A method for heat treatment of titanium alloy materials by drawing

By employing processes such as four-stage forging, multi-pass rolling, vacuum annealing, and precision grinding, the problems of microstructure uniformity and hydrogen content control in medical titanium alloy wires have been solved, enabling the preparation of high-performance medical titanium alloy wires that meet the stringent requirements of surgical implants.

CN123108236APending Publication Date: 2026-11-17BAOJI UNIQUE TITANIUNM IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202611587467.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing medical titanium alloy wires have shortcomings in terms of microstructure uniformity, hydrogen content control, forming stability, annealing process, dimensional accuracy, surface quality, and batch consistency, making it difficult to meet the high-performance requirements of surgical implants.

Method used

The process employs four-stage forging, multi-pass rolling and peeling grinding, vacuum annealing, various types of annealing, and precision grinding, combined with chemical, microstructure, and physical property testing, to ensure that the material has a uniform internal structure, low hydrogen content, and accurate dimensions. Batch consistency is controlled through multiple rounds of testing.

Benefits of technology

The structure of the titanium alloy wire was made uniform and dense, with a hydrogen content of less than 0.0003%, a tensile strength of 1000–1030 MPa, a yield strength of ≥840 MPa, a metallographic structure of A1 grade, and dimensional tolerance controlled within ±0.005 mm. This reduced the risk of hydrogen embrittlement and improved the safety and consistency of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108236A_ABST
    Figure CN123108236A_ABST
Patent Text Reader

Abstract

This invention discloses a heat treatment method for drawing titanium alloy materials. The method involves first performing four-pass forging, with two passes above the phase transformation point and two passes below it, followed by multi-pass rolling and peeling / grinding. Two rolling passes are completed sequentially, and the target specification billet is obtained through multi-pass, progressively cooling drawing. Vacuum annealing is then performed, with hydrogen content strictly controlled below 0.0003% to reduce the risk of hydrogen embrittlement. After atmospheric annealing, grinding, and stress-relief annealing at 380℃ are also performed. After chemical, microstructure, and physical property testing at each stage, the finished product is obtained through precision grinding, chamfering, and polishing. This invention can produce medical-grade titanium alloys with uniform and defect-free microstructure, a tensile strength of 1000-1030 MPa, dimensional tolerances of ±0.005 mm, an A1 grade microstructure, low impurity content, excellent mechanical properties, and stable product quality, making it suitable for the medical field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of medical titanium alloy material processing technology, and in particular to a drawing heat treatment method for titanium alloy materials. Background Technology

[0002] Ti-6Al-4V ELI (ultra-low gap) titanium alloy, with the domestic equivalent grade TC4ELI, is one of the most widely used medical titanium alloy materials in the field of surgical implants due to its excellent biocompatibility, corrosion resistance, fatigue resistance, and good strength-toughness ratio. It is widely used in the manufacture of trauma and joint implants such as pedicle screws, intramedullary nails, connecting rods, and bone plates. These implants mostly use titanium alloy wire as the base material. The microstructure, interstitial element content, surface quality, dimensional accuracy, and batch consistency of the wire directly determine the mechanical properties, fatigue life, and service safety of the final implant.

[0003] In existing technologies, medical titanium alloy wires are typically prepared following a process route of ingot smelting, forging, rolling, drawing, annealing, straightening, grinding, and inspection. Product quality is controlled through chemical analysis, mechanical property testing, and metallographic examination. Titanium and titanium alloy processed materials for surgical implants must meet the requirements of standards such as GB / T 13810 or ASTM F136. ASTM F136 specifies that Ti-6Al-4V ELI processed materials must have a hydrogen content of no more than 0.0125% (i.e., 125 ppm) and an oxygen content of no more than 0.13%. The lower limits of conventional mechanical properties are a tensile strength of no less than 860 MPa and a yield strength of no less than 795 MPa.

[0004] However, existing methods for preparing medical titanium alloy wires still have the following drawbacks. First, it is difficult to guarantee the uniformity of the microstructure. Existing processes involve fewer forging passes and insufficient deformation, making it difficult to fully break down the coarse β grains and original β grain boundaries in the ingot and transfer them to the finished wire. Uneven grain size distribution significantly reduces the high-frequency fatigue strength of the wire, and high-frequency fatigue is one of the most critical failure modes of implants such as pedicle screws and intramedullary nails.

[0005] Secondly, improper rolling temperature control. When the rolling temperature is too high, Widmanstätten structure is easily generated, which seriously damages the strength and toughness of the wire and easily induces cracks. If the oxide layer (α layer) and surface cracks formed on the surface after rolling are not removed before the next heat treatment, the defects will be pressed into the interior of the material and become fatigue crack sources of the finished wire.

[0006] Third, the wire drawing process is unstable. The plastic window of TC4 type high-strength titanium alloy is relatively narrow. When the deformation amount in a single pass is too large, defects such as wire breakage, burrs, and cracks are prone to occur. The heat generated during the drawing process can also cause oxidation and deterioration of the wire surface, resulting in poor dimensional accuracy and surface consistency of the finished product.

[0007] Fourth, insufficient control of hydrogen content poses a risk of hydrogen embrittlement. Hydrogen is a key interstitial element that causes hydrogen embrittlement in titanium alloys, and medical implants are highly sensitive to hydrogen-induced delayed fracture under long-term load conditions in the body. Current processes typically only meet the ASTM F136 limit of no more than 0.0125% (i.e., 125 ppm) for hydrogen content, leaving very little margin. Fluctuations in the process can lead to hydrogen embrittlement, making it difficult to fully guarantee the long-term service safety of implants.

[0008] Fifth, the annealing process is unreasonable, making it difficult to balance strength and plasticity. When the conventional annealing temperature exceeds 700℃, the yield strength of TC4ELI wire decreases significantly, and the performance margin is small. When the annealing temperature or holding time is insufficient, the microstructure recovery is incomplete, the material state is unstable, and the performance fluctuates greatly between batches.

[0009] Sixth, residual stress and dimensional accuracy are difficult to control. The straightening and grinding processes introduce a lot of residual stress into the wire, resulting in a decrease in the yield strength and a deterioration in the straightness of the finished product. At the same time, the existing process has limited diameter tolerance control capabilities, making it difficult to consistently meet the stringent dimensional accuracy requirements of the implant processing base material.

[0010] Seventh, surface quality is difficult to guarantee. High-temperature processing easily forms oxide scale and α-contamination layer on the surface of the wire, while cold processing easily produces defects such as scratches and burrs. Surface defects can not only act as fatigue crack sources, reducing the fatigue life of implanted devices, but also impair the biocompatibility and corrosion resistance of implants.

[0011] Eighth, batch stability and quality traceability are insufficient. Currently, high-quality medical titanium alloy rods and wires still largely rely on imports, resulting in high procurement costs. Domestic processes suffer from complex procedures, unstable processes, and low levels of tissue refinement control and strength-plasticity matching control, leading to large performance fluctuations between batches. Furthermore, there is a lack of comprehensive chemical, tissue, and physical performance testing covering the entire process, making it difficult to meet the requirements for material consistency and traceability for implantable devices.

[0012] In summary, existing methods for preparing medical titanium alloy wires have shortcomings in terms of tissue uniformity, hydrogen content control, forming stability, annealing process, dimensional accuracy, surface quality, and batch consistency. Therefore, there is an urgent need to develop a drawing heat treatment method for titanium alloy materials that can produce uniform, fine-grained tissues with extremely low hydrogen content, stable dimensions and surface quality, and good batch consistency, to meet the pressing demand for high-performance medical titanium alloy wires in the field of surgical implants.

[0013] (TIABC = (“medical titanium alloy” OR “biocompatible titanium alloy” OR “orthopedic implant titanium alloy” OR “dental titanium alloy” OR “medical titanium alloy” OR “biocompatible titanium alloy” OR “orthopedic titanium alloy” OR “dental titanium alloy”)) AND (TIABC = (“vacuum self-consuming arc melting” OR “electrode” OR “melting parameters” OR “ingot” OR “VAR melting” OR “electrode”) OR TIABC = (“cold hearth” OR “electron beam”) OR TIABC = (“induction skull” OR “water-cooled copper crucible” OR “melting” OR “titanium alloy” OR “induction skull” OR “water-cooled crucible”) OR TIABC = (“precision casting” OR “shell” OR “surface material” OR “binder” OR “investmentcasting” OR “shell”) OR TIABC = ("centrifugal casting" OR "microstructure" OR "shrinkage porosity" OR "medical titanium alloy" OR "centrifugal casting" OR "microstructure") OR TIABC = ("ingot" OR "elemental segregation" OR "solidification rate" OR "homogenization" OR "ingot" OR "segregation") OR TIABC = ("gas atomization" OR "titanium alloy powder" OR "particle size distribution" OR "sphericity" OR "gas atomization" OR "powder") OR TIABC = ("plasma spheroidization" OR "radio frequency plasma" OR "powder morphology" OR "flowability" OR "plasma spheroidization" OR "flowability") OR TIABC = ("selective laser melting" OR "scanning strategy" OR "density" OR "medical implants" OR "selective laser melting" OR "density") OR TIABC = ("electron beam melting" OR "residual stress") OR“Porous structure” OR “Orthopedic implant” OR “electron beam melting” OR “porous structure” OR TIABC = (“Hot isostatic pressing” OR “powder densification” OR “porosity” OR “cladding” OR “hot isostatic pressing” OR “porosity”) OR TIABC = (“metal injection molding” OR “debinding” OR “sintering” OR “binder” OR “metal injection molding” OR “debinding”) OR TIABC = (“β forging” OR “forging temperature” OR “grain size” OR “Widmanstätten structure” OR “beta forging” OR “grain size”) OR TIABC = (“isothermal forging” OR “die temperature” OR “superplasticity” OR “deformation rate” OR “isothermal forging” OR “superplasticity”) OR TIABC = (“hot rolling” OR “sheet” OR “pass design” OR “texture” OR “hot rolling” OR “sheet”) OR TIABC = (“cold rolling” OR “Annealing” OR “Recrystallization” OR “Mechanical Properties” OR “Cold Rolling” OR “Annealing” OR TIABC = (“Hot Extrusion” OR “Tube” OR “Extrusion Ratio” OR “Lubrication” OR “Hot Extrusion” OR “Tube”) OR TIABC = (“Extrusion” OR “Microstructure Orientation” OR “Anisotropy” OR “Fiber Structure” OR “Extrusion” OR “Anisotropy”) OR TIABC = (“Solution Temperature” OR “Aging System” OR “α Phase” OR “β Phase” OR “Solution Treatment” OR “Aging”) OR TIABC = (“β Solution” OR “Cooling Method” OR “Martensite” OR “Metastable β” OR “Beta Solution” OR “Cooling Rate”) OR TIABC = (“Double Annealing” OR “High-Temperature Annealing” OR “Low-Temperature Annealing” OR “Microstructure Homogeneity” OR “Duplex Annealing” OR “Homogeneity”) OR TIABC = (“Deformation Heat Treatment” ORThermomechanical treatment OR phase transformation OR strengthening OR TIABC = (nanoprecipitate OR second phase OR dispersion strengthening OR transmission electron microscopy OR nanoprecipitate OR dispersion) OR TIABC = (grain boundary OR grain refinement OR equiaxed grain OR β grain OR grain boundary OR refinement) OR TIABC = (hydroxyapatite OR coating OR bioactive OR plasma spraying OR hydroxyapatite OR coating) OR TIABC = (micro-arc oxidation OR ceramic layer OR porous OR electrolyte OR micro-arc oxidation OR ceramic layer) OR TIABC = (shot peening OR residual compressive stress OR fatigue life OR coverage OR shot peening OR residual stress) OR TIABC = ("Laser shock" OR "Surface strengthening" OR "Dislocation" OR "Surface morphology" OR "Laser shock peening" OR "Dislocation") OR TIABC = ("Anodizing" OR "Nanotube" OR "Titanium dioxide" OR "Electrolysis parameters" OR "Anodization" OR "Nanotube") OR TIABC = ("Acid etching" OR "Alkali heat treatment" OR "Surface hydrophilicity" OR "Bioactivity" OR "Acid etching" OR "Alkali treatment") OR TIABC = ("Drug coating" OR "Sustained release" OR "Antibacterial" OR "Drug loading" OR "Drug coating" OR "Release") OR TIABC = ("Gradient coating" OR "Multilayer structure" OR "Adhesion" OR "Abrasion resistance" OR "Gradient coating" OR "Adhesion")) AND (FULL = (Titanium) AND FULL = (Annealing) AND FULL = (Hydrogen))

[0014] CN122189534A belongs to the field of high-end biomedical metal material preparation technology, specifically involving a highly uniform, large-size Ti6Al7Nb medical titanium alloy ingot and its preparation method. This invention achieves deep integration of pre-alloying and micro-alloying material design with the three-stage VAR+EMS melting process through synergistic control of "high-purity sponge titanium pretreatment + TiAlNb ternary master alloy design + trace boron addition for grain refinement + precise segregation control during three-stage VAR melting." This addresses both thermodynamic and kinetic aspects simultaneously, ensuring that niobium is fully dissolved during the melting stage and uniformly distributed during the solidification stage; achieving highly uniform ingot composition, fine and dense microstructure, and excellent batch stability. The entire process of this invention maintains high cleanliness control, ensuring an oxygen content ≤0.10wt% and the absence of harmful inclusions larger than 15 micrometers, meeting the most stringent medical standards.

[0015] CN111745103A provides a forging method for medical titanium alloy femoral stem forgings, which effectively utilizes raw materials and produces titanium alloy femoral stem forgings with dimensions controlled within a reasonable range and good surface quality. The method includes the following steps: Step 1, blanking; using 3D software to create a model and measure its volume V, the blanking volume V = V + (1000-1300), determining the blanking diameter based on the maximum cross-sectional area of ​​the product, and determining the blanking length by using the blanking volume and blanking diameter to cut the corresponding bar stock; Step 2, upset bending; Step 3, pre-forging; Step 4, adjusting the surface and dimensions of the workpiece according to surface and dimensional conditions; Step 5, final forging; Step 6, trimming the edges of the final forging and then annealing it; Step 7, chemical milling the workpiece; Step 8, milling the flash and polishing the forging contour.

[0016] CN119082525A discloses a 1000MPa strength TC4ELI wire for dental central screws and its preparation method, belonging to the field of medical titanium alloy material processing technology. Based on the chemical composition of titanium alloy Ti6Al4V, this invention further controls the composition range and, through strict VAR melting parameter setting, dual heat treatment technology, and straightening technology, prepares a TC4ELI titanium alloy wire for dental central screws that, compared with conventional medical wires, exhibits superior comprehensive performance, high consistency in overall product performance, and low variation, meeting the requirements for special wires for dental central screws.

[0017] CN110157948A relates to the field of medical titanium alloy materials, specifically a special medical titanium alloy for immediate implantation of narrow-diameter, high-strength implants and its preparation method. The chemical composition of this medical titanium alloy is as follows (wt%): Zr: 1417; Cu: 3.010; balance Ti. The drawing heat treatment method for this titanium alloy material involves: after forging and before rolling, holding at 900-1200℃ for 0.5-6 hours, water-cooling to room temperature; rolling at 720-850℃ with a strain rate greater than 0.1s; the resulting bar is used for subsequent implant processing. This invention provides a special medical titanium alloy for immediate implantation of narrow-diameter, high-strength implants, achieving immediate implantation without any surface treatment, resulting in a firm bond between the implant and bone tissue. The drawing heat treatment method for this titanium alloy material can prepare narrow-diameter (3.0-3.5mm) implants with high strength, achieving the goal of firm implantation in narrow, edentulous dentitions.

[0018] CN106148759A discloses a medical titanium alloy, which is based on the composition of existing medical Ti-6Al-4V alloy with the addition of copper (Cu) and strontium (Sr), wherein the Cu content is 6-12% and the Sr content is 0.1-2%. The invention also provides a hot working method and a heat treatment method for this titanium alloy; and the application of this titanium alloy as an orthopedic implant. This novel medical titanium alloy possesses biomedical functions of osteogenic and angiogenic activity, significantly improving the repair capacity and speed of bone tissue, shortening bone reconstruction and repair time, and enhancing the integration strength between the implant material and bone tissue.

[0019] CN106826118A discloses a method for preparing medical titanium alloy rods for manufacturing pedicle screws, including the following steps: peeling; surface treatment; temperature-controlled drawing; cutting; high-temperature annealing; hyperbolic cold straightening; stress-relief annealing; and polishing. This invention employs a combined process of temperature-controlled drawing, full annealing, and cold straightening and stress-relief treatment to prepare medical titanium alloy rods. Specifically, hot-rolled material is used as a blank, and the final product is obtained through temperature-controlled drawing and stress-relief treatment. Compared with traditional processes such as hot rolling and hot drawing, during the temperature-controlled drawing deformation process, dislocation pile-up caused by grain deformation leads to work hardening of the material, resulting in increased material strength. Appropriate high-temperature heat treatment further enhances plasticity and maintains a high strength level, thereby improving the material's mechanical properties. When the medical titanium alloy rods obtained by this invention are used to manufacture pedicle screws, the U-shaped groove of the pedicle screw has a narrowing of less than 0.05 mm, and the narrowing is stable.

[0020] CN101942688A relates to a composite oxidation process for medical-grade titanium alloy surfaces, belonging to the field of chemical treatment technology for metal surfaces. The aim is to improve the corrosion resistance and wear resistance of the oxide layer on the surface of medical-grade titanium alloys. This method includes two key processes: an anodizing process and a thermal oxidation process. After surface polishing, alkaline washing, and activation, the titanium alloy is anodized using a mixture of ammonium phosphate, ammonium acetate, and hydrogen peroxide as the electrolyte. After drying, thermal oxidation is carried out in an atmosphere of nitrogen and oxygen in a certain proportion, with the temperature controlled between 500 and 700°C. The method provided by this invention is simple, easy to implement, does not damage the mechanical properties of the titanium alloy material, and does not pollute the environment. It is suitable for mass production and significantly reduces costs.

[0021] CN110494098A generally relates to the formation of a porous oxide film on the surface of titanium alloys used in bone implantation in the human body using plasma electrolytic oxidation. More specifically, it relates to a method for manufacturing dental implants containing an electrolyte composition of metals and silicon in the plasma electrolytic oxidation process, and a method for coating dental implants with hydroxyapatite containing metal ions and silicon ions using the same composition. This method involves using an electrolyte solution containing metals (magnesium, zinc, strontium, manganese) and silicon, which play important roles in cell adhesion and bone formation, among other ions found in the human body. On the surface of the dental implant, a porous oxide film containing metal ions, silicon ions, calcium, and phosphorus is formed by plasma electrolytic oxidation. A method for manufacturing dental implants to improve bioactivity includes the following steps: a titanium alloy preparation step, in which dental titanium alloy is sequentially ground, micro-ground, and ultrasonically cleaned; an immersion step, in which the titanium alloy prepared in the above preparation step is placed at the anode of an electrolytic cell, and platinum is placed as the cathode before immersion in an electrolyte solution; a plasma formation step, in which a specified voltage and current density are applied to generate plasma and form an oxide film on the titanium alloy; and a drying step, in which after the oxide film is formed on the titanium alloy in the above plasma formation step, it is washed with ethanol and distilled water and then dried.

[0022] CN120967274A belongs to the field of medical implant materials technology, specifically relating to a method for preparing dental medical titanium alloy thin rods. The method includes the following steps: heating a titanium alloy forging billet to the β-phase transformation point temperature and holding it thereafter, forging it into a billet; rolling the billet to obtain a titanium rod; sequentially peeling and hot rolling the titanium rod to obtain a coiled billet; subjecting the coiled billet to N multi-pass orthogonal cold rolling, with a total deformation of ≤40% in each multi-pass rolling, and each multi-pass orthogonal cold rolling including 3-6 passes, to obtain a cold-rolled wire blank; sequentially cold straightening, cutting, and grinding the cold-rolled wire blank to obtain dental medical titanium alloy thin rods. This invention uses a high-deformation orthogonal cold rolling process to induce dislocations in the grains, forming dislocation entanglements and cellular structures, greatly refining the microstructure and eliminating coarse grains left over from hot working, thereby achieving grain refinement and meeting the standard requirements for dental medical GR4B titanium thin rods. Summary of the Invention

[0023] Purpose of the invention: To provide a more effective heat treatment method for drawing titanium alloy materials, the specific purpose of which is explained in the detailed implementation section for several substantial technical effects.

[0024] To achieve the above objectives, the present invention adopts the following technical solution:

[0025] A method for heat treatment of titanium alloy materials by drawing, characterized by comprising the following steps:

[0026] The material undergoes four forging processes, with two forging processes above the phase transformation point and two forging processes below the phase transformation point. This is followed by multiple rolling and peeling / grinding processes to ensure that the internal structure of the material is uniform and free of defects.

[0027] Key heat treatment steps: Two rolling processes: The first rolling is to a diameter of 100mm at a temperature of 940℃, with 8 to 13 passes; after treatment, air cooling is performed, followed by peeling and grinding; the second rolling is to a diameter of 9.0mm at a temperature of 900℃, with the number of passes controlled between 13 and 15, followed by coiling and peeling.

[0028] Drawing: The following drawing process is carried out, with 11 passes. The diameter is reduced in each pass, and the temperature is also reduced. The diameter is drawn to 3.90mm to ensure dimensional accuracy and material properties.

[0029] Vacuum annealing: used to strictly control the content of harmful gases such as hydrogen, oxygen, and nitrogen. The hydrogen content must be less than 0.0003%, which is significantly better than the F136 standard (≤0.0125%). This is used to effectively prevent the risk of hydrogen embrittlement and ensure the safety of materials.

[0030] Atmospheric annealing: The temperature is set to 720℃, held for 70-80 minutes, and then air-cooled to achieve material sizing and provide a stable foundation for subsequent uncoiling and straightening.

[0031] Grinding: Grind to a diameter of 3.8mm;

[0032] Stress-relief annealing: Stress-relief annealing at 380℃;

[0033] Sampling and testing: All processes must pass chemical, tissue and physical property tests before proceeding to the next process.

[0034] A further technical solution of the present invention is that all processes must pass chemical, tissue and physical property tests before proceeding to the next process.

[0035] A further technical solution of the present invention is that the final product must meet the following requirements: tensile strength of 1000–1030 MPa, yield strength ≥840 MPa, metallographic structure must reach A1 grade, and dimensional tolerance after fine grinding must be controlled within ±0.005 mm.

[0036] A further technical solution of the present invention is that the titanium ingot is divided into equal parts before the four-stage forging process.

[0037] A further technical solution of the present invention is that the key heat treatment process also includes pickling and grinding: pickling and grinding are then performed to remove surface cracks and defects.

[0038] A further technical solution of the present invention is that the straightening length after atmospheric annealing is uniformly 3.2 meters.

[0039] A further technical solution of the present invention is that, after sampling and testing, the following steps are included: fine grinding: error control; after fine grinding, the dimensional tolerance is controlled within ±0.005mm; flattening, chamfering, polishing, and producing the finished product.

[0040] A further technical solution of the present invention is to feed φ100 mill bars, 22-25kg / bar, up to 3200kg, without any leftover material ends;

[0041] Pickling and polishing are performed.

[0042] First heat: 920℃, hold for 60 min to roll φ10.5×Lmm;

[0043] Peel the shell to φ10.2 (+0 / -0.05), collect in small trays of 700-800 mm, paying attention to tolerances;

[0044] The coil is pickled and cleaned by grinding.

[0045] 2920 kg of pickled and ground white-skinned discs of the above-mentioned spindle numbers were added.

[0046] Vacuum annealing at 750℃ for 2.5 hours to remove hydrogen;

[0047] Draw the wire at 820℃ to φ3.95 (-0 / +0.05)×L mm, cool down the mold by 5-10℃, and collect it into a 650mm small tray;

[0048] Annealing at 720℃ for 70 minutes; air cooling;

[0049] Unwind and straighten the coil; cut the material to a length of 3200mm. Note the length; any excess material exceeding 2000mm is acceptable for normal production.

[0050] Roughly grind to φ3.8 (-0 / +0.05) × 3200mm;

[0051] Stress-relief annealing at 380℃ for 5.5 hours; furnace cooling; after bar drawing is qualified, continue (performance requirements: 1000-1030 / 830 / 16 / 35, metallographic requirements A1-A9), one piece will be sent for performance, and one piece will be sent for H content;

[0052] Sampling is required according to the production notification. Mechanical testing and high-magnification inspection are required. Provide one 20mm thin film for contamination layer testing. Note: Send H content sample.

[0053] Grind to the finished size, paying attention to tolerances; bent materials are strictly prohibited from being ground.

[0054] Polishing; Inspecting diameter tolerances;

[0055] Mark the negative ruler section and cut it off to ensure the finished length;

[0056] Flat end, with 45° chamfered edges on both sides, 1-2mm deep;

[0057] Polishing; Inspecting diameter tolerances;

[0058] Return to warehouse for inspection.

[0059] The present invention, employing the above technical solution, offers the following advantages over existing technologies: Reduced hydrogen embrittlement risk and improved material safety: Strict control of harmful impurities such as hydrogen, oxygen, and nitrogen through vacuum annealing processes ensures hydrogen content is below 0.0003%, far exceeding the F136 standard requirements. This effectively suppresses hydrogen embrittlement defects, mitigates material failure risks in medical settings, and guarantees the safety and reliability of implantation. Uniform and dense structure, excellent product mechanical and dimensional accuracy: Employing a four-stage differentiated forging process, multi-pass rolling, and multi-pass progressive cooling drawing, combined with multi-round pickling, peeling, and grinding to remove surface cracks and defects, along with precision grinding, the finished product achieves a tensile strength of 1000-1030 MPa, high yield strength, A1-grade metallographic structure, and dimensional tolerances controlled within ±0.005 mm. Simultaneously, it ensures uniform and defect-free internal structure, meeting the stringent mechanical and precision requirements of medical titanium alloys. The process system is complete and controllable, resulting in high product quality stability: Progressive testing of chemical, metallographic structure, and physical properties is set between each process, including forging, rolling, drawing, various types of annealing, straightening, and polishing. Only products that pass the inspection of the previous process can proceed to the next process. At the same time, post-treatments such as stress-relief annealing and flat-end chamfering polishing are provided to eliminate residual processing stress, stabilize the material state, ensure the consistency of product performance in mass production, and adapt to the mass production application of medical devices.

[0060] Beneficial effects Attached Figure Description

[0061] To further illustrate the present invention, the following description is provided in conjunction with the accompanying drawings:

[0062] Figure 1 : Process flow diagram of the present invention. Detailed Implementation

[0063] The present invention will be further illustrated below with reference to the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. In the description of the present invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," "outer," "top," and "bottom," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention. In addition, unless otherwise expressly specified and limited, the terms "installed," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal communication of two components. For those skilled in the art, the specific meaning of the above terms in the present invention can be understood according to the specific circumstances.

[0064] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0065] This patent provides multiple parallel solutions; the different descriptions represent improved solutions or parallel solutions based on the basic solution. Each solution has its own unique characteristics. Furthermore, the technical features involved in the different embodiments of the invention described below can be combined with each other as long as they do not conflict with each other. Fixing methods not described herein can be any type of fixing, such as threaded fixing, bolt fixing, or adhesive bonding.

[0066] The choice of materials used in an invention does not limit the scope of protection.

[0067] Materials and forging: Medical-grade titanium alloy 3.606 is used, and four-pass forging is performed (two passes above the phase transformation point and two passes below the phase transformation point), combined with multiple rolling and peeling and grinding to ensure uniform and defect-free microstructure.

[0068] Key hot rolling control:

[0069] First rolling to a diameter of 100 mm (temperature 940℃);

[0070] The material is rolled a second time to a diameter of 9.0 mm (at a temperature of 900℃).

[0071] Pass control: All passes must be controlled between 8 and 15 to ensure dimensional accuracy and performance.

[0072] Vacuum annealing (gas control): Strict control of hydrogen, oxygen and nitrogen content, with hydrogen content required to be <0.0003% (significantly better than F136 standard ≤0.0125%) to prevent hydrogen embrittlement risk.

[0073] Atmospheric annealing and straightening: Atmospheric annealing is set at 720℃, held for 70-80 minutes and cooled in a controlled manner; the straightening length is uniformly 3.2 meters to provide a basis for subsequent unwinding.

[0074] Final inspection standards and workflow

[0075] Physicochemical properties: tensile strength 1000–1030 MPa, yield strength ≥840 MPa, metallographic structure reaches A1 grade.

[0076] This invention relates to a drawing heat treatment method for titanium alloy materials, the raw material of which is Ti-6Al-4V ELI (ultra-low gap) titanium alloy (the corresponding domestic grade is TC4ELI), and the preparation of medical titanium alloy wire as the processing master material for surgical implants such as pedicle screws, intramedullary nails, connecting rods, and bone plates.

[0077] The implementation process of the present invention (based on Example 1, combined with the examples described in Examples 4, 5, 6, 7, and 8) mainly includes: dividing the titanium ingot into equal parts (Example 4); then performing four-pass forging, wherein two passes are above the β phase transformation point and two passes are below the β phase transformation point, and combined with multi-pass rolling and peeling and grinding to ensure that the internal structure of the material is uniform and defect-free; entering the key heat treatment stage, the first rolling is performed to a diameter of 100 mm, a temperature of 940 °C, and 8 passes. —After 13 passes, the material is air-cooled, peeled, and ground. It is then rolled a second time to a diameter of 9.0 mm at 900 °C for 13-15 passes. After that, it is stripped and peeled, and then pickled and ground to remove surface cracks and defects (Example 5). Then, it is drawn for 11 passes, with the diameter and temperature reduced in each pass, until the diameter is 3.90 mm. Vacuum annealing strictly controls the content of harmful gases such as hydrogen, oxygen, and nitrogen. The hydrogen content is less than 0.0003%, which is significantly better than the 0.0125% limit specified in ASTM F136 standard. The atmospheric annealing temperature is set at 720 °C, held for 70-80 minutes, and then air-cooled to achieve material shaping. The straightening length after atmospheric annealing is uniformly 3.2 meters (Example 6). It is ground to a diameter of 3.8 mm. It is then stress-relieved annealed at 380 °C. Finally, it is finely ground (dimensional tolerance ±0.005 mm), flattened, chamfered, and polished (Example 7) to produce the finished product. All processes must pass chemical, microstructure and physical property tests before proceeding to the next process (Example 2). The final product meets the requirements of tensile strength of 1000-1030MPa, yield strength ≥840MPa, and metallographic structure reaching A1 grade (Example 3).

[0078] The following section addresses each of the eight defects listed in the existing technology defect document, explaining the principle by which the present invention addresses these defects.

[0079] II. Detailed Explanation of Solutions to Existing Technical Defects

[0080] The first explanation of the solution to the defect of "difficulty in ensuring the uniformity of microstructure"

[0081] In contrast to the shortcomings of existing technologies, such as "few forging passes, insufficient deformation, difficulty in fully breaking down coarse β grains and original β grain boundaries in the ingot and passing them on to the finished wire, and uneven grain size distribution that significantly reduces the high-frequency fatigue strength of the wire", this patent innovatively sets the forging process to a four-pass forging process, with two passes above the β phase transformation point and two passes below the β phase transformation point, followed by multiple passes of rolling and peeling grinding after forging.

[0082] The targeted solution lies in the following principle: Two forging passes above the β phase transformation point allow the ingot to undergo sufficient large deformation in the high-temperature β single-phase region, enabling the coarse β grains and their original β grain boundaries to be fully broken down and recrystallized, completing the initial microstructure. Two forging passes below the β phase transformation point further refine the grains in the α+β two-phase region through deformation, resulting in a fine and uniform two-phase microstructure. Subsequent multi-pass rolling at 940℃ and 900℃ continues to refine the grains with progressively smaller deformations, and surface defects are promptly removed through peeling and grinding, preventing the inheritance of coarse grains or surface defects to the finished wire. Therefore, this invention ensures uniform and refined microstructure throughout the entire process from ingot to finished wire, ultimately achieving an A1 grade microstructure, eliminating the adverse effects of uneven grain size distribution on high-frequency fatigue strength from the source.

[0083] Secondly, the solution to the defect of "improper rolling temperature control" is explained.

[0084] Compared to the shortcomings of existing technologies, such as "excessive rolling temperature easily produces Widmanstätten structure, which seriously damages the strength and toughness of the wire and easily induces cracks; if the oxide layer (α layer) and surface cracks formed on the surface after rolling are not removed before the next rolling pass, the defects will be pressed into the material and become the fatigue crack source of the finished wire", this patent innovatively and non-obviously controls the temperature of the two key rolling processes precisely below the β phase transformation point, that is, the first rolling temperature is 940℃ and the second rolling temperature is 900℃, and the number of rolling passes is controlled to 8-13 and 13-15 respectively, and peeling and pickling grinding processes are set after each rolling.

[0085] The targeted solution lies in the fact that 940℃ and 900℃ are both in the α+β two-phase region below the β phase transformation point. When the material deforms in the two-phase region, the microstructure always maintains a fine α+β state, which avoids the formation of coarse Widmanstätten structure in the high-temperature β region from the process source, thereby protecting the strength and toughness of the wire and avoiding crack induction. Replacing single-pass large-deformation rolling with multi-pass small-deformation rolling further prevents deformation overheating and cracking. The peeling and grinding, pickling and grinding immediately after rolling air cooling, remove the surface oxide layer (α layer) and surface cracks in time before the next process, so that defects cannot be pressed into the interior of the material, cutting off the path for surface defects to evolve into fatigue crack sources in the finished wire.

[0086] Thirdly, explanation of the solution to the defect of "instability in the wire drawing process".

[0087] In contrast to the shortcomings of existing technologies, such as "the plastic window of TC4 type high-strength titanium alloy drawing is relatively narrow, and defects such as wire breakage, burrs, and cracks are prone to occur when the deformation amount in a single pass is too large; the heat generated during the drawing process will also cause oxidation and deterioration of the wire surface, resulting in poor dimensional accuracy and surface consistency of the finished product", this patent innovatively sets the drawing process to 11 passes, with the diameter reduced and the temperature reduced in each pass, drawing to a diameter of 3.90mm, that is, multi-pass temperature-controlled drawing starting from 820℃ and cooling down by 5-10℃ in each pass.

[0088] The targeted solution is based on the following principle: distributing the total deformation over 11 passes, with each pass only subjecting a small amount of deformation, thus avoiding wire breakage, burrs, and cracking caused by large deformation in a single pass under the narrow plasticity window of TC4 high-strength titanium alloy; the starting drawing temperature of 820℃ is in the α+β two-phase region, ensuring the plasticity of the material during the deformation process; and actively reducing the temperature by 5-10℃ in each pass, which on the one hand offsets the heat generated by the drawing deformation and inhibits the oxidation and deterioration of the wire surface, and on the other hand ensures that the microstructure remains stable during the cooling process of each pass. Ultimately, while achieving a dimensional accuracy of 3.90mm, the solution also ensures the dimensional accuracy, surface consistency, and material properties of the finished product.

[0089] Fourthly, explanation of solutions to the defect of "insufficient control of hydrogen content and risk of hydrogen embrittlement".

[0090] In contrast to the shortcomings of existing technologies, which state that "hydrogen is a key interstitial element causing hydrogen embrittlement in titanium alloys, and medical implants are highly sensitive to hydrogen-induced delayed fracture under long-term load conditions in the body. Existing processes typically only meet the hydrogen content limit requirement of ASTM F136 of no more than 0.0125% (i.e., 125 ppm), with very little margin. Fluctuations in the process pose a risk of hydrogen embrittlement, making it difficult to fully guarantee the long-term service safety of implants," this patent innovatively and non-obviously introduces vacuum annealing as a key step in controlling hydrogen content. Annealing is performed in a vacuum environment, ensuring that the hydrogen content must be below 0.0003% (i.e., 3 ppm), which is significantly better than the 0.0125% limit specified in the ASTM F136 standard.

[0091] Its targeted solution lies in the fact that vacuum annealing significantly reduces the hydrogen partial pressure in the furnace through a vacuum environment, disrupting the balance between hydrogen in the titanium alloy matrix and the gas phase, and promoting the continuous diffusion and desorption of hydrogen dissolved in the material to the surface, thus achieving deep dehydrogenation. The hydrogen content of 0.0003% is only about one-fortieth of the ASTM F136 limit (0.0125%), and the hydrogen content surplus is dozens of times larger than that of existing technologies. Even if the process parameters fluctuate, it will not reach the hydrogen embrittlement critical value. It eliminates the risk of hydrogen-induced delayed fracture from the material's essence and ensures the safety of the implant under long-term load-bearing conditions in the body.

[0092] Fifthly, the explanation of solutions to the defects of "unreasonable annealing process and difficulty in balancing strength and plasticity".

[0093] In contrast to the shortcomings of existing technologies, such as "when the conventional annealing temperature exceeds 700℃, the yield strength of TC4ELI filament decreases significantly, and the performance margin is small; when the annealing temperature or holding time is insufficient, the microstructure recovery is incomplete, the material state is unstable, and the performance fluctuates greatly between batches," this patent innovatively and non-obviously decomposes the annealing process into a synergistic annealing system of "vacuum annealing - atmospheric annealing - stress-relief annealing": vacuum annealing (holding at 750℃ for 2.5 hours) completes the microstructure homogenization and dehydrogenation in a vacuum environment; atmospheric annealing is set at 720℃, the holding time is precisely controlled at 70-80 minutes, and air cooling is performed to achieve material stabilization and provide a stable foundation for subsequent uncoiling and straightening; stress-relief annealing is carried out at a low temperature of 380℃ to eliminate residual stress.

[0094] The underlying principle of this invention is as follows: The fundamental reason for the significant decrease in strength after annealing in existing technologies lies in the coarse microstructure and the coarse annealing process, resulting in low tolerance of the material to annealing softening. In this invention, the fine and uniform α+β microstructure is obtained through four-pass forging and multi-pass rolling, and the fine grain strengthening provides sufficient strength reserves, enabling the material to maintain high strength even after short-term annealing at 720℃. At the same time, the 720℃ atmospheric annealing strictly limits the holding time to 70-80 minutes and uses air cooling. The short holding time and relatively fast cooling rate together inhibit grain growth and strength loss, while ensuring sufficient microstructure recovery and material stability. The 380℃ stress-relief annealing eliminates stress at a temperature far below the recrystallization temperature without changing the strength and plasticity. The result of the synergy of these three factors is that the final product maintains good plasticity at a high strength level of 1000-1030MPa and yield strength ≥840MPa (higher than the standard lower limit of 795MPa), with a large performance margin. Furthermore, the annealing temperature, holding time, and cooling method are all quantified, and the performance fluctuations between batches are effectively suppressed.

[0095] The sixth point addresses the solution to the defect of "difficulty in controlling residual stress and dimensional accuracy".

[0096] In contrast to the shortcomings of existing technologies, such as the fact that "the straightening and grinding processes introduce more residual stress into the wire, resulting in a decrease in the yield strength and a deterioration in the straightness of the finished product; at the same time, the existing processes have limited diameter tolerance control capabilities, making it difficult to reliably meet the stringent dimensional accuracy requirements of the implant processing substrate," this patent innovatively and non-obviously unifies the straightening process to atmospheric annealing followed by uncoiling and straightening at a length of 3.2 meters, and sets up a stress-relief annealing process at 380℃ (holding for 5.5 hours and cooling in the furnace) after the grinding process, and precisely controls the dimensional tolerance of the finished product to ±0.005mm.

[0097] The targeted solution lies in the following principles: 380℃ stress-relief annealing at low temperatures fully releases the residual stress introduced during straightening and grinding, preventing the accumulation of residual stress from reducing the yield strength of the finished product. The slow cooling method of furnace cooling also prevents the reintroduction of thermal stress during the cooling process, thus ensuring both yield strength and straightness. Grinding adopts a two-stage control: "rough grinding to 3.8mm diameter - fine grinding to finished product size," and constrains the finished product diameter with a quantitative tolerance of ±0.005mm. This ensures that the wire dimensional accuracy meets the stringent requirements of the parent material for implant processing, laying the foundation for the consistency of subsequent implant device processing.

[0098] The seventh point addresses the solution to the defect of "difficulty in guaranteeing surface quality".

[0099] In contrast to the shortcomings of existing technologies, such as "high-temperature processing easily forms oxide scale and α-contamination layer on the surface of wire, while cold processing easily produces defects such as scratches and burrs; surface defects can not only reduce the fatigue life of implanted devices as fatigue crack sources, but also damage the biocompatibility and corrosion resistance of implants", this patent innovatively and non-obviously sets peeling and grinding and pickling and grinding steps after high-temperature processes, such as peeling and grinding after rolling, peeling of coiled wire, and pickling and grinding, to remove surface cracks and defects, and sets fine grinding, polishing and flattening, and double-sided chamfering 45° processes in the finished product stage.

[0100] Its targeted solution lies in the following principles: peeling and grinding, and acid pickling and grinding, promptly remove surface oxide scale, α-contamination layer, and surface microcracks after each high-temperature processing and before the next process, preventing the accumulation of high-temperature surface defects and their embedding into the material throughout the entire process; fine grinding and polishing in the finished product stage eliminate cold-working scratches and burrs, and flattening and double-sided chamfering remove sharp corner defects at the ends, ultimately obtaining a smooth, defect-free surface. A clean surface eliminates fatigue crack sources, improves the fatigue life of implanted devices, and ensures the biocompatibility and corrosion resistance of the contact surface between the implant and human tissue.

[0101] The eighth point addresses the solution to the deficiency of "insufficient batch stability and quality traceability".

[0102] In contrast to the shortcomings of existing technologies, such as the fact that "high-quality medical titanium alloy rods and wires still largely rely on imports, resulting in high procurement costs; domestic processes suffer from complex procedures, unstable processes, low levels of tissue refinement control and strength-plasticity matching control, large batch-to-batch performance fluctuations, and a lack of comprehensive chemical, tissue, and physical property testing, making it difficult to meet the requirements of implantable devices for material consistency and traceability," this patent innovatively embeds comprehensive quality control into the preparation method itself: stipulating that all processes must pass chemical, tissue, and physical property testing before proceeding to the next process (Example 2), and dividing the titanium ingot into equal parts before the fourth forging (Example 4) to ensure ingot consistency.

[0103] Its targeted solution lies in the following principles: all parameters such as temperature, number of passes, holding time, and dimensions in each process, including forging, rolling, drawing, and annealing, are quantified and fixed as clear process windows, enabling the process to have good replicability and stability, and eliminating dependence on imported materials; the titanium ingots are divided equally to ensure that each batch of raw materials is in a consistent state, controlling batch differences from the source; a full-process inspection system consisting of "chemical testing (hydrogen content testing) - microstructure testing (metallographic structure and contamination layer testing) - physical property testing (mechanical property testing)" ensures that materials that fail to meet the standards in any process cannot flow into the next process, achieving full-process quality control and traceability from ingot to finished wire, ultimately obtaining medical titanium alloy wire with small performance fluctuations between batches, good material consistency, and good traceability.

[0104] III. Summary

[0105] In summary, compared to the shortcomings of existing technologies, this patent innovatively and non-obviously constructs a complete technical system of "four-pass forging refinement—multi-pass rolling in the two-phase region—11-pass temperature-controlled drawing—vacuum annealing for deep dehydrogenation—synergistic annealing for strength and plasticity matching—stress relief and precision grinding—full-process inspection gate": four-pass forging and multi-pass rolling solve the defects of microstructure uniformity; two-phase temperature control solves the defects of rolling microstructure; multi-pass temperature-controlled drawing solves the defects of forming stability; vacuum annealing solves the defects of hydrogen embrittlement risk; synergistic annealing system solves the defects of difficulty in balancing strength and plasticity; stress relief annealing and ±0.005mm precision grinding solve the defects of residual stress and dimensional accuracy; peeling and grinding, pickling and grinding and polishing and chamfering solve the defects of surface quality; and full-process inspection gate and equal division of titanium ingots solve the defects of batch stability and quality traceability. The solution of this invention achieves comprehensive improvements over the prior art in terms of uniform and fine structure (metallographic structure reaches A1 grade), extremely low hydrogen content (less than 0.0003%), precise dimensional tolerance (±0.005mm), excellent surface quality, good strength-plasticity matching (tensile strength 1000-1030MPa, yield strength ≥840MPa), and batch consistency, and can meet the urgent needs of the surgical implant field for high-performance medical titanium alloy wire.

[0106] IV. Specific Solutions to the Defects of the Existing Technology in Each Embodiment

[0107] The following describes the principle of addressing the defects of the prior art in each embodiment of this patent. Embodiment 1 is the basic embodiment, and Embodiments 2 to 8 are further improved solutions, parallel solutions, or optional independent solutions based on the basic embodiment.

[0108] Example 1; The proposed solution includes the following steps: four forging passes, two above the phase transformation point and two below, followed by multi-pass rolling and peeling / grinding to ensure a uniform and defect-free internal structure; key heat treatment steps: two rolling passes: the first rolling to a diameter of 100mm at 940℃, with 8 to 13 passes; after treatment, air cooling, followed by peeling and grinding; the second rolling to a diameter of 9.0mm at 900℃, with the number of passes controlled between 13 and 15, followed by coiling and peeling; drawing: followed by a drawing process, 11 passes, each pass reducing the diameter and temperature; the drawing process is... Diameter 3.90mm; ensuring dimensional accuracy and material properties; Vacuum annealing: used to strictly control the content of harmful gases such as hydrogen, oxygen, and nitrogen, with the hydrogen content required to be below 0.0003%, significantly better than the F136 standard (≤0.0125%), effectively preventing hydrogen embrittlement risk and ensuring material safety; Atmospheric annealing: temperature set at 720℃, held for 70-80 minutes, air-cooled to achieve material shaping and provide a stable foundation for subsequent uncoiling and straightening; Grinding: grinding to a diameter of 3.8mm; Stress-relief annealing: stress-relief annealing at 380℃; Sampling and testing: all processes must pass chemical, microstructure, and physical property tests before proceeding to the next process.

[0109] Regarding this document: In contrast to the shortcomings of existing technologies such as "few forging passes and insufficient deformation, making it difficult to fully break down and inherit the coarse β grains and original β grain boundaries in the ingot and transfer them to the finished wire, and the uneven grain size distribution will significantly reduce the high-frequency fatigue strength of the wire", this patent innovatively and non-obviously constructs the preparation of medical titanium alloys into a complete process chain of "four-pass forging - multi-pass rolling and peeling and grinding - two-phase zone temperature-controlled rolling - 11-pass temperature-controlled drawing - vacuum annealing - atmospheric annealing - grinding - stress-relief annealing - inspection gating". The targeted solution lies in the following principles: forging above the two-stage phase transformation point allows coarse β grains and original β grain boundaries to be fully broken and recrystallized in the high-temperature β single-phase region, completing the initial structure; forging below the two-stage phase transformation point further refines the grains through deformation in the α+β two-phase region; subsequent multi-pass rolling at 940℃ and 900℃ refines the structure through successive small deformations, and surface defects are promptly removed through peeling and grinding; 11-pass drawing converges to a dimensional accuracy of 3.90mm in diameter through successive reductions in diameter and temperature; vacuum annealing controls the hydrogen content below 0.0003%, essentially eliminating the risk of hydrogen embrittlement; atmospheric annealing at 720℃ for 70-80 minutes achieves material shaping, providing a stable foundation for subsequent uncoiling and straightening; after grinding to a diameter of 3.8mm, residual stress is released by stress-relief annealing at 380℃; finally, chemical, microstructure, and physical property testing serve as the quality gates for the entire process. Each process creates favorable conditions for the next: forging refinement is a prerequisite for rolling homogenization, temperature-controlled rolling is a prerequisite for drawing stability, vacuum annealing provides a low-hydrogen matrix for atmospheric annealing, stress-relief annealing ensures final dimensional accuracy, and inspection gate control ensures that only qualified products flow into the next stage. In this way, the existing technical defects such as microstructure uniformity, rolling structure control, drawing stability, hydrogen embrittlement risk, strength-plasticity matching, residual stress and dimensional accuracy, surface quality, and batch stability are solved simultaneously as a whole.

[0110] Example 2; Regarding the solution: All processes must pass chemical, tissue, and physical property tests before proceeding to the next process.

[0111] Regarding the shortcomings of existing technologies—namely, the high cost of importing high-quality medical titanium alloy rods and wires, the complexity and instability of domestic processes, low levels of microstructure refinement control and strength-plasticity matching control, large batch-to-batch performance fluctuations, and the lack of comprehensive chemical, tissue, and physical performance testing to meet the consistency and traceability requirements of implantable devices—this patent innovatively embeds comprehensive quality control into the manufacturing process itself: from forging, rolling, drawing, annealing to finished product processing, each step must pass chemical, tissue, and physical performance testing before proceeding to the next stage. The targeted solution lies in: chemical testing (hydrogen content detection) controls the composition to prevent materials with excessive harmful gas content from entering subsequent processes; tissue testing (metallographic structure and contamination layer detection) controls the microstructure to prevent substandard materials from continuing processing; and physical performance testing controls the mechanical properties to prevent substandard materials from entering the finished product stage. Three inspection gates operate simultaneously at each process node, preventing substandard materials from flowing downstream. This process system effectively plugs the loopholes of large performance fluctuations between batches and lack of quality traceability, ensuring the consistency and traceability of the final filament material in terms of composition, structure, and performance. This provides institutional guarantees for reducing dependence on imported materials.

[0112] Example 3; Regarding the solution: The final product must meet the following requirements: tensile strength 1000–1030 MPa, yield strength ≥840 MPa, metallographic structure must reach A1 grade, and dimensional tolerance after fine grinding must be controlled within ±0.005 mm.

[0113] Regarding the shortcomings of existing technologies, such as "when the conventional annealing temperature exceeds 700℃, the yield strength of TC4ELI filament decreases significantly, and the performance margin is small; when the annealing temperature or holding time is insufficient, the microstructure recovery is inadequate, the material state is unstable, and the performance fluctuates greatly between batches" and "the diameter tolerance control capability of existing processes is limited, making it difficult to consistently meet the stringent dimensional accuracy requirements of implant processing substrates," this patent innovatively and non-obviously quantifies the final product into clear dual acceptance thresholds for performance and dimensions: tensile strength 1000–1030MPa, yield strength ≥840MPa, metallographic structure must reach A1 grade, and dimensional tolerance after fine grinding is controlled within ±0.005mm. The targeted solution lies in the following: the preceding four-pass forging and multi-pass rolling processes have yielded a fine and uniform α+β microstructure. Fine grain strengthening provides ample strength reserves, ensuring that the wire, after atmospheric annealing at 720℃ and stress-relief annealing at 380℃, maintains a stable tensile strength range of 1000–1030 MPa, with a yield strength not lower than 840 MPa (higher than the standard lower limit of 795 MPa). The A1 grade metallographic structure is a quantitative representation of the uniform and fine microstructure. A precision grinding tolerance of ±0.005 mm locks the finished product diameter within the stringent requirements of the implant material. This quantitative threshold is both the acceptance result of the synergistic effect of the aforementioned processes and the last line of defense against insufficient performance margins, batch fluctuations, and dimensional deviations. It transforms "balancing strength and plasticity, and meeting dimensional accuracy standards" from an empirical description into a verifiable and replicable hard standard.

[0114] Example 4; Solution: Before the four-stage forging process, the titanium ingot is divided into equal parts.

[0115] This document addresses the shortcomings of existing technologies, such as "complex processes, unstable processes, low levels of microstructure refinement control and strength-plasticity matching control in domestic processes, large batch-to-batch performance fluctuations, and a lack of comprehensive chemical, microstructural, and physical property testing, making it difficult to meet the requirements of material consistency and traceability for implantable devices." This patent innovatively introduces a non-obvious step of dividing titanium ingots into equal parts before the four-pass forging process. The underlying principle is that ingots exhibit compositional segregation and microstructure differences along their length and cross-section. Without pre-division, the state of raw materials used in each batch will be inconsistent, inevitably leading to fluctuations in microstructure and properties after forging and rolling. Dividing the titanium ingots ensures that each batch yields ingots with consistent specifications and state, allowing subsequent four-pass forging, multi-pass rolling, drawing, and annealing to all be based on a unified raw material foundation, thus suppressing batch-to-batch differences from the outset. The equal-splitting operation fixes the "ingot consistency," a fundamental factor affecting batch stability, at extremely low cost. This, combined with full-process testing gating, forms the basis for a process with minimal performance fluctuations between batches, material consistency, and good traceability.

[0116] Example 5; Regarding the solution: the key heat treatment steps also include pickling and grinding: pickling and grinding are then performed to remove surface cracks and defects;

[0117] Regarding the shortcomings of existing technologies, such as "if the oxide layer (α layer) and surface cracks formed on the surface after rolling are not removed before the next heat treatment, the defects will be pressed into the material and become fatigue crack sources of the finished wire" and "high-temperature processing easily forms oxide scale and α contamination layer on the surface of the wire, while cold processing easily produces defects such as scratches and burrs; surface defects can not only reduce the fatigue life of implanted devices as fatigue crack sources, but also damage the biocompatibility and corrosion resistance of implants", this patent innovatively introduces pickling and grinding into the key heat treatment process in a non-obvious way. After high-temperature processing and before the next process, the surface cracks and defects are removed by pickling and grinding. The targeted solution is based on the following principle: High-temperature rolling will form oxide scale and α-contamination layer on the surface of the wire and induce surface microcracks. If left untreated, subsequent deformation and processing steps such as drawing and grinding will press these surface defects into the material, making them fatigue crack sources in the finished wire. Pickling chemically dissolves the loose oxide scale and contamination layer, while grinding mechanically removes residual cracks and burrs. The combination of these two methods completely removes the defects before they accumulate, so that the clean surface no longer carries defect sources that propagate into the material. This not only improves the fatigue life of the implanted device, but also ensures the biocompatibility and corrosion resistance of the contact surface between the implant and human tissue.

[0118] Example 6; For the proposed solution: the straightening length after atmospheric annealing is uniformly 3.2 meters.

[0119] Regarding this document: In contrast to the shortcomings of existing technologies, such as "the straightening and grinding processes introduce more residual stress into the wire, resulting in a decrease in the yield strength and a deterioration in the straightness of the finished product; at the same time, the diameter tolerance control capability of existing processes is limited, making it difficult to reliably meet the stringent dimensional accuracy requirements of the implant processing base material", this patent innovatively and non-obviously standardizes the straightening length after atmospheric annealing to 3.2 meters. The underlying principle of this solution is as follows: Unwinding and straightening are crucial processes for eliminating coil bending and establishing straightness and flatness. If the straightening length is not uniform, the stress state and deformation history of each section of the filament will differ, resulting in uneven distribution of residual stress and flatness after straightening, directly affecting the consistency of subsequent grinding and finished product dimensions. By unifying the straightening length to 3.2 meters, each section of filament enters straightening and subsequent processing with the same length specification. The bending and reverse bending deformation during the straightening process remains consistent, the residual stress distribution is uniform and controllable, and the flatness is stable and consistent. This provides a uniform reference length for subsequent rough grinding to 3.8mm and fine grinding to the finished product dimensions. Thus, with the support of subsequent 380℃ stress-relief annealing, the yield strength, flatness, and dimensional accuracy of the finished filament are simultaneously guaranteed, meeting the stringent requirements for straightness and dimensional consistency of the implant processing substrate.

[0120] Example 7; Regarding the solution: After sampling and testing, the following steps are also included: fine grinding: error control. After fine grinding, the dimensional tolerance is controlled within ±0.005mm; flattening, chamfering, polishing, and producing the finished product.

[0121] Regarding this document: In contrast to the shortcomings of existing technologies, such as "cold working is prone to scratches, burrs and other defects; surface defects can not only reduce the fatigue life of implanted devices as fatigue crack sources, but also impair the biocompatibility and corrosion resistance of implants" and "existing processes have limited diameter tolerance control capabilities, making it difficult to consistently meet the stringent dimensional accuracy requirements of the implant processing base material", this patent innovatively and non-obviously sets the finishing process of "fine grinding - flattening - chamfering - polishing" after sampling and inspection: fine grinding controls the dimensional tolerance of the finished product to ±0.005mm, flattening removes unevenness at the ends, chamfering removes sharp corners and burrs at the ends, and polishing eliminates cold working scratches and finally obtains a smooth surface. The targeted solution lies in the following principle: after rough grinding, the wire surface still retains grinding marks and micro-scratches, and the dimensions have not yet met the final tolerance requirements. Burrs and sharp corners will also form at the ends during the cutting process. Fine grinding converges the diameter dimension with a quantitative tolerance of ±0.005mm, so that the finished product meets the stringent dimensional accuracy requirements of the implant processing base material. Flattening and chamfering eliminate stress concentration and burrs / sharp corners at the ends, and polishing further removes surface scratches and micro-defects, making the finished product surface smooth and defect-free. A clean and dimensionally accurate surface eliminates fatigue crack sources and improves the fatigue life of the implant device. On the other hand, it ensures the biocompatibility and corrosion resistance of the contact surface between the implant and human tissue, thus completing the final sealing of surface quality and dimensional accuracy defects at the finished product stage.

[0122] Example 8; For the proposed solution: Feed φ100 mill bars, 22-25 kg / bar, totaling 3200 kg, discarding any excess material; pickle and grind clean; first heat: 920℃, hold for 60 min to roll φ10.5×Lmm; peel to φ10.2 (+0 / -0.05), collect 700-800 small coils, paying attention to tolerances; pickle and grind the coils clean; feed 2920 kg of the above-mentioned pickled and ground white-skinned coils; vacuum anneal at 750℃, hold for 2.5 hours, dehydrogenation; draw to φ3.95 (-0 / +0.05)×L at 820℃. mm, each mold is cooled by 5-10℃, and a 650mm small tray is collected; annealing is carried out at 720℃ and held for 70 minutes; air cooling is performed; uncoiling and straightening are carried out, and the material length is 3200mm; attention is paid to the length, and the remaining material length is more than 2000mm for normal production; rough grinding is carried out to φ3.8 (-0 / +0.05)×3200mm; stress-relief annealing is carried out at 380℃ and held for 5.5 hours; cooling is carried out in the furnace, and after the bar drawing is qualified, the process continues (performance requirements are: 1000-1030 / 830 / 1 6 / 35, metallographic requirements A1-A9), submit 1 sample for performance testing, submit 1 sample for H content testing; sampling is required according to the production notification; mechanical testing, high-magnification inspection, provide 1 piece of 20mm thin sheet for contamination layer testing; note: submit H content sample; grind to finished size, pay attention to tolerances, bent materials are strictly prohibited from being ground; polish; inspect diameter tolerances; scribing and cutting off the negative length portion to ensure finished length; flatten the end, chamfer both sides at 45°, depth 1-2mm; polish; inspect diameter tolerances; return to warehouse for inspection.

[0123] Regarding the shortcomings of this document: "Domestic processes suffer from complex procedures, unstable processes, low levels of microstructure refinement control and strength-plasticity matching control, large batch-to-batch performance fluctuations, and a lack of comprehensive chemical, tissue, and physical property testing, making it difficult to meet the material consistency and traceability requirements of implantable devices," and "the hydrogen content of existing processes typically only meets ASTM standards." "F136 has a limit requirement of no more than 0.0125%, with very little margin, and faces the risk of hydrogen embrittlement when the process fluctuates." This patent innovatively and non-obviously refines the entire process parameters into directly executable quantitative windows and fixes them: the feed rate is 22-25kg / piece, enough to reach 3200kg without leaving any scrap, after pickling and grinding, it is rolled to φ10.5mm at 920℃ for 60min, peeled to φ10.2mm and collected into 700-800 small coils, after pickling and grinding of the coils, 2920kg of white sheet coils are fed, vacuum annealed at 750℃ for 2.5 hours for dehydrogenation, drawn to φ3.95mm at 820℃ with a temperature drop of 5-10℃ per die, and collected into 650mm small coils. After annealing at 720℃ for 70 minutes and then air cooling, the coil is uncoiled, straightened, and divided into sections with a length of 3200mm and a remaining length of 2000mm or more for normal production. After rough grinding to φ3.8mm, the coil is stress-relieved annealed at 380℃ for 5.5 hours and then cooled in the furnace. The performance requirements of 1000-1030 / 830 / 16 / 35 and the metallographic requirements of A1-A9 are used as the criteria for acceptance. One sample is sent for performance and another for hydrogen content. Sampling is performed for mechanical testing and high-magnification inspection. A 20mm thin sheet is provided for contamination layer detection. After grinding to the finished size, the coil is polished and the diameter tolerance is inspected. The negative length is marked and cut off to ensure the finished length. The coil is flattened and the double-sided chamfer is 45° with a depth of 1-2mm. After polishing and inspection, the coil is returned to the warehouse for inspection. Its targeted solution lies in the following principle: the temperature, holding time, number of passes, dimensions, and material input of each process are all quantified and fixed into a clear process window, making the process highly reproducible and stable, and eliminating dependence on imported materials; among them, rolling at 920℃ is in the two-phase region below the β phase transformation point, avoiding Widmanstätten structure; vacuum annealing at 750℃ for 2.5 hours achieves deep dehydrogenation, making the hydrogen content far below the ASTM F136 limit; drawing at 820℃ cools down by 5-10℃ per die to offset deformation heat and avoid wire breakage and roughening; annealing at 720℃ for 70 minutes stabilizes the structure and enhances plasticity; stress-relief annealing at 380℃ for 5.5 hours is followed by furnace cooling to eliminate residual stress; rough grinding and fine grinding control dimensional tolerances; and finally, a complete inspection chain is formed by mechanical inspection, high-magnification inspection, contamination layer detection, hydrogen content detection, diameter tolerance inspection, and return-to-warehouse inspection. Therefore, this embodiment uses a quantitative process that can be directly executed to bring the microstructure, hydrogen content, plasticity, size and surface quality into a controlled range, thus fundamentally solving the defects of insufficient batch stability and quality traceability.

[0124] Precise definition of process terminology

[0125] 1. Forging: A hot working process in which metal undergoes plastic deformation in a solid state with the help of external forces (pressure, impact), changing its shape, breaking up the original coarse grains in the cast state, and achieving a refined and dense microstructure. Titanium alloy forging is usually carried out within a set temperature range. It eliminates porosity and segregation defects inside the ingot through large deformation and is the core process for controlling the microstructure of titanium alloy billets.

[0126] 2. **Heat Cycle:** A term in the field of hot working, a heat cycle refers to the complete processing cycle from reheating the workpiece from room temperature to the target process temperature, completing one round of deformation processing, until the workpiece temperature drops to a temperature where further processing is not possible. Each reheat-deformation process is considered one heat cycle. This patent employs four-heat forging, i.e., four rounds of heating-deformation, with two heat cycles above the phase transformation point and two heat cycles below the phase transformation point, respectively achieving grain breakage in the β region and grain refinement in the α+β two-phase region.

[0127] 3. Phase transformation point (β phase transformation point / β transformation temperature): For TC4-ELI (Ti-6Al-4V-ELI) titanium alloy, this refers to the critical temperature at which the α+β phases in the titanium alloy completely transform into a single β phase. Above the phase transformation point, the alloy is in the β single-phase region; below the phase transformation point, it is in the α+β coexistence region.

[0128] Forging above the β phase transformation point: Deformation in the high-temperature β single-phase region, mainly breaking the coarse original β grains of the ingot;

[0129] Forging below the β phase transformation point: Deformation in the α+β two-phase region to obtain a fine equiaxed α+β structure and avoid Widmanstätten structure.

[0130] 4. Coil: A semi-finished product formed by rolling metal into a continuous long filament and winding it into a coil, rather than a straight bar. Coils facilitate subsequent multi-pass continuous drawing processes and reduce the frequency of loading and unloading. In this patent, the coiled billet obtained after rolling needs to be peeled, pickled and ground to remove surface oxidation and crack defects in the coiled state.

[0131] 5. Drawing (Wire Drawing): A cold / warm forming process that forces the blank through a die (wire drawing die) with a hole diameter smaller than the blank diameter, causing the material to undergo plastic reduction in diameter to obtain a smaller diameter wire. This invention involves 11 passes of progressively cooling drawing, with each pass reducing the wire diameter while actively lowering the processing temperature to counteract the heat generated by deformation and avoid wire breakage, fraying, and surface oxidation.

[0132] 6. Peeling and Grinding: A special surface treatment process for titanium alloys. Peeling refers to turning / planing to remove the oxide layer (α-contamination layer) and micro-cracks on the surface of the material; grinding is the finishing process. The two are often used together to remove surface defects caused by high-temperature processing and prevent the defects from being pressed into the matrix by subsequent deformation and becoming fatigue sources.

[0133] 7. Vacuum Annealing: Annealing heat treatment carried out in a high-vacuum furnace. On one hand, it achieves microstructure recovery and eliminates residual processing stress; on the other hand, it utilizes the low hydrogen partial pressure environment of the vacuum to allow dissolved hydrogen within the matrix to diffuse out, achieving deep dehydrogenation and suppressing hydrogen embrittlement. The hydrogen content in this patent is controlled to be <0.0003% (3ppm).

[0134] 8. Atmospheric annealing: Annealing treatment under normal air atmosphere. This patent uses 720℃ for 70-80 minutes. The purpose is to fix the material shape and fully restore the structure, so as to provide a stable plastic state for subsequent uncoiling and straightening. No dehydrogenation function is performed.

[0135] 9. Stress-relief annealing: Low-temperature annealing (380℃ in this patent) is much lower than the recrystallization temperature of the alloy. It only eliminates the residual stress caused by grinding and straightening, without changing the microstructure and mechanical properties of the alloy, and prevents deformation and strength reduction caused by stress release during later use.

[0136] 10. Hydrogen embrittlement: Hydrogen atoms penetrate the titanium alloy matrix, causing a decrease in material plasticity and delayed cracking under stress. Medical implants bear loads in the human body for a long time, and hydrogen-induced delayed fracture can directly cause implant failure. This is a risk that must be strictly controlled for medical titanium alloys.

[0137] Standards and testing related terminology

[0138] 1. ASTM F136 (F136 Standard): The American Society for Testing and Materials (ASTM) standard for Ti-6Al-4V ELI titanium alloy processed materials for surgical implants, corresponding to the Chinese standard GB / T13810. This standard specifies that the hydrogen content of Ti-6Al-4V ELI material should be ≤0.0125% (125ppm); this invention controls the hydrogen content to <0.0003% (3ppm), far below the standard limit, thus improving the safety margin against hydrogen embrittlement.

[0139] 2. Metallographic Structure Grade A1: This metallographic rating, used in this patent, is used to evaluate the microstructure of TC4-ELI titanium alloy. Grade A1 represents a fine, uniform, equiaxed α+β microstructure, free of coarse β grains, Widmanstätten structure, and residual original grain boundaries. It represents the microstructure grade with the best high-frequency fatigue performance. A larger A number indicates microstructure deterioration, with A9 being the worst grade in this series. This rating mainly considers grain size, morphology, the presence of Widmanstätten structure, and grain boundary conditions, directly determining the fatigue life of orthopedic implants.

[0140] 3. Contamination layer (α layer): During the high-temperature processing of titanium alloys, oxygen and nitrogen in the air diffuse to the surface, forming an oxygen-rich brittle surface layer. This layer is brittle and prone to cracking, and must be completely removed by peeling, pickling, and grinding. The patent specifically uses 20mm thin slices for contamination layer detection.

[0141] 4. Full-process chemical, tissue, and physical property testing:

[0142] Chemical testing: Detection of components and interstitial elements (H / O / N content);

[0143] Organizational testing: High-magnification metallography and contamination layer inspection;

[0144] Physical property testing: tensile strength, yield strength, elongation, reduction of area, and other mechanical properties;

[0145] Each process must pass three tests before it can be transferred to the next process, thus ensuring quality traceability.

[0146] Key Performance Indicators (KPIs) Explanation

[0147] Tensile strength 1000-1030MPa: the maximum stress the material can withstand before it breaks; Yield strength ≥840MPa: the critical stress at which the material undergoes irreversible plastic deformation; the specifications of this patent are higher than the minimum requirements of ASTM F136 standard (tensile strength ≥860MPa, yield strength ≥795MPa).

[0148] Dimensional tolerance ±0.005mm: The diameter of the finished wire is allowed to fluctuate within only 5 micrometers, meeting the requirements of the base material for high-precision machining of orthopedic screws and connecting rods.

[0149] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claims.

Claims

1. A method for heat treatment of titanium alloy materials by drawing, characterized in that, The process includes the following steps: four forging passes, two of which are above the phase transformation point and two of which are below the phase transformation point, followed by multiple rolling passes and peeling and grinding to ensure that the internal structure of the material is uniform and defect-free; key heat treatment steps: two rolling passes: the first rolling is to a diameter of 100mm at a temperature of 940℃, with 8 to 13 passes; after treatment, air cooling is performed, followed by peeling and grinding; the second rolling is to a diameter of 9.0mm at a temperature of 900℃, with the number of passes controlled between 13 and 15, followed by coiling and peeling. Drawing: The following drawing process involves 11 passes, each reducing the diameter and temperature; the diameter is drawn to 3.90mm to ensure dimensional accuracy and material properties. Vacuum annealing: This is used to strictly control the content of harmful gases such as hydrogen, oxygen, and nitrogen. The hydrogen content must be below 0.0003%, significantly better than the F136 standard (≤0.0125%), to effectively prevent hydrogen embrittlement and ensure material safety. Atmospheric annealing: The temperature is set at 720℃, held for 70-80 minutes, and then air-cooled to achieve material sizing and provide a stable foundation for subsequent uncoiling and straightening. Grinding: Grind to a diameter of 3.8mm; Stress-relief annealing: Stress-relief annealing at 380℃; Sampling and testing: All processes must pass chemical, microstructure and physical property tests before proceeding to the next process.

2. The method for drawing and heat treating titanium alloy materials as described in claim 1, characterized in that, All processes must pass chemical, tissue, and physical property tests before proceeding to the next stage.

3. The method for drawing and heat treating titanium alloy materials as described in claim 2, characterized in that, The final product must meet the following requirements: tensile strength 1000–1030 MPa, yield strength ≥840 MPa, metallographic structure must reach A1 grade, and dimensional tolerance after fine grinding must be controlled within ±0.005 mm.

4. The method for drawing and heat treating titanium alloy materials as described in claim 2, characterized in that, Before the four-stage forging process, the titanium ingot is divided into equal parts.

5. The method for drawing and heat treating titanium alloy materials as described in claim 1, characterized in that, Key heat treatment steps also include pickling and grinding: pickling and grinding are then performed to remove surface cracks and defects.

6. The method for drawing and heat treating titanium alloy materials as described in claim 1, characterized in that, The straightening length after atmospheric annealing is uniformly 3.2 meters.

7. The method for drawing and heat treating titanium alloy materials as described in claim 1, characterized in that, After sampling and testing, the following steps are included: fine grinding: error control. After fine grinding, the dimensional tolerance is controlled within ±0.005mm; flattening, chamfering, polishing, and producing the finished product.

8. The method for drawing and heat treating titanium alloy materials as described in claim 1, characterized in that, Feed φ100 mill bars, 22-25kg / bar, totaling 3200kg, discarding any excess material; pickle and grind clean; first heat: 920℃, hold for 60min to roll φ10.5×Lmm; peel to φ10.2 (+0 / -0.05), collect 700-800 small coils, paying attention to tolerance; pickle and grind the coils clean; feed 2920kg of pickled and ground white-skinned coils of the above ingot number; vacuum anneal at 750℃, hold for 2.5 hours, dehydrogenation; draw to φ3.95 (-0 / +0.05)×L at 820℃. mm, each mold is cooled by 5-10℃, and a 650mm small plate is collected; annealing at 720℃ and holding for 70 minutes; air cooling; uncoiling and straightening, with a material length of 3200mm; pay attention to the length, and the remaining material length of more than 2000mm is normal for production; rough grinding to φ3.8 (-0 / +0.05)×3200mm; stress-relief annealing at 380℃ and holding for 5.5 hours; cooling with the furnace, and continuing after the bar drawing is qualified (performance requirements are: 1000-1030 / 830 / 16 / 35, metallographic requirements A1-A9), one piece is sent for performance, and one piece is sent for H content; sampling is according to the production notice, mechanical inspection is performed, high magnification inspection is performed, one 20mm thin sheet is provided for contamination layer testing, note: send H content; grind to the finished size, pay attention to tolerance, bent material is strictly prohibited from being ground; polish; inspect the diameter tolerance; mark and cut off the negative length part to ensure the finished length; Flat head, 45° chamfer on both sides, 1-2mm depth; polished; diameter tolerance checked; back to warehouse for inspection.

Citation Information

Patent Citations

  • Composite oxidation technology for medicinal titanium alloy

    CN101942688A

  • Medical titanium alloy with biological function of promoting regeneration of bones and blood vessels and preparation method of medical titanium alloy

    CN106148759A

  • Method for preparing medical titanium alloy bars for manufacturing pedicle screws

    CN106826118A

  • Medical titanium alloy special for implant capable of being immediately implanted and preparation method of medical titanium alloy

    CN110157948A

  • Electrolyte composition containing metals and silicon in plasma electrolytic oxidation process and method for manufacturing dental implants coated with hydroxyapatite and containing metal ions and silicon ions by using same composition