32 minutes, and the total time to restore the furnace to normal was approximately 9 hours. The lowest physical heat of the molten iron during the entire handling process was 1498℃, which was close to but did not fall below the 1480℃ melting threshold. There was no risk of furnace cooling or hearth freezing. Subsequently, a comprehensive inspection and rectification of key equipment such as the furnace opening machine was organized, and the furnace equipment inspection and maintenance process was optimized to avoid abnormal slag and iron discharge due to equipment failure, thus eliminating the inducing factors of pipeline travel at the root.
[0095] The cause of this embodiment is: a malfunction of the furnace tapping machine, a delay in the tapping operation, an actual tapping interval that is 30 minutes longer than the normal interval, a total of 1 hour without normal slag and iron discharge, a large accumulation of slag and iron in the hearth, a sharp deterioration in the permeability of the material column, a significant reduction in the resistance of the local airflow channel, and ultimately, a severe pipeline stroke.
[0096] The handling logic of this embodiment is as follows: the third-level pipeline is in serious abnormality, and the core of the handling is "rapid flow control and external furnace coordination": immediately reduce the wind and oxygen enrichment, significantly reduce the blast energy, and weaken the impact force of the pipeline airflow; cooperate with a large amount of coke and silica to quickly increase the hearth heat and improve the slag and iron fluidity; urgently handle the equipment failure in front of the furnace, start the overlapping iron tapping mode, and maximize the speed of slag and iron discharge, and start from the top and bottom at the same time to quickly curb the pipeline development.
[0097] In this embodiment, the furnace interior and exterior work together to make slag and iron discharge disposal a core means of pipeline management; seven furnace interior parameters are adjusted synchronously, with the magnitude precisely matching the pipeline development level, thus avoiding abnormal and continuous deterioration.
[0098] The pipeline treatment effect data of Examples 1-3 were statistically analyzed and compared with the average level of the traditional single air reduction treatment mode. The results are shown in Table 1 below: Table 1. Effects of Examples 1-3 and Traditional Treatment Modes
[0099] As can be seen from the data in the table, after adopting the method described in this invention, the suppression time and furnace condition recovery time of different levels of pipeline stroke are significantly shorter than those of the traditional treatment mode; there is no interruption of ventilation or pipeline recurrence throughout the process, the furnace temperature fluctuation is significantly smaller, the minimum physical heat of molten iron is always maintained above the melting threshold of 1480℃, the furnace cooling accident rate is 0, the increase in fuel consumption is greatly reduced, and the treatment effect is stable.
[0100] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A 3000m 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, The operation is as follows: Phase 1: Based on changes in wind pressure and differential pressure, three response levels are defined according to pipeline duration and supporting operating conditions. Each level is precisely matched with seven in-furnace coordinated parameters, including air volume, oxygen enrichment, pulverized coal injection, blast humidity, air temperature, coke reheating, and ore batch adjustment. Corresponding slag and iron discharge control standards are implemented simultaneously to quickly curb the development of pipeline airflow. Phase Two: After the pipeline travel characteristics have completely disappeared, the core references are the recovery status of the material line, furnace temperature level, permeability index, and heat load change trend. The six furnace parameters of air volume, oxygen enrichment, pulverized coal injection, blast humidity, blast temperature, and ore batch are adjusted in a step-by-step manner at nine time nodes. The adjustment range and observation interval of the parameters are strictly controlled to gradually restore the furnace thermal regime and material column permeability, ensuring that the furnace condition returns to normal smelting state smoothly. During the recovery process, if the physical heat of molten iron is <1480℃, all blasting and oxygen enrichment operations are immediately suspended, and coke is added first for supplemental heating. After the furnace temperature trend rises, the gradient recovery plan is continued.
2. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first stage, when the pipeline duration is 1-2 minutes, the material line is 1500-1900 mm, the furnace top temperature reaches a maximum of 380-450℃, and the heat load increases by 1800×10⁻⁶. 7 When J / h, it is determined to be a first-level pipeline stroke; When the pipeline duration is 2-3.5 minutes, the material line is 1900-2100 mm, the furnace top temperature reaches a maximum of 450-480℃, and the heat load increases by 3000×10⁻⁶. 7 When the speed is J / h, it is determined to be a secondary pipeline stroke; When the pipeline duration is 3.5-8 minutes, the material line is 2100-2500 mm, the furnace top temperature reaches a maximum of 480-660℃, and the heat load increases by 4500×10⁻⁶. 7 When the working condition of the air outlet fluctuates (J / h), it is determined to be a third-level pipeline stroke.
3. The 3000m as described in claim 2 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first stage, when in the primary duct travel, the air volume is reduced to 5600-5700 m³ / h. 3 / min, control the differential pressure target value <185kPa; maintain oxygen enrichment flow rate at 23000m 3 / h remains unchanged; hourly pulverized coal injection rate reduced to 56-58 t / h; blower humidity maintained at 12 g / m³ 3 The air temperature was kept constant at 1170℃; 1 ton of ore was removed to reduce the load on the material column; 2 tons of coke were added to the furnace for reheating to compensate for the heat loss of the downward material column in the furnace. When in the secondary pipeline stage, the air volume is reduced to 5400-5500 m³ / h. 3 / min, control the differential pressure target value <183kPa; reduce the oxygen enrichment flow rate to 22000m 3 / h; Hourly pulverized coal injection rate remains unchanged at 58t / h; Blower air humidity remains unchanged at 12g / m³ 3 The blast temperature was kept constant at 1170℃; 2t of ore was removed to reduce the load on the material column; 3t of coke was added to the furnace for reheating, along with 0.6t of silica to improve the fluidity of slag and iron. When in the third-stage duct travel, the air volume is rapidly reduced to 5200-5300 m³ / h. 3 / min, control the differential pressure target value <181kPa; reduce the oxygen enrichment flow rate to 21000m 3 / h; the hourly pulverized coal injection rate was reduced to 56t / h; the blast humidity was reduced to 10g / m³; the blast temperature was maintained at 1170℃; 3t of ore was removed to minimize the load on the material column; 5t of coke was added to the furnace for reheating, along with 1t of silica, which significantly improved the fluidity of slag and iron.
4. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first stage, drilling the tapping hole shortens the tapping interval, increases the tapping frequency, ensures smooth discharge of slag and iron, and avoids slag and iron accumulation in the hearth, which increases the load on the material column.
5. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the second stage, during the first hour, the reduced air volume is maintained, the blast humidity is reduced, and the blast temperature is increased to compensate for the heat in the hearth. The ore batch is kept in a state of ore withdrawal to reduce the load on the material column. The tapping nozzle is maintained in front of the furnace, and the normal tapping interval is maintained to ensure timely discharge of slag and iron. During the second hour, all operating parameters from the first hour were kept unchanged, and data on air pressure, differential pressure, and furnace top temperature were continuously collected to confirm that the furnace condition was stable and that there were no signs of pipeline travel recurrence. In the third hour, after the physical heat of the molten iron recovers, the blast humidity is increased, the blast temperature is gradually reduced, and the hourly pulverized coal injection rate is gradually decreased to avoid the heat accumulation after the coke reaches the tuyeres. The blast volume is maintained, and the ore batch gradually recovers. The drilling taphole in front of the furnace is expanded, and overlapping tapping operations are started to accelerate the slag and iron discharge speed. Hours 4-6: Maintain stable blast humidity and constant blast temperature to prevent overheating of the furnace; reduce pulverized coal injection rate in advance to avoid heat accumulation after coke replenishment reaches the tuyeres; if the pressure differential shows signs of rising, reduce the blast rate slightly by 3-5 kPa at a time to ensure the material rate remains stable at over 7 batches / hour; ore batches recover steadily and heat load gradually decreases. Hours 7-8: Gradually increase the humidity of the blower, and increase the air volume and oxygen enrichment flow rate. Observe for 30 minutes or more after each adjustment. Fine-tune the material distribution matrix to increase the ore-coke angle difference by 2-4°, increase the proportion of central coke by 10-15%, and optimize the coal gas flow distribution pattern. 9th hour: All parameters gradually returned to the normal smelting benchmark range, the ore batch returned to normal, and all indicators of molten iron returned to normal levels.
6. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, During both the first and second phases, the adjusted air volume must not be lower than 5550 m³ for an extended period. 3 / min, to ensure basic blast energy and maintain basic air permeability of the material column in the furnace.
7. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In both the first and second stages, the interval between each air injection should be no less than 5 to 6 minutes, and the air injection range should not exceed 300 m. 3 / min, and the change in air pressure after adding air must not exceed 20 kPa.
8. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first and second stages, sufficient hearth heat is a prerequisite for all operations, with the physical heat of molten iron ≥1510℃.
9. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first and second stages, if the air permeability index is >100, immediately suspend the air supply operation, maintain the current air volume level, and continue the air supply process after the air permeability of the material column improves to a reasonable range.
10. The 3000m as described in claim 1 3 A method for rapid recovery of pipeline stroke in a blast furnace, characterized in that, In the first and second stages, the oxygen enrichment recovery rhythm was synchronized with the air volume recovery rhythm, and the linkage between the oxygen enrichment rate and the pulverized coal ratio followed the following pattern: for every 10 kg / t increase in the pulverized coal ratio, the oxygen enrichment rate increased by 0.2% to 0.3%. The adjustment of the mine batch and the restoration of the ventilation volume should be synchronized. For every 100 m³ increase in ventilation volume, the ventilation volume should be increased accordingly. 3 / min, the ore batch recovers by 0.5 to 1 t accordingly, to avoid the ore batch recovering too quickly and increasing the load on the material column.